Conductive aluminum paste composition for topcon-type solar cell electrodes, and topcon-type solar cell having laminated back surface electrodes from said composition

By using a conductive aluminum paste composition of aluminum-silicon alloy powder and glass powder with a specific composition, the alignment problem and conversion efficiency reduction problem of aluminum paste forming the back electrode in TOPCon solar cells were solved, achieving burn-through without LCO and good ohmic contact, thus improving the conversion efficiency of the cell.

CN118984816APending Publication Date: 2024-11-19TOYO ALUMINIUM KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030117.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-23
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When using aluminum paste to form the back electrode in TOPCon solar cells, LCO formation is required, along with high-precision alignment technology, which increases costs. At the same time, existing aluminum paste cannot effectively burn through the passivation film or form an alloy layer, resulting in reduced cell conversion efficiency.

Method used

A conductive aluminum paste composition containing aluminum-silicon alloy powder and glass powder with specific compositions, wherein the silicon concentration of the aluminum-silicon alloy powder is 30-40% by mass and the glass powder is composed of first and second glass powders with specific compositions, is capable of burning through the passivation film and forming good ohmic contacts without forming LCO.

Benefits of technology

This technology eliminates the need for LCO formation in TOPCon solar cells, avoids the formation of alloy layers, reduces costs, and improves the conversion efficiency of the cell, with a contact resistance of less than 10 mΩ·cm2.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The present invention relates to a conductive aluminum paste composition for TOPCon-type solar cell electrodes, which contains an aluminum-silicon alloy powder, an organic vehicle, and a glass powder, and satisfies the following conditions (1) and (2): (1) the silicon concentration of the aluminum-silicon alloy powder is 30-40 mass%; (2) The glass powder contains a first glass powder and a second glass powder, the first glass powder contains 45-71% of PbO, 5-35% of B2O3, and 0.1-25.0% of SiO2 in terms of oxide mol%, and when x% of B2O3, y% of SiO2, and z% of PbO are contained, the value of [(x + y) / z] is 0.40-1.00, and the second glass powder contains 35.0-55.0% of B2O3, 5.0-10.0% of SiO2, 1.0-20.0% of BaO, 5.0-25.0% of CaO, and 3.0-30.0% of K2O in terms of oxide mol%, and does not substantially contain PbO.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a conductive aluminum paste composition for TOPCon type solar cell electrodes and a TOPCon type solar cell having a back electrode laminated thereon which is a fired product of the composition. Background Art

[0002] In the past, as one of the technologies for improving the efficiency and reliability of solar cells, a solar cell element using a TOPCon (Tunnel Oxide Passivated Contact) structure has been investigated. Hereinafter, in this specification, a solar cell using this structure is referred to as a "TOPCon type solar cell".

[0003] In the TOPCon structure, in order to reduce the recombination loss between the n-type silicon substrate as the base substrate and the back electrode made of silver, aluminum, etc., a thin tunneling oxide layer of about several nanometers made of silicon oxide and a semiconductor layer doped with high concentrations of phosphorus, boron, etc. (microcrystalline n-type silicon substrate) are formed between the base substrate and the back electrode. + The structure is characterized by the tunnel effect produced by the oxide layer, thereby suppressing the connection between the n-type silicon substrate and the microcrystalline n + Carrier losses at the interfaces between silicon layers.

[0004] In a TOPCon solar cell, when a silver paste is used to form a back electrode, the passivation film is heat-treated after the silver paste is applied, and the back electrode can be formed by partially penetrating the passivation film by fire-through. In contrast, when an aluminum paste is used to form a back electrode, since the passivation film cannot be burnt through, an opening (LCO: laser contact opening) is formed to expose the n-type silicon substrate by laser treatment of the connection portion with the n-type silicon substrate in advance, and the back electrode is formed by heat-treating the aluminum paste after applying it in a manner overlapping with the opening (Patent Document 1). In Patent Document 1, a study was conducted on the use of a conductive aluminum paste composition containing aluminum-silicon alloy particles, an organic carrier, and glass powder.

[0005] In addition to TOPCon type solar cells, as a burn-through aluminum paste that can form a back electrode without forming LCO, there is a known back electrode paste containing aluminum powder, lead glass powder and an organic carrier facing a p-type silicon substrate (Patent Document 2). As a lead-free solution, there is a known back electrode paste containing aluminum powder, lead-free glass powder and an organic carrier (Patent Document 3).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2021-2460

[0009] Patent Document 2: Japanese Patent Application Publication No. 2019-127404

[0010] Patent Document 3: Japanese Patent Application Publication No. 2020-198380 Summary of the invention

[0011] 1. Technical issues to be resolved

[0012] However, when aluminum paste is used to form the back electrode in a TOPCon solar cell, a higher alignment technology is required because an LCO (opening) needs to be formed and the aluminum paste needs to be applied (printed) in a manner overlapping the LCO. In addition, it is difficult to meet the demand for cost reduction from the perspective of forming an LCO compared to the case of using a silver paste. On the other hand, when only an aluminum paste as in Patent Document 1 is used without forming an LCO, the passivation film cannot be burned through (penetrated) when the aluminum paste coating is fired as described above, and the microcrystalline n + Silicon layer, so the conversion efficiency of the battery cell will be greatly reduced.

[0013] Furthermore, if the aluminum paste for p-type silicon substrates as described in Patent Documents 2 and 3 is applied to TOPCon solar cells, even if burn-through is possible, an alloy layer (aluminum-silicon alloy layer) will be generated by the reaction between the n-type silicon substrate and aluminum, and the formed p-type silicon substrate will be + Layer and crystallite + The silicon layer will shunt and the conversion efficiency of the battery cell will still be greatly reduced.

[0014] Therefore, the object of the present invention is to provide a conductive aluminum paste composition, which has the burn-through property of the passivation film itself without forming LCO in the formation of the back electrode of the TOPCon type solar cell, and further can obtain good ohmic contact without forming an n-type silicon substrate and an alloy layer. In addition, it is also an object to provide a TOPCon type solar cell stacked with a back electrode which is a fired product of the conductive aluminum paste composition.

[0015] (II) Technical solution

[0016] The inventors of the present application conducted intensive studies to achieve the above-mentioned purpose and found that the above-mentioned purpose can be achieved by using a conductive aluminum paste composition containing aluminum-silicon alloy powder and glass powder of a specific composition, thereby completing the present invention.

[0017] That is, the present invention relates to the following conductive aluminum paste composition for TOPCon type solar cell electrodes and a TOPCon type solar cell using the composition.

[0018] 1. A conductive aluminum paste composition for TOPCon type solar cell electrodes, which is a conductive aluminum paste composition containing aluminum-silicon alloy powder, an organic carrier and glass powder, characterized in that:

[0019] (1) The silicon concentration of the aluminum-silicon alloy powder is greater than or equal to 30% by mass and less than or equal to 40% by mass;

[0020] (2) The glass powder includes a first glass powder and a second glass powder,

[0021] The first glass powder contains, expressed in terms of oxide mol%, 45% to 71% PbO, 5% to 35% B2O3, and 0.1% to 25.0% SiO2, wherein the content of B2O3 is x mol%, the content of SiO2 is y mol%, the content of PbO is z mol%, and the value of [(x+y) / z] is in the range of 0.40 to 1.00.

[0022] The second glass powder contains, expressed in terms of oxide mol %, 35.0% to 55.0% B2O3, 5.0% to 10.0% SiO2, 1.0% to 20.0% BaO, 5.0% to 25.0% CaO, 3.0% to 30.0% K2O, and substantially no PbO.

[0023] 2. The conductive aluminum paste composition according to item 1 above, wherein the first glass powder contains a total of 1% to 10% of Al2O3 and / or ZnO expressed in terms of oxide mol%.

[0024] 3. The conductive aluminum paste composition according to item 1 or 2 above, wherein the second glass powder contains 1.0% to 10.0% SrO expressed in terms of oxide mol%.

[0025] 4. A TOPCon type solar cell, wherein a back electrode is stacked on a silicon semiconductor substrate, and the back electrode is a fired product of the conductive aluminum paste composition according to any one of items 1 to 3 above.

[0026] (III) Beneficial effects

[0027] By making the conductive aluminum paste composition of the present invention contain aluminum-silicon alloy powder and glass powder of a specific composition, the paste itself has the property of burning through the passivation film in the formation of the back electrode of the TOPCon type solar cell without forming LCO, and further, a good ohmic contact can be obtained without forming an n-type silicon substrate and an alloy layer. In addition, not forming an n-type silicon substrate and an alloy layer means that the microcrystalline n + Silicon layer, can obtain good ohmic contact means that the contact resistance is 10mΩ·cm, which is an indicator of high conversion efficiency 2 the following. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 FIG. 1 is a schematic cross-sectional view showing an example of the structure of a TOPCon type solar cell.

[0029] Figure 2 To illustrate the effect of screen printing the conductive aluminum paste composition on the microcrystalline n + The figure shows the printing width when printing on the surface of the silicon layer. Specifically, the figure shows the case where the printing width is 1 mm, the length is 10 mm, and the printing intervals are 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, and 2.0 mm. DETAILED DESCRIPTION

[0030] The conductive aluminum paste composition for TOPCon type solar cell electrodes of the present invention and the TOPCon type solar cell using the same are described in detail below. In addition, in this specification, unless otherwise specified, the numerical range indicated by "~" means "above, below". That is, "A~B" means a range above A and below B.

[0031] 1. TOPCon type solar cell

[0032] The conductive aluminum paste composition of the present invention is for TOPCon type solar cell electrodes. The conductive aluminum paste composition contains aluminum-silicon alloy powder, organic carrier and glass powder. In particular, as long as the aluminum-silicon alloy powder and the glass powder have a specified specific composition, the other requirements can apply the requirements of the known TOPCon type solar cell.

[0033] Figure 1 FIG. 1 is a schematic cross-sectional view showing an example of the structure of a TOPCon type solar cell. Figure 1 The TOPCon type solar cell shown in the figure has a p-type impurity layer 2 formed on the light-receiving side of the n-type silicon semiconductor substrate 1 of the base substrate, a back electrode 6 on the back side of the n-type silicon semiconductor substrate 1, and an extremely thin oxide layer 3 and microcrystalline n-type silicon semiconductor substrates doped with a high concentration of dopants between the n-type silicon semiconductor substrate 1 and the back electrode 6.+ Specifically, between the n-type silicon semiconductor substrate 1 and the back electrode 6, an oxide layer 3 is provided on the n-type silicon semiconductor substrate 1 side, and a microcrystalline n-type silicon semiconductor layer 4 is provided on the back electrode 6 side. + Silicon layer 4. With this structure, the TOPCon type solar cell can generate a tunnel effect through the oxide layer 3, thereby suppressing the n-type silicon semiconductor substrate 1 (n - Silicon layer) and microcrystalline n + Silicon layer 4 (n + Carrier loss at the interface of the silicon layer).

[0034] As the oxide layer 3, for example, silicon oxide can be used. The thickness of the oxide layer 3 is not limited, and can be, for example, 1 to 10 nm, preferably 3 to 8 nm. By setting the thickness of the oxide layer 3 to 1 to 10 nm, the above-mentioned tunnel effect is easily induced, and carriers are easily moved to the back side of the solar cell, thereby improving the conversion efficiency. In addition, if the thickness of the oxide layer 3 is 1 to 10 nm, it is also easy to suppress the n - Silicon layer and n + The carrier loss at the interface of the silicon layer is small, so it is not easy to cause a decrease in conversion efficiency.

[0035] As the n-type silicon semiconductor substrate 1 , for example, a silicon semiconductor substrate used for semiconductor applications or solar cell applications can be widely applied.

[0036] In the TOPCon solar cell of the present invention, the microcrystalline n + A passivation film 5 is provided between the silicon layer 4 and the back electrode 6. Since the conductive aluminum paste composition of the present invention has the property of burning through the passivation film 5, it is not necessary to form an LCO (opening) on ​​the passivation film 5 when forming the back electrode 6. Finger electrodes (not formed on the surface of the n-type silicon semiconductor substrate 1 on the opposite side to the back electrode 6) are formed via a p-type impurity layer. Figure 1 The finger electrodes may be made of, for example, silver or aluminum.

[0037] The back electrode 6 can be formed by the conductive aluminum paste composition of the present invention. The details are described below. By making the conductive aluminum paste composition of the present invention contain aluminum-silicon alloy powder and glass powder of a specific composition, in the formation of the back electrode 6 of the TOPCon type solar cell, the paste itself has the burn-through property of the passivation film 5 without forming LCO, and further, a good ohmic contact can be obtained without forming an n-type silicon semiconductor substrate 1 and an alloy layer. In addition, by being a conductive aluminum paste composition, from the perspective of being able to use a well-known printing method such as a screen printing method, the pre-fired coating film of the back electrode 6 can be easily formed.

[0038] 2. Conductive aluminum paste composition

[0039] The conductive aluminum paste composition of the present invention is used for TOPCon type solar cell electrodes, and more specifically, is used for forming a back electrode. The paste composition contains aluminum-silicon alloy powder, an organic vehicle, and glass powder, and the paste composition is characterized in that:

[0040] (1) the aluminum-silicon alloy powder has a silicon concentration of 30 mass % or more and 40 mass % or less,

[0041] (2) The glass powder includes a first glass powder and a second glass powder,

[0042] The first glass powder contains, expressed in terms of oxide mol%, 45% to 71% PbO, 5% to 35% B2O3, and 0.1% to 25.0% SiO2, wherein the content of B2O3 is x mol%, the content of SiO2 is y mol%, the content of PbO is z mol%, and the value of [(x+y) / z] is in the range of 0.40 to 1.00.

[0043] The second glass powder contains, expressed in terms of oxide mol %, 35.0% to 55.0% B2O3, 5.0% to 10.0% SiO2, 1.0% to 20.0% BaO, 5.0% to 25.0% CaO, 3.0% to 30.0% K2O, and substantially no PbO.

[0044] According to the conductive aluminum paste composition of the present invention having the above characteristics, in the formation of the back electrode of the TOPCon type solar cell, the paste itself has the property of burning through the passivation film without forming LCO, and further, a good ohmic contact can be obtained without forming an n-type silicon substrate and an alloy layer. In addition, not forming an n-type silicon substrate and an alloy layer means that the microcrystalline n + Silicon layer, can obtain good ohmic contact means that the contact resistance is 10mΩ·cm, which is an indicator of high conversion efficiency 2 the following.

[0045] Hereinafter, each component of the conductive aluminum paste composition of the present invention will be described in detail.

[0046] <Aluminum-silicon alloy powder>

[0047] In the conductive aluminum paste composition, the aluminum-silicon alloy powder is a component that can play a role in bringing about conductivity. In the conductive aluminum paste composition of the present invention, as the aluminum-silicon alloy powder, an aluminum-silicon alloy powder having a silicon concentration of 30 mass % or more and 40 mass % or less (preferably 35 mass % or more and 40 mass % or less) is used. In the present invention, by using the aluminum-silicon alloy powder as a conductive component, migration of the electrode material does not occur compared to silver, and the risk of short circuit can be reduced.

[0048] By setting the silicon concentration to 30 mass % or more and 40 mass % or less, the conductive aluminum paste composition is less likely to be mixed with the microcrystalline n + The silicon layer melts, and the conductive aluminum paste composition and the microcrystalline n + The silicon layer is difficult to form an aluminum-silicon alloy layer. As a result, the reduction in conversion efficiency of the battery cell caused by carrier loss can be suppressed. If the silicon concentration is less than 30% by mass, p + If the silicon concentration is greater than 40 mass %, the resistance will increase and there is a risk that it will be difficult to produce the aluminum-silicon alloy powder. Therefore, in the present invention, an aluminum-silicon alloy powder having a silicon concentration of 30 mass % or more and 40 mass % or less is used.

[0049] The size of the aluminum-silicon alloy powder particles is not particularly limited. For example, the volume average particle size D50 of the aluminum-silicon alloy powder (particles) can be set to 1 to 10 μm. Among them, the volume average particle size D50 is preferably 5 to 8 μm. In addition, the volume average particle size D50 of the aluminum-silicon alloy powder in this specification is a value measured by laser diffraction method.

[0050] In addition, the aluminum-silicon alloy powder may contain strontium as a third component. That is, as the conductive powder containing strontium, in addition to the aluminum-silicon-strontium (Al-Si-Sr) alloy powder, an aluminum-silicon alloy powder and an aluminum-silicon-strontium alloy powder may be used simultaneously.

[0051] The amount of strontium contained in the conductive powder containing strontium is not particularly limited, and can be 0.01 to 1 mass %. Adding strontium to the conductive powder has the effect of increasing the liquid phase composition during firing, promoting sintering, and reducing surface resistance when the silicon concentration is high.

[0052] <Organic carrier>

[0053] In the conductive aluminum paste composition of the present invention, the type of organic vehicle is not particularly limited, and for example, a known organic vehicle for forming a back electrode of a solar cell can be widely used. As the organic vehicle, a material in which a resin is dissolved in a solvent can be cited. Alternatively, the organic vehicle may contain no solvent and the resin itself can be used directly.

[0054] The type of the solvent is not limited, and examples thereof include diethylene glycol monobutyl ether, diethylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether, etc. The solvent contained in the organic vehicle may be one type or two or more types.

[0055] As the resin, for example, various known resins can be listed, specifically, ethyl cellulose resin, nitrocellulose resin, polyvinyl butyral resin, phenolic resin, melamine resin, urea resin, xylene resin, alkyd resin, unsaturated polyester resin, acrylic resin, polyimide resin, furan resin, urethane resin, isocyanate compound, cyanate compound, polyethylene resin, polypropylene resin, polystyrene resin, ABS resin, polymethyl methacrylate resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl acetate resin, polyvinyl alcohol resin, polyacetal resin, polycarbonate resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyphenylene ether resin, polysulfone resin, polyimide resin, polyether sulfone resin, polyarylate resin, polyether ether ketone resin, polytetrafluoroethylene resin, silicone resin, etc. The resin contained in the organic vehicle can be one or more.

[0056] The organic carrier may also contain various additives as required. As additives, for example, antioxidants, corrosion inhibitors, defoamers, thickeners, dispersants, tackifiers, coupling agents, static imparting agents, polymerization inhibitors, thixotropic agents, sedimentation inhibitors, etc. can be listed. Specifically, polyethylene glycol ester compounds, polyethylene glycol ether compounds, polyoxyethylene sorbitan ester compounds, sorbitan alkyl ester compounds, aliphatic polycarboxylic acid compounds, phosphate ester compounds, amide amine salts of polyester acids, oxidized polyethylene compounds, fatty acid amide waxes, alkaline earth metal salts of stearic acid, etc. can be listed.

[0057] The ratio of the resin, the solvent, and various additives contained in the organic vehicle can be arbitrarily adjusted, and can be, for example, the same component ratio as that of a known organic vehicle.

[0058] The content of the organic carrier is not particularly limited. For example, from the perspective of good coating (printing) properties, it is preferably 10 parts by mass or more and 500 parts by mass or less, and more preferably 20 parts by mass or more and 45 parts by mass or less, relative to 100 parts by mass of the aluminum-silicon alloy powder.

[0059] <Glass powder>

[0060] The glass powder contained in the conductive aluminum paste composition of the present invention is a vitreous glass material (powder). In particular, the present invention is characterized in that the glass powder of the following specific composition is used:

[0061] The glass powder includes a first glass powder (lead-containing glass) and a second glass powder (borosilicate glass substantially free of lead).

[0062] The first glass powder contains, expressed in terms of oxide mol%, 45% to 71% PbO, 5% to 35% B2O3, and 0.1% to 25.0% SiO2, wherein the content of B2O3 is x mol%, the content of SiO2 is y mol%, the content of PbO is z mol%, and the value of [(x+y) / z] is in the range of 0.40 to 1.00.

[0063] The second glass powder contains, expressed in terms of oxide mol %, 35.0% to 55.0% B2O3, 5.0% to 10.0% SiO2, 1.0% to 20.0% BaO, 5.0% to 25.0% CaO, 3.0% to 30.0% K2O, and substantially no PbO.

[0064] In the present invention, by combining the first glass powder and the second glass powder, it is possible to obtain a good ohmic contact while making the passivation film excellent in the fire-through property, without forming an n-type silicon semiconductor substrate and an alloy layer (aluminum-silicon alloy layer) (i.e., the microcrystalline n-type silicon semiconductor substrate is not formed during the firing process). + The corrosion of the silicon layer is suppressed. As a result, the conversion efficiency of the solar cell can be improved.

[0065] The first glass powder is lead-containing glass, which contains, expressed in terms of oxide mol %, more than 45% and less than 71% of PbO, more than 5% and less than 35% of B2O3, and more than 0.1% and less than 25.0% of SiO2, and the content of B2O3 is set to x mol %, the content of SiO2 is set to y mol %, and the content of PbO is set to z mol %, and the value of [(x+y) / z] is in the range of more than 0.40 and less than 1.00.

[0066] In the first glass powder, the content of PbO can be set to be greater than 50% and less than 71%, or greater than 60% and greater than 71%. The content of B2O3 can be set to be greater than 10% and less than 32%, or greater than 20% and less than 32%. The content of SiO2 can be set to be greater than 1.0% and less than 23.0%, or greater than 8.0% and less than 23.0%. In addition, the value of [(x+y) / z] can be set to be greater than 0.40 and less than 0.90, or greater than 0.43 and less than 0.86.

[0067] The first glass powder may also contain Al2O3 and / or ZnO in an amount of 1% or more and 10% or less in total, expressed as oxide mole %. By containing these components, the viscosity of the paste can be stabilized while improving the weather resistance of the first glass powder. The content of Al2O3 can be set to, for example, 1% or more and 7% or less. In addition, the content of ZnO can be set to, for example, 2% or more and 5% or less, or can be set to, for example, 3% or more and 4% or less.

[0068] The second glass powder is a borosilicate glass that is substantially free of lead, and contains, expressed in terms of oxide mol %, 35.0% to 55.0% B2O3, 5.0% to 10.0% SiO2, 1.0% to 20.0% BaO, 5.0% to 25.0% CaO, 3.0% to 30.0% K2O, and substantially no PbO.

[0069] With respect to the second glass powder, the content of B2O3 can be set to be greater than 40.0% and less than 53.0%, or greater than 41.2% and less than 45.5%. The content of SiO2 can be set to be greater than 6.5% and less than 9.0%, or greater than 6.9% and less than 7.6%. The content of BaO can be set to be greater than 10.0% and less than 20.0%, or greater than 15.1% and less than 18.4%. The content of CaO can be set to be greater than 6.0% and less than 20.0%, or greater than 6.4% and less than 19.0%. In addition, the content of K2O can be set to be greater than 10.0% and less than 30.0%, or greater than 11.4% and less than 20.1%. In addition, the second glass powder does not substantially contain a lead component (PbO), which means that, through component analysis, the lead component does not reach the detection limit or its content can be regarded as equivalent to an unavoidable impurity.

[0070] The second glass powder may also contain 1.0% to 10.0% SrO expressed in terms of oxide mol%. The SrO content can be set to 3.0% to 6.0%. By containing SrO, the weather resistance of the second glass powder can be improved while the viscosity of the paste can be stabilized. In addition, the second glass powder may also contain 0.0% (including substantially no) to 25.0% ZnO expressed in terms of oxide mol%. The ZnO content can be set to 1.0% to 25.0%, and can also be set to 5.0% to 25.0%. By making the second glass powder contain ZnO in the above range, the weather resistance of the glass can be improved and the viscosity of the paste can be stabilized.

[0071] The content of the glass powder is not particularly limited. For example, from the perspective of balancing the adhesion to the n-type silicon semiconductor substrate and the resistance of the back electrode, the total of the first glass powder and the second glass powder is preferably 0.5 parts by mass or more and 40 parts by mass or less, and more preferably 4 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the aluminum-silicon alloy powder. In addition, as a mixing ratio of the first glass powder to the second glass powder, it is preferably in the range of second glass powder: second glass powder (mass ratio) = 1:3~3:1. Furthermore, the softening point of each glass powder is preferably below 650°C, and the volume average particle size D50 of the glass particles constituting each glass powder is preferably 1~3μm.

[0072] The conductive aluminum paste composition of the present invention is useful as a paste composition for the back electrode of the TOPCon type solar cell described initially in the specification. In addition to the invention of the conductive aluminum paste composition, the present invention also includes the invention of a TOPCon type solar cell characterized by a back electrode laminated with a fired product of the conductive aluminum paste composition.

[0073] The firing temperature when firing the coating film of the conductive aluminum paste composition is not limited as long as the desired back electrode can be formed, but the firing temperature is preferably set to 700° C. or higher. This prevents the conductive aluminum paste composition from reacting with the microcrystalline n + The silicon layer forms an alloy layer (aluminum-silicon alloy layer), which makes it easy to form the desired back electrode. The upper limit of the firing temperature is preferably lower than the melting point of the aluminum-silicon alloy powder contained in the conductive aluminum paste composition. At this time, the conductive aluminum paste composition and the microcrystalline n + It is more difficult for a silicon layer to form an alloy layer. From this perspective, the sintering temperature is preferably 900° C. or lower, more preferably 850° C. or lower, and particularly preferably 800° C. or lower.

[0074] The firing time of the coating can be appropriately determined according to the firing temperature. For example, it can be set to more than 1 minute and less than 300 minutes, preferably more than 1 minute and less than 5 minutes. The firing can be carried out in any atmosphere of air atmosphere and nitrogen atmosphere. The firing method is not particularly limited either, for example, a known heating furnace can be used for firing treatment.

[0075] Example

[0076] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.

[0077] Example 1

[0078] Aluminum-silicon alloy powder is manufactured by gas atomization. Aluminum-silicon alloy powder is manufactured in a manner that the silicon concentration reaches 36% by mass and the volume average particle size D50 reaches 6.0 μm. A lead-containing glass powder (abbreviated as P1) composed of PbO: 50.00 mol%, SiO2: 23.00 mol%, B2O3: 20.00 mol%, Al2O3: 7.00 mol% as the first glass powder and a borosilicate glass powder (abbreviated as B1) composed of B2O3: 45.50 mol%, SiO2: 7.60 mol%, CaO: 19.00 mol%, BaO: 15.90 mol%, K2O: 12.00 mol% as the second glass powder are prepared to be mixed in a mass ratio of 1:1 to form a mixed glass powder. In addition, a resin solution with a concentration of 10% by mass prepared by dissolving ethyl cellulose in diethylene glycol butyl ether is prepared as an organic carrier.

[0079] Next, 100 parts by mass of the aluminum-silicon alloy particles and 5 parts by mass of the mixed glass powder were dispersed in 30 parts by mass of the organic vehicle using a dispersing device (disperser) to obtain a conductive aluminum paste composition.

[0080] Example 2

[0081] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that a lead-containing glass powder (P2) composed of PbO: 54.40 mol%, SiO2: 12.80 mol%, B2O3: 23.50 mol%, Al2O3: 5.70 mol%, and ZnO: 3.60 mol% is used as the first glass powder.

[0082] Example 3

[0083] A conductive aluminum paste composition is obtained by the same method as Example 1, except that a lead-containing glass powder (P3) consisting of the first glass powder composed of PbO: 45.00 mol%, SiO2: 15.00 mol%, B2O3: 30.00 mol%, Al2O3: 7.00 mol%, and ZnO: 3.00 mol% is used.

[0084] Example 4

[0085] A conductive aluminum paste composition was obtained in the same manner as in Example 1, except that a lead-containing glass powder (P4) composed of 60.00 mol% PbO, 14.00 mol% SiO2, 22.00 mol% B2O3, and 4.00 mol% Al2O3 was used as the first glass powder.

[0086] Example 5

[0087] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that a lead-containing glass powder (P5) composed of PbO: 63.00 mol%, SiO2: 8.00 mol%, B2O3: 22.00 mol%, Al2O3: 3.00 mol%, and ZnO: 4.00 mol% is used as the first glass powder.

[0088] Example 6

[0089] A conductive aluminum paste composition was obtained in the same manner as in Example 1, except that a lead-containing glass powder (P6) composed of PbO: 66.00 mol%, SiO2: 1.00 mol%, B2O3: 32.00 mol%, and Al2O3: 1.00 mol% was used as the first glass powder.

[0090] Example 7

[0091] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that a lead-containing glass powder (P7) composed of PbO: 71.00 mol%, SiO2: 16.00 mol%, and B2O3: 13.00 mol% is used as the first glass powder, and a borosilicate glass powder (B2) composed of B2O3: 43.70 mol%, SiO2: 7.10 mol%, CaO: 18.00 mol%, BaO: 15.10 mol%, SrO: 4.70 mol%, and K2O: 11.40 mol% is used as the second glass powder.

[0092] Example 8

[0093] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that a borosilicate glass powder (B3) composed of B2O3: 52.60 mol%, SiO2: 8.70 mol%, CaO: 6.40 mol%, BaO: 18.40 mol%, and K2O: 13.90 mol% is used as the second glass powder.

[0094] Example 9

[0095] A conductive aluminum paste composition is obtained by the same method as in Example 5, except that borosilicate glass powder (B4) composed of B2O3: 41.20 mol%, SiO2: 6.90 mol%, CaO: 17.30 mol%, BaO: 14.50 mol%, and K2O: 20.10 mol% is used as the second glass powder.

[0096] Example 10

[0097] A conductive aluminum paste composition was obtained in the same manner as in Example 3 except that an aluminum-silicon alloy powder having a D50 of 6.0 μm and a silicon concentration of 30 mass % produced by a gas atomization method was used.

[0098] Embodiment 11

[0099] A conductive aluminum paste composition was obtained in the same manner as in Example 3 except that an aluminum-silicon alloy powder having a D50 of 6.0 μm and a silicon concentration of 40 mass % produced by a gas atomization method was used.

[0100] Comparative Example 1

[0101] A conductive aluminum paste composition was obtained in the same manner as in Example 1 except that an aluminum powder having a D50 of 6.0 μm (silicon concentration of 0 mass %) produced by a gas atomization method was used.

[0102] Comparative Example 2

[0103] A conductive aluminum paste composition was obtained in the same manner as in Example 1 except that an aluminum-silicon alloy powder having a D50 of 6.0 μm and a silicon concentration of 25 mass % produced by a gas atomization method was used.

[0104] Comparative Example 3

[0105] A conductive aluminum paste composition was obtained in the same manner as in Example 1, except that a lead-containing glass powder (P8) composed of PbO: 13.00 mol%, SiO2: 5.00 mol%, B2O3: 28.00 mol%, and ZnO: 54.00 mol% was used as the first glass powder.

[0106] Comparative Example 4

[0107] A conductive aluminum paste composition was obtained by the same method as in Example 1, except that a lead-containing glass powder (P9) composed of PbO: 34.00 mol%, SiO2: 57.00 mol%, B2O3: 5.00 mol%, Al2O3: 2.00 mol%, and ZnO: 2.00 mol% was used as the first glass powder.

[0108] Comparative Example 5

[0109] A conductive aluminum paste composition was obtained in the same manner as in Example 8 except that a lead-containing glass powder (P10) composed of PbO: 40.00 mol % and B2O3: 60.00 mol % was used as the first glass powder.

[0110] Comparative Example 6

[0111] A conductive aluminum paste composition was obtained in the same manner as in Example 8, except that a lead-containing glass powder (P11) composed of PbO: 47.00 mol%, SiO2: 42.00 mol%, B2O3: 8.00 mol%, and Al2O3: 3.00 mol% was used as the first glass powder.

[0112] Comparative Example 7

[0113] A conductive aluminum paste composition was obtained in the same manner as in Example 1, except that a lead-containing glass powder (P12) consisting of 54.00 mol% PbO, 15.00 mol% SiO2, 4.00 mol% B2O3, 6.00 mol% Al2O3, and 21.00 mol% ZnO was used as the first glass powder.

[0114] Comparative Example 8

[0115] A conductive aluminum paste composition was obtained in the same manner as in Example 1, except that a lead-containing glass powder (P13) composed of PbO: 74.00 mol%, SiO2: 16.00 mol%, and B2O3: 10.00 mol% was used as the first glass powder.

[0116] Comparative Example 9

[0117] A conductive aluminum paste composition was obtained in the same manner as in Example 8, except that a lead-containing glass powder (P14) composed of PbO: 76.00 mol%, SiO2: 16.00 mol%, B2O3: 4.00 mol%, and Al2O3: 4.00 mol% was used as the first glass powder.

[0118] Comparative Example 10

[0119] A conductive aluminum paste composition was obtained in the same manner as in Example 8, except that a lead-containing glass powder (P15) composed of PbO: 80.00 mol % and B2O3: 20.00 mol % was used as the first glass powder.

[0120] Comparative Example 11

[0121] A conductive aluminum paste composition was obtained in the same manner as in Example 1, except that borosilicate glass powder (B5) composed of B2O3: 52.10 mol%, SiO2: 8.50 mol%, CaO: 21.50 mol%, and BaO: 17.90 mol% was used as the second glass powder.

[0122] Comparative Example 12

[0123] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B6) composed of B2O3: 47.40 mol%, SiO2: 7.70 mol%, CaO: 19.50 mol%, BaO: 16.30 mol%, and PbO: 9.10 mol% is used as the second glass powder.

[0124] Comparative Example 13

[0125] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B7) composed of B2O3: 22.10 mol%, SiO2: 8.60 mol%, CaO: 11.40 mol%, BaO: 19.60 mol%, K2O: 6.70 mol%, and ZnO: 31.60 mol% is used as the second glass powder.

[0126] Comparative Example 14

[0127] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B8) composed of B2O3: 55.20 mol%, SiO2: 8.80 mol%, CaO: 5.30 mol%, BaO: 15.90 mol%, K2O: 9.00 mol%, and ZnO: 5.80 mol% is used as the second glass powder.

[0128] Comparative Example 15

[0129] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B9) composed of B2O3: 54.10 mol%, SiO2: 4.50 mol%, CaO: 6.00 mol%, BaO: 18.40 mol%, SrO: 4.80 mol%, K2O: 5.50 mol%, and ZnO: 6.70 mol% is used as the second glass powder.

[0130] Comparative Example 16

[0131] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B10) composed of B2O3: 38.90 mol%, SiO2: 30.70 mol%, CaO: 6.40 mol%, BaO: 12.80 mol%, and K2O: 11.20 mol% is used as the second glass powder.

[0132] Comparative Example 17

[0133] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B11) composed of B2O3: 45.50 mol%, SiO2: 8.90 mol%, CaO: 20.00 mol%, BaO: 0.40 mol%, SrO: 4.20 mol%, K2O: 14.50 mol%, and ZnO: 6.50 mol% is used as the second glass powder.

[0134] Comparative Example 18

[0135] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B12) composed of B2O3: 43.40 mol%, SiO2: 8.70 mol%, CaO: 7.90 mol%, BaO: 30.00 mol%, and K2O: 10.00 mol% is used as the second glass powder.

[0136] Comparative Example 19

[0137] A conductive aluminum paste composition was obtained in the same manner as in Example 1, except that borosilicate glass powder (B13) composed of B2O3: 45.50 mol%, SiO2: 9.90 mol%, BaO: 18.40 mol%, and K2O: 26.20 mol% was used as the second glass powder.

[0138] Comparative Example 20

[0139] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B14) composed of B2O3: 32.00 mol%, SiO2: 7.60 mol%, CaO: 35.10 mol%, BaO: 10.00 mol%, SrO: 3.30 mol%, K2O: 2.00 mol%, and ZnO: 10.00 mol% is used as the second glass powder.

[0140] Comparative Example 21

[0141] A conductive aluminum paste composition is obtained by the same method as in Example 1, except that borosilicate glass powder (B15) composed of B2O3: 39.50 mol%, SiO2: 7.60 mol%, CaO: 5.50 mol%, BaO: 9.80 mol%, K2O: 35.60 mol%, and ZnO: 2.09 mol% is used as the second glass powder.

[0142] Example 12

[0143] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder composition of borosilicate glass powder (B16) consisting of B2O3: 36.00 mol%, SiO2: 10.00 mol%, CaO: 19.00 mol%, BaO: 15.00 mol%, and K2O: 20.00 mol% is used.

[0144] Embodiment 13

[0145] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder composition of borosilicate glass powder (B18) consisting of B2O3: 43.50 mol%, SiO2: 7.10 mol%, CaO: 23.00 mol%, BaO: 15.00 mol%, and K2O: 11.40 mol% is used.

[0146] Embodiment 14

[0147] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder composition of borosilicate glass powder (B20) consisting of B2O3: 48.50 mol%, SiO2: 7.50 mol%, CaO: 18.90 mol%, BaO: 3.20 mol%, and K2O: 21.90 mol% is used.

[0148] Embodiment 15

[0149] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder is used to form a borosilicate glass powder (B22) composed of B2O3: 43.70 mol%, SiO2: 9.90 mol%, CaO: 9.00 mol%, BaO: 4.70 mol%, SrO: 5.30 mol%, K2O: 3.10 mol%, and ZnO: 24.30 mol%.

[0150] Example 16

[0151] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder is used to form a borosilicate glass powder (B23) composed of B2O3: 40.20 mol%, SiO2: 9.50 mol%, CaO: 5.00 mol%, BaO: 5.80 mol%, SrO: 3.30 mol%, K2O: 28.50 mol%, and ZnO: 7.70 mol%.

[0152] Comparative Example 22

[0153] A conductive aluminum paste composition is obtained by the same method as Example 8, except that a lead-containing glass powder (P16) consisting of the first glass powder composed of PbO: 45.00 mol%, SiO2: 27.00 mol%, B2O3: 20.00 mol%, Al2O3: 2.00 mol%, and ZnO: 6.00 mol% is used.

[0154] Comparative Example 23

[0155] A conductive aluminum paste composition was obtained in the same manner as in Example 8, except that a lead-containing glass powder (P17) consisting of the first glass powder composed of PbO: 45.00 mol%, SiO2: 16.00 mol%, B2O3: 38.00 mol%, and Al2O3: 1.00 mol% was used.

[0156] Comparative Example 24

[0157] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder composition of borosilicate glass powder (B17) consisting of B2O3: 40.00 mol%, SiO2: 11.00 mol%, CaO: 15.00 mol%, BaO: 20.00 mol%, K2O: 4.00 mol%, and ZnO: 10.00 mol% is used.

[0158] Comparative Example 25

[0159] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder is used to form a borosilicate glass powder (B19) composed of B2O3: 36.10 mol%, SiO2: 8.70 mol%, CaO: 27.10 mol%, BaO: 8.90 mol%, K2O: 9.80 mol%, and ZnO: 9.40 mol%.

[0160] Comparative Example 26

[0161] A conductive aluminum paste composition is obtained by the same method as Example 4, except that a second glass powder composition of borosilicate glass powder (B21) consisting of B2O3: 38.70 mol%, SiO2: 9.70 mol%, CaO: 8.80 mol%, BaO: 22.20 mol%, K2O: 9.50 mol%, and ZnO: 11.10 mol% is used.

[0162] (Preparation of fired substrate for contact resistance evaluation)

[0163] like Figure 1 , Figure 2As shown, an n-type silicon semiconductor substrate 1 is provided with a p-type impurity layer 2 on the opposite side thereof, and an oxide (silicon oxide) layer 3 with a thickness of 5 nm, a microcrystalline n-type semiconductor substrate 2 with a thickness of 200 nm are sequentially stacked from the inner side. + The wafer of silicon layer 4 and passivation film 5. The conductive aluminum paste composition prepared in the embodiment and comparative example was screen-printed on the back of the wafer, and the composition was set to be arranged under the conditions of 20-30μm thickness, 1mm width, 10mm length, and 1.2mm, 1.4mm, 1.6mm, 1.8mm and 2.0mm printing intervals after printing. Then, the printed laminate was placed in an infrared conveyor furnace set at 700℃ and fired at this temperature to form a back electrode 6. Thus, a fired substrate for evaluation was prepared.

[0164] (Measurement and evaluation of contact resistance)

[0165] The resistance of the obtained fired substrate for evaluation was measured using a resistance measuring instrument (product name: mΩ HiTESTER HiTESTER 3540) manufactured by HIOKI EE CORPORATION, and the resistance between the back electrode 6 and the microcrystalline n was calculated according to the TLM (Transmission Line Method). + Contact resistance of silicon layer 4. The contact resistance that can obtain good ohmic contact is 10mΩ・cm 2 the following.

[0166] (Production of Solar Cells)

[0167] On the back side of the wafer, the conductive aluminum paste composition prepared in the examples and comparative examples was printed in a comb-tooth pattern in a manner of 0.2-0.3 g / 1 battery cell, and then a silver paste for forming finger electrodes was printed on the light-receiving surface of the wafer, and a back electrode and a finger electrode were formed using an infrared conveyor furnace set at 800° C. Thus, a solar cell was manufactured.

[0168] (Whether it penetrates the passivation film and the microcrystal + Evaluation of corrosion of silicon layer 4)

[0169] After the back electrode 6 formed on the solar cell was removed by immersing it in a hydrochloric acid aqueous solution at room temperature for 60 minutes, it was observed by an optical microscope to confirm whether it penetrated the passivation film 5. The case of penetrating the passivation film 5 (burn-through) was evaluated as "A", and the case of not penetrating the passivation film 5 was evaluated as "B". In addition, for the case of penetrating the passivation film 5, a scanning electron microscope (SEM) was used to observe whether the microcrystalline n + Silicon layer 4. There will be no erosion of microcrystals n +The evaluation of the silicon layer 4 is "A", and the microcrystalline n + The case of silicon layer 4 was evaluated as "B". The case of no penetration of passivation film 5 was not confirmed as to whether the microcrystalline n was corroded. + Silicon layer 4 is therefore recorded as "-".

[0170] The above results are shown in Table 1.

[0171] [Table 1]

[0172] As shown in Table 1, it was confirmed that by containing aluminum-silicon alloy powder and glass powder of the specific composition specified in the present invention, in the formation of the back electrode of the TOPCon type solar cell, the paste itself has the property of burning through the passivation film without forming LCO, and further, good ohmic contact can be obtained without forming an n-type silicon substrate and an alloy layer.

[0173] Description of Reference Numerals

[0174] 1: n-type silicon semiconductor substrate; 2: p-type impurity layer; 3: oxide layer; 4: microcrystalline n + Silicon layer; 5: passivation film; 6: fired product of the conductive aluminum paste composition (back electrode).

Claims

1. A conductive aluminum paste composition for TOPCon type solar cell electrodes, which is a conductive aluminum paste composition containing aluminum-silicon alloy powder, an organic carrier and glass powder, characterized in that: (1) The silicon concentration of the aluminum-silicon alloy powder is greater than or equal to 30% by mass and less than or equal to 40% by mass; (2) The glass powder includes a first glass powder and a second glass powder, The first glass powder contains, expressed in terms of oxide mol%, 45% to 71% PbO, 5% to 35% B2O3, and 0.1% to 25.0% SiO2, wherein the content of B2O3 is x mol%, the content of SiO2 is y mol%, the content of PbO is z mol%, and the value of [(x+y) / z] is in the range of 0.40 to 1.

00. The second glass powder contains, expressed in terms of oxide mol %, 35.0% to 55.0% B2O3, 5.0% to 10.0% SiO2, 1.0% to 20.0% BaO, 5.0% to 25.0% CaO, 3.0% to 30.0% K2O, and substantially no PbO.

2. The conductive aluminum paste composition according to claim 1, wherein: The first glass powder contains, expressed as oxide mol %, Al 2 O 3 and / or ZnO in a total amount of 1% to 10%.

3. The conductive aluminum paste composition according to claim 1, wherein: The second glass powder contains 1.0% to 10.0% SrO, expressed in terms of oxide mol%.

4. A TOPCon type solar cell, wherein: A back surface electrode is stacked on a silicon semiconductor substrate, and the back surface electrode is a fired product of the conductive aluminum paste composition according to any one of claims 1 to 3.