Water-based matte light curing coating as well as preparation method and application thereof

By using a photoinitiator to form a polymer coating under the combination of aqueous UV curing resin and urea modified polyurethane resin, the problem of gloss unstable in water-based UV curing coating at high temperatures is solved, and gloss stability and resistance are achieved The thermal properties are improved, while maintaining the stain resistance and scratch resistance of the coating, meeting the requirements of environmentally friendly solvent-free volatility.

CN118978856APending Publication Date: 2024-11-19WANHUA CHEM GRP CO LTD

Patent Information

Application Number
CN202411128754.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing water-based UV cured polyurethane acrylic resin coating has unstable gloss after high temperature treatment, affecting the product quality of PVC floors.

Method used

Using a combination of aqueous UV curing resin and urea modified polyurethane resin, the resin and monomer cross-linking is initiated under ultraviolet irradiation through photoinitiators to form a polymer coating, combining matting powder and functional additives to improve the gloss of the coating Stability and heat resistance.

Benefits of technology

The gloss stability of the coating is significantly improved under high temperature conditions, the coating is maintained with stain resistance and scratch resistance, and is environmentally friendly and solvent-free, reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of water-based coatings, and particularly relates to a water-based matte light curing coating as well as a preparation method and application thereof. The water-based matte light curing coating comprises the following raw materials in parts by weight: 40-70 parts of water-based UV curing resin, 10-40 parts of urea modified polyurethane resin, 1-5 parts of matting powder, 1-5 parts of a coalescing agent, 5-15 parts of water, 1-5 parts of a photoinitiator and 1-8 parts of other functional aids. Compared with the prior art, the water-based matte light curing coating provided by the invention not only has the characteristics of the conventional water-based matte UV curing coating, but also has the characteristic that the gloss stability under a high-temperature condition is obviously improved; the VOC emission amount is small, and the environmental pollution is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of water-based coatings, and specifically relates to a water-based matte photocuring coating and a preparation method and application thereof. Background Art

[0002] In recent years, environmental protection requirements have become increasingly stringent. As an environmentally friendly emerging surface treatment solution, water-based matte ultraviolet (UV) curing coating has been widely used in many fields due to its fast curing speed and high production efficiency, and is gradually expanding at a high growth rate every year. Polyvinyl chloride (PVC) flooring is a synthetic floor decoration material, mainly used in residential home decoration and office buildings, hospitals, schools and other floors. The construction process of PVC flooring is simple, the cost is low, and it is easy to renovate. As an important material for the surface treatment of PVC flooring materials, water-based matte UV curing coatings play a key role in the long-term and stable use of PVC flooring materials due to their gloss, hardness, stain resistance, scratch resistance, etc.

[0003] PVC floor coatings are available in two types: glossy and matte. Matte coatings mainly add matting powder to the high-gloss formula. The matting powder is first added to the coating by physical mixing. After construction, the matting powder is distributed on the surface or inside of the coating when the coating film is dry. The main raw material for the most widely used matte coating is water-based UV-curable polyurethane acrylic resin. The resin itself is easy to matte and has good compatibility. Whether it is configured alone or mixed with other resin emulsions, a matte coating with high hardness and excellent scratch resistance can be obtained; but during the PVC floor coating construction, the uncured or cured coating will be heated to 130-170°C, and mechanical embossing will be performed on the high-temperature surface to improve the decorativeness. However, the water-based UV-curable polyurethane acrylic resin coating in the prior art will affect the arrangement of the matting powder after high-temperature treatment, causing problems such as increased gloss and shiny coatings, affecting product quality.

[0004] Therefore, there is an urgent need to develop a water-based matte UV-curing coating with stable gloss under high-temperature baking. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present application is to overcome the defects of the prior art water-based UV-curable polyurethane acrylic resin coating such as unstable gloss after high-temperature treatment, thereby providing a water-based matte light-curing coating and its preparation method and application.

[0006] To this end, this application provides the following technical solutions: The present invention provides a water-based matte light-curing coating, comprising the following raw materials in parts by weight: 40-70 parts of water-based UV curing resin, 10-40 parts of urea modified polyurethane resin, 1-5 parts of matting powder, 1-5 parts of film-forming aid, 5-15 parts of water, 1-5 parts of photoinitiator, and 1-8 parts of other functional additives.

[0007] In some optional embodiments, the water-based UV curable resin can be 40 parts, 48 ​​parts, 50 parts, 55 parts, 60 parts, 63 parts, 70 parts, or within the range of any of the above values; the urea-modified polyurethane resin can be 10 parts, 20 parts, 30 parts, 40 parts, or within the range of any of the above values; the matting powder can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, or within the range of any of the above values; the film-forming aid can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, or within the range of any of the above values; the water can be 5 parts, 7 parts, 9 parts, 11 parts, 12 parts, 13 parts, 15 parts, or within the range of any of the above values; the photoinitiator can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, or within the range of any of the above values; other functional additives can be 1 part, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, or within the range of any of the above values.

[0008] In some optional embodiments, the water-based matte light-curing coating comprises the following raw materials in parts by weight: 50-60 parts of water-based UV curing resin, 20-30 parts of modified polyurethane resin, 3-4 parts of matting powder, 2-3 parts of film-forming aid, 6-12 parts of water, 1-3 parts of photoinitiator, and 4-7 parts of other functional additives.

[0009] In the present application, the urea-modified polyurethane resin refers to a polyurethane resin containing a urea group, and the urea group refers to a structural unit generated after the isocyanate group (NCO) in the polyurethane resin reacts with the amine group in the polyamine.

[0010] In some optional embodiments, the urea-modified polyurethane resin comprises the following raw materials in percentage by weight: 15%-21% polyol, 8%-10% isocyanate, 2%-5% hydrophilic monomer, 2%-5% silicone oil, 0.05%-0.1% catalyst, 2%-5% chain extender, 0%-2% neutralizer, and the balance is organic solvent and water; In some optional embodiments, in the raw materials of the urea-modified polyurethane resin, the content of polyol can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, or within the range of any of the above values, the content of isocyanate can be 8%, 8.5%, 9%, 9.5%, 10%, or within the range of any of the above values, the content of hydrophilic monomer can be 2%, 2.5%, 3%, 4%, 5%, or within the range of any of the above values, and the content of silicone oil can be 2%, 2.5%, 3%, 4%, 5%, or within the range of any of the above values. %, 4%, 5%, or within the range formed by any of the above values; the content of the catalyst may be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, or within the range formed by any of the above values; the content of the chain extender may be 2%, 2.5%, 3%, 4%, 5%, or within the range formed by any of the above values; the content of the neutralizer may be 0%, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.7%, 2%, or within the range formed by any of the above values, and the balance is the solvent.

[0011] Wherein, the chain extender is a polyamine chain extender, and optionally, includes at least one of diethylenetriamine, triethylenetetramine, polypropylene glycol-based polyetheramine (such as Jeffamine T-403) or tetraethylenepentamine.

[0012] In some optional embodiments, the solid content of the urea-modified polyurethane resin is 30-50%; And / or, the polyol comprises at least one of polyester polyol, polyether polyol and polycarbonate polyol; And / or, the isocyanate comprises at least one of isophorone diisocyanate and hexamethylene diisocyanate; And / or, the hydrophilic monomer comprises a carboxylic acid containing hydroxymethyl, optionally comprising at least one of dimethylol propionic acid and dimethylol butyric acid; and / or, the silicone oil comprises amino-modified polyorganosiloxane; and / or, the catalyst comprises dibutyltin dilaurate; And / or, the neutralizing agent is an organic amine neutralizing agent, including but not limited to triethylamine, etc.; And / or, the organic solvent is for dissolving the hydrophilic monomer, including but not limited to acetone.

[0013] In some optional embodiments, the other functional additives include: at least one of a pH regulator, a wetting agent, a defoaming agent, and a thickener; Optionally, 0-2 parts of pH adjuster, 0-2 parts of wetting agent, 0-2 parts of defoaming agent, and 0-2 parts of thickener.

[0014] In some optional embodiments, the waterborne UV curable resin has a solid content of 30wt%-50wt%, a monomer content of 6-15wt%, and a monomer functionality of 4-6; In some optional embodiments, the solid content of the water-based UV curable resin can be 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, or within the range of any of the above values; the monomer content can be 6wt%, 8wt%, 10wt%, 12wt%, 13wt%, 15wt%, or within the range of any of the above values; the monomer functionality can be 4-official, 5-official or 6-official.

[0015] Optionally, the water-based UV curable resin includes a water-based UV curable polyurethane acrylic resin, the water-based UV curable polyurethane acrylic resin has a pH range of 7.0-9.0 and a viscosity range of 10-1000 mPa·s, including but not limited to Wanhua industrial products Urosin 4616, Urosin 4626, etc.

[0016] In some optional embodiments, the matting powder includes at least one of E-1011 and TS100; And / or, the film-forming aid includes at least one of ethylene glycol butyl ether, diethylene glycol butyl ether, propylene glycol methyl ether and propylene glycol butyl ether; And / or, the photoinitiator includes at least one of TPO-L and 1173.

[0017] The present invention also provides a method for preparing the above-mentioned water-based matte light-curing coating, comprising the following steps: S1, mixing a water-based UV curable resin, a urea-modified polyurethane resin and water to obtain a mixed emulsion; S2, mixing the obtained mixed emulsion, a photoinitiator and other functional additives to obtain a coating base; S3, adding matting powder to the obtained coating base material, dispersing, and obtaining the water-based matte light-curing coating.

[0018] In some optional embodiments, in step S1, the speed of the mixing process is 300-600 r / min, and the mixing time is 5-10 minutes; typically, but not limited to, the speed of the mixing process is 300 r / min, 400 r / min, 500 r / min, 600 r / min, or within the range of any of the above values; the mixing time is 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, or within the range of any of the above values; And / or, in step S2, the rotation speed of the mixing process is 500-800 r / min, and the mixing time is 20-30 minutes; typically, but not limitedly, the rotation speed of the mixing process is 500 r / min, 600 r / min, 700 r / min, 800 r / min, or within the range of any of the above values; the mixing time is 20 minutes, 22 minutes, 25 minutes, 28 minutes, 30 minutes, or within the range of any of the above values.

[0019] And / or, in step S3, the speed of the dispersion process is 1000-1500 r / min, and the dispersion time is 20-30 minutes. Typically, but not limited to, the speed of the dispersion process is 1000 r / min, 1100 r / min, 1200 r / min, 1300 r / min, 1400 r / min, 1500 r / min, or in the range of any of the above values; the dispersion time is 20 minutes, 22 minutes, 25 minutes, 27 minutes, 30 minutes, or in the range of any of the above values.

[0020] The present invention also provides an application of the above-mentioned water-based matte light-curing coating or the water-based matte light-curing coating prepared by the above-mentioned method in floor decoration materials and 3C electronic products.

[0021] In this application, the above-mentioned other functional additives are conventional in the field, and those skilled in the art can choose to add them according to product requirements. Typically, but not limited to, the pH adjuster includes but is not limited to at least one of dimethylethanolamine (DMEA), AMP-95, and triethylamine; the wetting agent includes but is not limited to at least one of BYK-346 and BYK-348; the defoaming agent includes but is not limited to at least one of BYK-011 and BYK-015; the thickener includes but is not limited to at least one of Vesmody U300 and Vesmody U505.

[0022] In some optional implementations, the floor decoration material includes but is not limited to PVC flooring, and the 3C electronic products include but are not limited to mouse, keyboard, mobile phone, notebook, etc. In some optional embodiments, the surface UV coating is applied to 3C electronic products to improve wear resistance and alcohol resistance and extend the service life of the equipment.

[0023] In the present application, the urea-modified polyurethane resin can be obtained through commercial channels (or customized with the manufacturer), such as 2110 from Covestro, Daotan 6450 from Allnex, and R4000 from DSM, or can be homemade.

[0024] In some optional embodiments, the method for preparing the urea-modified polyurethane resin generally comprises the following steps: S11, mixing a polyol, a hydrophilic monomer, and an organic solvent until the hydrophilic monomer is dissolved; S12, adding isocyanate and a catalyst to the above system to carry out a urethanization reaction to obtain a polyurethane prepolymer; S13, adding a neutralizing agent to the obtained polyurethane prepolymer, adding water to disperse it, adding a chain extender to carry out a chain extension reaction, and adding silicone oil to obtain a urea-modified polyurethane.

[0025] Specifically, the preparation method of the urea-modified polyurethane resin may include: adding polyol, hydrophilic monomer and organic solvent to a reaction vessel with a stirrer, a reflux condenser and a thermometer inserted under a nitrogen flow, heating and stirring at 60-65°C, and confirming that the hydrophilic monomer is dissolved. Add isocyanate and a catalyst, heat to 85-90°C, and perform a carbamate reaction for 4-6 hours to obtain a polyurethane prepolymer. The free isocyanate group content at the end of the carbamate reaction is less than 2.7%. The reaction mixture is cooled to 70-80°C, a neutralizer is added thereto, and water is added under strong stirring for dispersion. Then, a chain extender aqueous solution with a mass concentration of 20-50% is added to carry out a chain extension reaction, silicone oil is added, and part of the organic solvent and water are removed to obtain a urea-modified polyurethane resin with a certain solid content.

[0026] In the present application, the dry film thickness of the water-based matte photocuring coating applied on the substrate or article is 5-100 μm, optionally, the dry film thickness is 5 μm, 10 μm, 20 μm, 30 μm, 50 μm, 70 μm, 80 μm, 90 μm, 100 μm, or within the range of any of the above values, and then undergoes the steps of drying and radiation curing.

[0027] In some optional embodiments, the drying temperature is 50-200°C.

[0028] In some optional embodiments, the total UV dose for radiation curing is 1200-3000 mJ / cm 2 Typically, but not limited to, the total UV dose for radiation curing is 1200 mJ / cm 2 , 1500mJ / cm 2 , 1800mJ / cm 2 , 2000mJ / cm 2 , 2300mJ / cm 2 , 2500mJ / cm 2 , 2700mJ / cm 2 , 3000mJ / cm 2 , or within a range consisting of any of the above values.

[0029] The technical solution of this application has the following advantages: The water-based matte light-curing coating provided by the present application comprises the following raw materials in parts by weight: 40-70 parts of water-based UV curing resin, 10-40 parts of urea-modified polyurethane resin, 1-5 parts of matting powder, 1-5 parts of film-forming aid, 5-15 parts of water, 1-5 parts of photoinitiator, and 3-8 parts of other functional additives. Compared with the prior art, the water-based matte light-curing coating provided by the present application not only has the characteristics of conventional water-based matte UV curing coatings, but the most important thing is that the gloss stability under high temperature conditions is significantly improved; and the VOC emission is small, which effectively reduces environmental pollution. Specifically, the present application is based on water-based UV curing resin and urea-modified polyurethane as the main film-forming materials, and the photoinitiator is cracked under ultraviolet irradiation to produce free radicals, and the active free radicals initiate the unsaturated double bonds in the resin and its monomers, and the double bonds are changed into single bonds, so that the water-based UV curing resin and the monomers are cross-linked to form a polymer coating, and the energy consumption required for film formation is small, and it is environmentally friendly and solvent-free, and does not affect the health of the operator. The formed cured film has ultra-low surface energy, and the anti-fouling and scratch resistance properties are quite excellent. The present application introduces a certain amount of urea-modified polyurethane resin into the traditional water-based UV-curing resin. The urea-modified polyurethane resin is a self-cross-linking material, which has good compatibility with the light-curing polyurethane resin, can wet and disperse the matting powder, and is quick-drying and temperature-resistant. The appropriate amount of introduction can ensure the arrangement of the matting powder during high-temperature treatment, improve the gloss stability of the water-based matte UV-curing coating, and will not lose the product's stain resistance, etc., thereby meeting the performance requirements. DETAILED DESCRIPTION

[0030] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.

[0031] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0032] Examples 1-8 This embodiment provides a water-based matte light-curing coating, the specific composition and type of its raw materials are shown in Table 1, and the specific preparation method and operating parameters are as follows: S1, taking a water-based UV curable resin and a urea-modified polyurethane resin in proportion and placing them in a container, adding a certain amount of deionized water, and mixing at 500 r / min for 10 minutes to obtain a mixed emulsion; S2, adding a pH adjuster, a wetting agent, a film-forming aid, a photoinitiator, and a thickener to the mixed emulsion, and mixing at 800 r / min for 30 minutes to obtain a coating base; S3, adding matting powder to the above coating base material, dispersing at a high speed of 1200 r / min for 30 minutes, filtering, and obtaining a water-based matte light-curing coating with stable gloss.

[0033] The specific steps of preparing the self-made urea-modified polyurethane resin used in Examples 4 and 7 are as follows: In a reaction vessel with a stirrer, a co-current condenser and a thermometer, 180 g of polycarbonate diol (Kuraray C-2090), 20.9 g of dimethylol propionic acid (DMPA) and 152 g of acetone were added under nitrogen flow, and then heated and stirred at 60°C to confirm that DMPA was dissolved. 90 g of hydrogenated phenylmethane diisocyanate (H12MDI) and 0.7 g of dibutyltin dilaurate (catalyst) were added, heated to 90°C, and urethanization reaction was carried out for 5 hours to obtain a polyurethane prepolymer. The free isocyanate group content at the end of the urethanization reaction was <2.67%. The reaction mixture was cooled to 80°C, 15.4 g of triethylamine was added and mixed, and water was added to the reaction vessel to 780 g under strong stirring for dispersion. Next, 65 g of a 35% aqueous solution of diethylenetriamine was added to carry out a chain extension reaction, the mixture was kept at 50°C for 30 min, 25 g of KH-792 (silicone oil) was added, 180 g of the organic solvent and water were extracted from the resulting mixture, and a urea-modified polyurethane resin (solid content of 35 wt%) was obtained.

[0034] Comparative Examples 1-4 This comparative example provides a water-based matte light-curing coating, the specific composition and type of its raw materials are shown in Table 1, and the specific preparation method and operating parameters are as follows: S1, taking water-based UV curable resin and urea-modified polyurethane resin in proportion (if the component is not contained, no addition will be made) and placing them in a container, adding a certain amount of deionized water, and mixing at 500 r / min for 10 minutes to obtain a mixed emulsion; S2, adding a pH adjuster, a wetting agent, a film-forming aid, a photoinitiator, and a thickener to the mixed emulsion, and mixing at 800 r / min for 30 minutes to obtain a coating base; S3, adding matting powder to the above coating base material, dispersing at a high speed of 1200 r / min for 30 minutes, filtering, and obtaining a water-based matte light-curing coating with stable gloss.

[0035] Table 1

[0036] Note: The unit of dosage of each component in the above table is kg, and the blank part means that the component is not added.

[0037] Test Case The performance of the water-based matte light-curing coatings prepared in each embodiment and comparative example was tested, and the specific testing method is as follows: Initial gloss: The coating was applied on a PVC substrate with a 100um wire rod and baked at 80°C for 10 min. The gloss data of the coating at 60° was tested in accordance with EN ISO2813:2014 and recorded as the initial gloss.

[0038] 160℃ gloss: bake the above sample at 160℃ for 3min, and test the 60° gloss data of the coating in accordance with EN ISO 2813:2014, which is recorded as 160℃ gloss.

[0039] Stability: The coating storage stability test was carried out in accordance with GB / T 6753.3-1986.

[0040] Stain resistance: The above samples were subjected to radiation curing (the total UV dose of radiation curing was 1500mJ / cm 2 ) and then conduct stain resistance test according to ISO26987:2013.

[0041] Scratch resistance: The above samples were subjected to radiation curing (the total UV dose of radiation curing was 1500mJ / cm 2 ) and then perform a scratch resistance test according to EN 16094 (B). The specific test results are shown in the table below: Table 2

[0042] Note: OK means the requirements are met, NG means the requirements are not met.

[0043] From the data in the above table, it can be seen that the water-based matte light-curing coating provided in the embodiment of the present application has better heat resistance, and can still have a stable gloss performance after a high temperature of 160 degrees Celsius, and also has stain resistance and scratch resistance. The present application can improve the gloss stability of the formula by introducing urea-modified polyurethane, and at the same time control the dosage, and has no obvious damage to stain resistance and scratch resistance, mainly because the introduction of the urea bond structure has better heat resistance on the basis of providing stain resistance and scratch resistance.

[0044] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A water-based matte light-curing coating, characterized in that: The invention comprises the following raw materials in parts by weight: 40-70 parts of water-based UV curing resin, 10-40 parts of urea modified polyurethane resin, 1-5 parts of matting powder, 1-5 parts of film-forming aid, 5-15 parts of water, 1-5 parts of photoinitiator, and 1-8 parts of other functional additives.

2. The water-based matte light-curing coating according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 50-60 parts of water-based UV curing resin, 20-30 parts of urea modified polyurethane resin, 3-4 parts of matting powder, 2-3 parts of film-forming aid, 6-12 parts of water, 1-3 parts of photoinitiator, and 4-7 parts of other functional additives.

3. The water-based matte light-curing coating according to claim 1 or 2, characterized in that: The urea-modified polyurethane resin comprises the following raw materials in percentage by weight: 15%-21% polyol, 8%-10% isocyanate, 2%-5% hydrophilic monomer, 2%-5% silicone oil, 0.05%-0.1% catalyst, 2%-5% chain extender, 0%-2% neutralizer, and the balance is organic solvent and water; Wherein, the chain extender is a polyamine chain extender, and optionally, includes at least one of diethylenetriamine, triethylenetetramine, polypropylene glycol-based polyetheramine or tetraethylenepentamine.

4. The water-based matte light-curing coating according to claim 3, characterized in that: The solid content of the urea-modified polyurethane resin is 30-50wt%; And / or, the polyol comprises at least one of polyester polyol, polyether polyol and polycarbonate polyol; And / or, the isocyanate comprises at least one of isophorone diisocyanate and hexamethylene diisocyanate; And / or, the hydrophilic monomer comprises a carboxylic acid containing hydroxymethyl, optionally comprising at least one of dimethylol propionic acid and dimethylol butyric acid; and / or, the silicone oil comprises amino-modified polyorganosiloxane; And / or, the catalyst comprises dibutyltin dilaurate And / or, the neutralizing agent is an organic amine neutralizing agent; And / or, the organic solvent comprises acetone.

5. The water-based matte light-curing coating according to claim 1 or 2, characterized in that: The other functional additives include: at least one of a pH regulator, a wetting agent, a defoaming agent, and a thickener; Optionally, 0-2 parts of pH adjuster, 0-2 parts of wetting agent, 0-2 parts of defoaming agent, and 0-2 parts of thickener.

6. The water-based matte light-curing coating according to claim 1 or 2, characterized in that: The water-based UV curable resin has a solid content of 30wt%-50wt%, a monomer content of 6wt%-15wt%, and a monomer functionality of 4-6; Optionally, the water-based UV curable resin includes a water-based UV curable polyurethane acrylic resin. Further optionally, the water-based UV curable polyurethane acrylic resin has a pH range of 7.0-9.0 and a viscosity range of 10-1000 mPa·s.

7. The water-based matte light-curing coating according to claim 1 or 2, characterized in that: The matting powder includes at least one of E-1011 and TS100; And / or, the film-forming aid includes at least one of ethylene glycol butyl ether, diethylene glycol butyl ether, propylene glycol methyl ether and propylene glycol butyl ether; And / or, the photoinitiator includes at least one of TPO-L and 1173.

8. A method for preparing the water-based matte photocurable coating according to any one of claims 1 to 7, characterized in that: The steps include: S1, mixing a water-based UV curable resin, a urea-modified polyurethane resin and water to obtain a mixed emulsion; S2, mixing the obtained mixed emulsion, a photoinitiator and other functional additives to obtain a coating base; S3, adding matting powder to the obtained coating base material, dispersing, and obtaining the water-based matte light-curing coating.

9. The method for preparing a water-based matte light-curing coating according to claim 8, characterized in that: In step S1, the rotation speed of the mixing process is 300-600 r / min, and the mixing time is 5-10 minutes; And / or, in step S2, the rotation speed of the mixing process is 500-800 r / min, and the mixing time is 20-30 minutes; And / or, in step S3, the rotation speed of the dispersion process is 1000-1500 r / min, and the dispersion time is 20-30 minutes.

10. Use of the water-based matte photocuring coating according to any one of claims 1 to 7 or the water-based matte photocuring coating prepared by the method according to any one of claims 8 or 9 in floor decoration materials and 3C electronic products.

Citation Information

Patent Citations

  • Organosilicon modified aqueous polyurethane resin and preparation thereof

    CN101348554A

  • Aqueous UV (ultraviolet) spray coating dull flat varnish

    CN102827548A

  • Organosilicon modified waterborne polyurethane resin and preparation method thereof

    CN103275298A

  • Double-curing water-based Primer coating and preparation method and application thereof

    CN110511658A

  • Polyurethane urea water dispersion, matte coating material, and surface treatment agent

    CN113195647A

Cited By

  • Preparation method of stain-resistant and wiping-resistant water-based UV matte coating

    CN119978941A