Water-based artistic coating, preparation method and construction process

By using a combination of aqueous emulsion, potassium silicate and titanium dioxide in artistic paints, combined with specific coating ratios and construction processes, the problem of formaldehyde exceeding the standard caused by existing coatings is solved, and a more environmentally friendly and economical decorative effect is achieved.

CN118994974APending Publication Date: 2024-11-22GUI ZHOU FU SE XIN XING CAI LIAO YOU XIAN GONG SI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411093189.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing wallpapers and oily artistic paints can easily cause formaldehyde in the room to exceed the standard during the decoration process, affecting the air quality, and have a high preparation cost.

Method used

Using water-based art paints, the VOC index is reduced through the combination of aqueous emulsion, potassium silicate and titanium dioxide, and a two-layer coating process, including primer and topcoat, combined with specific ratios and process flows, reduce material use and Preparation cost.

Benefits of technology

It effectively reduces indoor formaldehyde volatility, improves air quality, and saves material use and preparation costs, providing an environmentally friendly decoration solution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of artistic coatings, and provides a water-based artistic coating, a preparation method and a construction process, the water-based artistic coating comprises two layers of coatings including a primer and a finish, the primer comprises the following components in parts by mass: 100-120 parts of a water-based emulsion, 550-759 parts of water, 2-3 parts of a wetting agent and 120-170 parts of inorganic potassium silicate; the finishing paint is prepared from the following components in parts by mass: 458 to 724 parts of water, 200 to 240 parts of a thickening agent, 70 to 100 parts of titanium dioxide and 20 to 30 parts of an auxiliary agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of artistic coatings, and in particular to a water-based artistic coating, a preparation method and a construction process. Background Art

[0002] In the current home decoration, the walls of the house need further decoration. Most of the wall decoration solutions on the market are divided into wallpaper, latex paint and artistic paint. Wallpaper and latex paint can easily cause formaldehyde to exceed the standard in the room. Even after formaldehyde removal treatment, it will continue to volatilize.

[0003] Oil-based artistic paints also have the above-mentioned formaldehyde problem, which affects the air quality in the room. For this reason, we propose a water-based artistic paint, a preparation method and a construction process. Summary of the invention

[0004] 1. Technical issues to be solved

[0005] In view of the deficiencies in the prior art, the present invention provides a water-based artistic paint, a preparation method and a construction process. By using water-based emulsion, potassium silicate and titanium dioxide, the VOC index in the overall paint is reduced, which greatly avoids the impact of formaldehyde volatilization on indoor air quality. At the same time, it can also save material usage to a certain extent and reduce preparation costs.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A water-based artistic paint, characterized in that it comprises: two layers of paint, divided into a primer and a topcoat, the components of the primer comprising, by mass ratio, 100-120 parts of water-based emulsion, 550-759 parts of water, 2-3 parts of wetting agent, and 120-170 parts of inorganic potassium silicate; the components of the topcoat comprising, by mass ratio, 458-724 parts of water, 200-240 parts of thickener, 70-100 parts of titanium dioxide, and 20-30 parts of additives.

[0009] Preferably, the auxiliary agent includes 6-9 parts of dispersant, 4-6 parts of defoamer, and 10-15 parts of drying agent.

[0010] Preferably, the aqueous emulsion is a styrene-acrylic copolymer emulsion, and the wetting agent is a polyether-modified polysiloxane.

[0011] Preferably, the thickener is bentonite, the main component of which is montmorillonite minerals, with a content of between 85% and 90%.

[0012] Preferably, the dispersant is an anionic dispersant, the defoaming agent is mineral oil and the drier is a rare earth element drier.

[0013] A method for preparing a water-based artistic paint, used for preparing the water-based artistic paint according to any one of claims 1 to 5, characterized in that it comprises

[0014] S1. First prepare the required raw materials and weigh them according to the proportion;

[0015] S2, add water, aqueous emulsion and wetting agent to the stirring tank in sequence and stir evenly;

[0016] S3, then add inorganic potassium silicate into the stirring kettle, set the speed to 800r / min, and the time is 15min;

[0017] S4, storing the primer after stirring and mixing;

[0018] S5. Weigh the materials needed for topcoat according to the proportion;

[0019] S6, add water, thickener, titanium dioxide and additives into a stirring tank in sequence and stir evenly at a speed of 1000r / min for 8min;

[0020] S7. Take out the prepared topcoat and store it.

[0021] A construction process of a water-based artistic paint, used for constructing the water-based artistic paint of any one of claims 1 to 5, characterized in that it comprises

[0022] A1. First dry the construction surface to ensure that the temperature of the construction surface meets the construction requirements;

[0023] A2. Then, roll the primer on the construction surface for the first time and let it solidify. Then, roll the primer for the second time 2 hours after the first time.

[0024] A3. Then roll the topcoat evenly onto the primer and wait for it to dry;

[0025] A4. Check whether there are gaps or missing parts on the wall after construction and fill them up.

[0026] (III) Beneficial effects

[0027] The embodiment of the present invention provides a water-based artistic paint, a preparation method and a construction process, which have the following beneficial effects:

[0028] By using water-based emulsion, potassium silicate and titanium dioxide, the VOC index in the overall coating can be reduced, which can greatly prevent the indoor air quality from being affected by formaldehyde volatilization. At the same time, it can also save material usage and reduce preparation costs to a certain extent. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] A water-based artistic paint includes two layers of paint, which are divided into a primer and a topcoat. The primer is applied to the construction surface after drying. The components of the primer (according to the mass ratio) include: 100 parts of water-based emulsion, 550 parts of water, 2 parts of wetting agent, and 120 parts of inorganic potassium silicate; the components of the topcoat (according to the mass ratio) include: 458 parts of water, 200 parts of thickener, 70 parts of titanium dioxide, and 20 parts of additives. The additives include a dispersant, a defoamer, and a drying agent.

[0032] Furthermore, the aqueous emulsion is a styrene-acrylic copolymer emulsion, and the wetting agent is a polyether-modified polysiloxane.

[0033] The thickener is further bentonite, the main component of which is montmorillonite minerals, with a content of between 85% and 90%.

[0034] The additives include 6 parts of dispersant, 4 parts of defoamer and 10 parts of drying agent.

[0035] The dispersant is an anionic dispersant.

[0036] The defoamer is mineral oil.

[0037] The drying agent is a rare earth element drying agent.

[0038] Embodiment 2:

[0039] A water-based artistic paint includes two layers of paint, which are divided into a primer and a topcoat. The primer is applied to the construction surface after drying. The components of the primer (according to the mass ratio) include: 120 parts of water-based emulsion, 759 parts of water, 3 parts of wetting agent, and 170 parts of inorganic potassium silicate; the components of the topcoat (according to the mass ratio) include: 724 parts of water, 240 parts of thickener, 100 parts of titanium dioxide, and 30 parts of additives, wherein the additives include a dispersant, a defoamer, and a drying agent.

[0040] Furthermore, the aqueous emulsion is a styrene-acrylic copolymer emulsion, and the wetting agent is a polyether-modified polysiloxane.

[0041] The thickener is further bentonite, the main component of which is montmorillonite minerals, with a content of between 85% and 90%.

[0042] The auxiliary agents include 9 parts of dispersant, 6 parts of defoamer and 15 parts of drying agent.

[0043] The dispersant is an anionic dispersant.

[0044] The defoamer is mineral oil.

[0045] The drying agent is a rare earth element drying agent.

[0046] Embodiment 3:

[0047] A water-based artistic paint includes two layers of paint, which are divided into a primer and a topcoat. The primer is applied to a construction surface after drying. The components of the primer (according to the mass ratio) include: 110 parts of water-based emulsion, 655 parts of water, 3 parts of wetting agent, and 150 parts of inorganic potassium silicate; the components of the topcoat (according to the mass ratio) include: 591 parts of water, 225 parts of thickener, 85 parts of titanium dioxide, and 25 parts of additives, wherein the additives include a dispersant, a defoamer, and a drying agent.

[0048] Furthermore, the aqueous emulsion is a styrene-acrylic copolymer emulsion, and the wetting agent is a polyether-modified polysiloxane.

[0049] The thickener is further bentonite, the main component of which is montmorillonite minerals, with a content of between 85% and 90%.

[0050] The auxiliary agents include 7 parts of dispersant, 5 parts of defoamer and 13 parts of drying agent.

[0051] The dispersant is an anionic dispersant.

[0052] The defoamer is mineral oil.

[0053] The drying agent is a rare earth element drying agent.

[0054] Preparation method of water-based art paint:

[0055] S1. First prepare the required raw materials and weigh them according to the proportion;

[0056] S2, add water, aqueous emulsion and wetting agent to the stirring tank in sequence and stir evenly;

[0057] S3, then add inorganic potassium silicate into the stirring kettle, set the speed to 800r / min, and the time is 15min;

[0058] S4, storing the primer after stirring and mixing;

[0059] S5. Weigh the materials needed for topcoat according to the proportion;

[0060] S6. Add water, thickener, titanium dioxide and additives into the stirring tank in sequence and stir evenly at a speed of 1000 r / min for 8 minutes.

[0061] S7. Take out the prepared topcoat and store it.

[0062] Construction technology of water-based art paint

[0063] A1. First dry the construction surface to ensure that the temperature of the construction surface meets the construction requirements;

[0064] A2. Then, roll the primer on the construction surface for the first time and let it solidify. Then, roll the primer for the second time 2 hours after the first time.

[0065] A3. Then roll the topcoat evenly onto the primer and wait for it to dry.

[0066] A4. Check whether there are gaps or missing parts on the wall after construction and fill them up.

[0067] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0068] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A water-based artistic paint, characterized in that: include: The two-layer coating is divided into a primer and a topcoat. The components of the primer include, by mass ratio, 100-120 parts of aqueous emulsion, 550-759 parts of water, 2-3 parts of wetting agent, and 120-170 parts of inorganic potassium silicate; the components of the topcoat include, by mass ratio, 458-724 parts of water, 200-240 parts of thickener, 70-100 parts of titanium dioxide, and 20-30 parts of additives.

2. A water-based artistic paint according to claim 1, characterized in that: The auxiliary agent includes 6-9 parts of dispersant, 4-6 parts of defoamer and 10-15 parts of drying agent.

3. A water-based artistic paint as claimed in claim 2, characterized in that: The aqueous emulsion is a styrene-acrylic copolymer emulsion, and the wetting agent is a polyether-modified polysiloxane.

4. A water-based artistic paint as claimed in claim 3, characterized in that: The thickener is bentonite, the main component of which is montmorillonite minerals, with a content of 85% to 90%.

5. A water-based artistic paint according to claim 1, characterized in that: The dispersant is an anionic dispersant, the defoamer is mineral oil and the drier is a rare earth element drier.

6. A method for preparing a water-based artistic coating, for preparing the water-based artistic coating according to any one of claims 1 to 5, characterized in that: include S1. First prepare the required raw materials and weigh them according to the proportion; S2, add water, aqueous emulsion and wetting agent to the stirring tank in sequence and stir evenly; S3, then add inorganic potassium silicate into the stirring kettle, set the speed to 800r / min, and the time is 15min; S4, storing the primer after stirring and mixing; S5. Weigh the materials needed for topcoat according to the proportion; S6, add water, thickener, titanium dioxide and additives into the stirring tank in sequence and stir evenly at a speed of 1000r / min for 8min; S7. Take out the prepared topcoat and store it.

7. A construction process of a water-based artistic paint, used for constructing the water-based artistic paint of any one of claims 1 to 5, characterized in that: include A1. First dry the construction surface to ensure that the temperature of the construction surface meets the construction requirements; A2. Then, roll the primer on the construction surface for the first time and let it solidify. Then, roll the primer for the second time 2 hours after the first time. A3. Then roll the topcoat evenly onto the primer and wait for it to dry; A4. Check whether there are gaps or missing parts on the wall after construction and fill them up.

Citation Information

Patent Citations

  • Waterborne coating with cracking effect

    CN105949970A

  • Anti-scrubbing aqueous inorganic odorless inner wall latex paint and preparation method thereof

    CN109401468A

  • Inorganic fireproof artistic coating for wall decoration and preparation method of inorganic fireproof artistic coating

    CN112898807A

  • Beaded colored clay art coating and preparation method thereof

    CN113528022A

  • Spraying type water-based inorganic multicolor fantasy-color coating

    CN114437601A