Smelting method for producing cold forging steel in low-iron-consumption mode and improving C content at end point of converter

By optimizing operations during blast furnace tapping and converter smelting, the problem of insufficient carbon content at the converter endpoint in cold heading steel under low iron consumption mode was solved, improving steel quality and reducing production costs. This method is suitable for low-cost and high-efficiency production of high-quality cold heading steel.

CN118996035APending Publication Date: 2024-11-22WUHAN IRON & STEEL GRP ECHENG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411209276.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Under the low iron consumption production mode, the carbon content at the converter endpoint of cold heading steel is insufficient, which leads to difficulties in refining and deoxidation, low alloy recovery rate, high consumption of deoxidation materials, and difficulty in controlling the inclusion and gas content in the steel, thus affecting the quality of steel.

Method used

By adding scrap steel and baking it during blast furnace tapping, the temperature of molten iron is controlled; during converter smelting, the use of flux and oxygen lance operation are optimized, combined with bottom blowing argon stirring, to ensure that the carbon content at the converter endpoint reaches more than 0.10%, thereby reducing the oxygen content of molten steel.

Benefits of technology

This technology enables the increase of converter final carbon content under low iron consumption mode, improves steel quality, reduces production costs and energy consumption, and enhances product competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a smelting method for producing cold forging steel in a low-iron-consumption mode and increasing the converter end point C content, which comprises the following steps of: firstly, ensuring heat balance required by converter smelting through measures of adding part of scrap steel into a molten iron tank for baking, stabilizing the components of molten iron, increasing the temperature of molten iron entering the converter, baking alloy behind the converter, tapping at low temperature and the like; secondly, through oxygen lance position and oxygen flow control in the smelting process and a reasonable slagging system, rapid P removal in the low flux amount smelting middle stage, rapid heating in the smelting later stage and bottom argon blowing before tapping are achieved to further homogenize the temperature and reduce the oxygen content in steel, so that heat loss in the smelting process is reduced, and converter end point carbon is increased; according to the method, the principle of the converter smelting process is deeply studied, and the method for improving the converter end point carbon content in the low-iron-loss mode is explored, so that the product quality of the cold forging steel is guaranteed, a foundation is laid for low-cost production of high-quality cold forging steel, and meanwhile the market competitiveness of the product is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, in particular to a smelting method for producing cold heading steel in a low iron consumption mode and increasing the C content at the converter end point. Background Art

[0002] The main raw materials for converter steelmaking are molten iron and scrap steel. Due to the difference in energy consumption per ton of steel between molten iron and scrap steel, reducing molten iron consumption can effectively reduce the energy consumption per ton of crude steel in steel enterprises and reduce carbon emissions. In addition, due to the limitation of ironmaking capacity, reducing molten iron consumption can give full play to steelmaking capacity and production efficiency, and reduce production costs and energy and power consumption.

[0003] Cold heading steel is usually formed by one or more impact loading at room temperature and is widely used in automobiles, shipbuilding, machinery, white appliances, electronics, furniture, construction fasteners, connectors (such as screws, bolts, nuts, pins, rivets, etc.). With the development of the national economy, the demand for high-strength cold heading steel is increasing. Cold heading steel is in line with national policies in reducing energy consumption and improving product materials. Strengthening the quality control of this material is conducive to improving the economic benefits of steel companies and upstream and downstream companies, thus becoming a key production variety for the adjustment of product structure of various steel companies.

[0004] Cold heading steel has high quality requirements. Good steel deoxidation is beneficial to reducing inclusions in the steel and preventing pores and cracks on the surface of the steel, thereby improving the surface and internal quality of the steel. In the low iron consumption production mode with molten iron consumption ≤730kg / t, due to the insufficient chemical heat of the main raw materials of the converter, it is easy to cause imbalance in the smelting heat balance, low carbon at the converter end (C content is only 0.06-0.08%), and even overoxidation of molten steel, which makes refining and deoxidation difficult in the production of cold heading steel, low alloy recovery rate, high consumption of deoxidation materials, and difficult control of inclusions and gas content in the steel, which has a great impact on the quality of the steel. How to increase the carbon content at the converter end when producing cold heading steel under the low iron consumption mode requires the support of new technologies. Summary of the invention

[0005] The main purpose of the present invention is to provide a smelting method for producing cold heading steel in a low iron consumption production mode with a molten iron consumption of ≤730kg / t, in which the C content at the converter end point is only 0.06-0.08% using a conventional process, and even molten steel is overoxidized, resulting in difficulties in subsequent refining and deoxidation, low alloy recovery rate, high consumption of deoxidation materials, and difficulty in controlling the content of inclusions and gas in the steel, which has a significant impact on the quality of the steel.

[0006] A smelting method for producing cold heading steel in a low iron consumption mode to increase the C content at the converter end point comprises the following steps: (1) Blast furnace iron tapping: Scrap steel is added to the empty molten iron tank after the converter is ironed in time, with the added amount being 50-70kg / t steel. After the molten iron tank is added with scrap steel, it is transported to the bottom of the blast furnace for online baking for 1.0-2.0h to ensure that the surface temperature of the scrap steel is ≥400℃. The molten iron temperature of the blast furnace is ≥1500℃, and the amount of molten iron per tank is accurately controlled at 725-732kg / t steel. After the blast furnace is tapped, a high turnover rate heat preservation mode is used to transport the molten iron tank to ensure that the molten iron temperature is ≥1340℃ when entering the converter. (2) Converter smelting: After the converter is loaded with steel, the whole slag is retained to reduce lime consumption. The remaining scrap steel is added after the slag splashing to protect the furnace. The target lime consumption for converter smelting is ≤32kg / t, the amount of magnesium balls is controlled at 3.0-3.5kg / t (the MgO content in the slag is controlled in the range of 4-6%), and the sodium-containing slag-reducing agent is controlled at 1-1.5kg / t. Reducing the total flux amount is conducive to reducing heat loss in the smelting process and achieving the high carbon target at the end point; (3) 0.5 min after the converter starts to blow and stabilize, lime and magnesium balls are added in 8-10 batches, 500-800 kg per batch. Sodium-containing slagging agent is added 2 min after the start of blowing. The above three fluxes are added within 8-10 min of smelting, thereby improving the slagging effect in the early stage of the converter; (4) After the oxygen lance under the converter is ignited normally, the oxygen flow rate in the early stage of smelting is 36000-38000Nm 3 / h control, the gun position is controlled at 1400-1600mm, rapid heating and slag melting, ensuring the slag is thoroughly melted; (5) According to the real-time monitoring system of the smelting process, when the temperature of the molten steel in the furnace reaches 1400℃, the oxygen lance position is raised to 1700-2000mm and the oxygen flow rate is reduced to 28000-30000Nm 3 / h, ensuring that the temperature of the molten steel in the furnace is maintained at 1400-1450℃ for 4-5min, so that the slag and molten steel are fully mixed under this low temperature condition, achieving a better early dephosphorization effect; (6) When the monitoring system shows that the temperature of the molten steel in the furnace rises to 1500-1520℃, the lower auxiliary lance measures the temperature. The heating time is determined according to the actual temperature of the molten steel measured by TSC in the furnace. It is usually calculated at 30-40℃ / min. The oxygen lance position is pressed to 1200-1400mm and the oxygen flow rate is 36000-38000Nm 3 / h control, rapid heating; (7) After the final temperature of the molten steel reaches the requirement, the oxygen lance is raised to stop blowing oxygen, and the auxiliary lance is lowered to measure the temperature TSO, so that both the temperature and the final carbon are hit to prevent re-blowing. The C and P of the final sample are analyzed, and the final C: 0.10-0.20%, the final P ≤ 0.015%, the steel tapping temperature: 1580-1600℃, and the converter smelting target is achieved; (8) After stopping oxygen blowing, the bottom blowing argon flow rate is increased from 1200Nm3 / h in the normal smelting process to 1800Nm3 / h, and pure bottom blowing argon stirring is carried out. The stirring time is controlled at 4.5-5.5min to further reduce the oxygen content of the molten steel to 200-300ppm; (9) Steel tapping: The steel tapping process is normally carried out after the furnace alloying. An alloy baking device is installed after the converter to bake the alloyed alloy after the furnace. The baking time is controlled at 20-25 minutes and the baking temperature is 300-400℃. Alloy baking is beneficial to control the temperature of the molten steel in the ladle above 1530℃ after lowering the steel tapping temperature of the converter, preventing the blockage of the ladle transparent bricks and ensuring the normal smelting operation of the subsequent steps.

[0007] The converter described in the present invention is a 130t top and bottom double-blown converter.

[0008] In the above method, the molten iron in step (1) contains the following chemical components in percentage by weight: C: 4.0-4.5%, Mn: 0.20-0.40%, Si: 0.35-0.60%, P≤0.140%, S≤0.035%.

[0009] In the above method, the quality requirements of lime in step (2) are: the mass fraction of CaO ≥ 90%, the activity ≥ 380ml; the quality requirements of magnesium balls are: the mass fraction of MgO ≥ 70%, the mass fraction of SiO2 ≤ 5%; the sodium-containing slagging agent contains the following chemical components in mass percentage: F: 3-8%, CaO: 3-8%, Al2O3: 15-20%, Fe2O3: 35-45%, Na2O: 20-30%, and the rest are impurities.

[0010] The principle of converter metallurgy is to rely on the elements such as C, Mn, Si in the oxidized iron water to provide chemical heat energy to melt the scrap steel and increase the temperature of the molten steel, remove the P in the steel, and ensure that the subsequent steps can carry out the smelting operation normally. In the low iron consumption production mode, the C at the converter end must be controlled above 0.10% due to process requirements. The principle of the technical solution of the present invention is: first, by adding some scrap steel to the molten iron tank for baking, stabilizing the composition of the molten iron, increasing the temperature of the molten iron entering the furnace, baking the alloy after the furnace, and tapping at low temperature, the heat balance required for converter smelting is ensured; second, by controlling the position of the oxygen lance and the oxygen flow rate during the smelting process, and a reasonable slag making system, the P can be quickly removed in the middle stage of low flux smelting, and the temperature can be quickly increased in the later stage of smelting. Bottom blowing of argon before tapping further evens out the temperature and reduces the oxygen content in the steel, thereby reducing the heat loss during the smelting process and increasing the carbon at the converter end.

[0011] The beneficial effects of the present invention are as follows: (1) Through the operation of this technology, when producing cold heading steel, the converter final carbon content can be controlled above 0.10% under the low iron consumption production mode of molten iron consumption ≤730kg / t, which reduces the original oxygen content of molten steel, reduces the refining operation pressure, creates better conditions for controlling the inclusion and gas content in steel, and thus improves product quality; (2) Carbon-retaining steelmaking is achieved in the low iron consumption mode, meeting the requirements of low-carbon, environmentally friendly, green and high-quality development. In addition, due to the reduction of oxygen content in molten steel after converter steelmaking, steel material consumption is stably controlled below 1062kg / t, and alloy consumption is further reduced (residual Mn in steel is increased from 0.08% to 0.12%, silicon-manganese alloy recovery rate is increased from 95% to 97%, and total aluminum consumption is reduced from 2.6kg / t to 1.8kg / t), thus reducing production costs; (3) This smelting technology can be extended and applied to the production of other industrial materials.

[0012] The method of the present invention conducts in-depth research on the principles of the converter smelting process and explores a method to increase the converter final carbon content (to above 0.10%) under a low iron consumption mode, thereby ensuring the product quality of cold heading steel, laying a foundation for the low-cost production of high-quality cold heading steel, and greatly improving the market competitiveness of the product. DETAILED DESCRIPTION

[0013] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely exemplary of the technical solution of the present invention and do not limit the present invention in any form. The serial numbers of the following embodiments are only for description and do not represent the advantages and disadvantages of the embodiments.

[0014] The following is an example of the production of cold heading steel SWRCH35K using the existing 130-ton combined blowing converter of a steel plant as the basis, using the 130-ton top and bottom combined blowing converter - LF furnace - billet continuous casting machine process flow. A total of 8 furnaces were produced, and the specific smelting parameters and processes are as follows.

[0015] Table 1 below is a list of chemical composition tests of molten iron in various embodiments of the present invention; Table 2 below is a list of molten iron consumption, scrap steel consumption, steel production, etc. in various embodiments of the present invention; Table 3 below is a list of results of solvent consumption in various embodiments of the present invention; Table 4 below is a list of main production process parameter values ​​for various embodiments of the present invention; Table 5 below is a list of the detection results at the end point of the molten steel converter in various embodiments of the present invention.

[0016] A smelting method for producing cold heading steel in a low iron consumption mode to increase the C content at the converter end point in each embodiment of the present invention comprises the following steps: (1) Blast furnace iron tapping: Scrap steel is added to the empty molten iron tank after the converter is ironed in time, with the added amount being 50-70kg / t steel. After the molten iron tank is added with scrap steel, it is transported to the bottom of the blast furnace for online baking for 1.0-2.0h to ensure that the surface temperature of the scrap steel is ≥400℃. The molten iron temperature of the blast furnace is ≥1500℃, and the amount of molten iron per tank is accurately controlled at 725-732kg / t steel. After the blast furnace is tapped, a high turnover rate heat preservation mode is used to transport the molten iron tank to ensure that the molten iron temperature is ≥1340℃ when entering the converter. (2) Converter smelting: After the converter is loaded with steel, the whole slag is retained to reduce lime consumption. The remaining scrap steel is added after the slag splashing to protect the furnace. The target lime consumption for converter smelting is ≤32kg / t, the amount of magnesium balls is controlled at 3.0-3.5kg / t (the MgO content in the slag is controlled in the range of 4-6%), and the sodium-containing slag-reducing agent is controlled at 1-1.5kg / t. Reducing the total flux amount is conducive to reducing heat loss in the smelting process and achieving the high carbon target at the end point; (3) 0.5 min after the converter starts to blow and stabilize, lime and magnesium balls are added in 8-10 batches, 500-800 kg per batch. Sodium-containing slagging agent is added 2 min after the start of blowing. The above three fluxes are added within 8-10 min of smelting, thereby improving the slagging effect in the early stage of the converter; (4) After the oxygen lance under the converter is ignited normally, the oxygen flow rate in the early stage of smelting is 36000-38000Nm 3 / h control, the gun position is controlled at 1400-1600mm, rapid heating and slag melting, ensuring the slag is thoroughly melted; (5) According to the real-time monitoring system of the smelting process, when the temperature of the molten steel in the furnace reaches 1400℃, the oxygen lance position is raised to 1700-2000mm and the oxygen flow rate is reduced to 28000-30000Nm 3 / h, ensuring that the temperature of the molten steel in the furnace is maintained at 1400-1450℃ for 4-5min, so that the slag and molten steel are fully mixed under this low temperature condition, achieving a better early dephosphorization effect; (6) When the monitoring system shows that the temperature of the molten steel in the furnace rises to 1500-1520℃, the lower auxiliary lance measures the temperature. The heating time is determined according to the actual temperature of the molten steel measured by TSC in the furnace. It is usually calculated at 30-40℃ / min. The oxygen lance position is pressed to 1200-1400mm and the oxygen flow rate is 36000-38000Nm 3 / h control, rapid heating; (7) After the final temperature of the molten steel reaches the requirement, the oxygen lance is raised to stop blowing oxygen, and the auxiliary lance is lowered to measure the temperature TSO, so that both the temperature and the final carbon are hit to prevent re-blowing. The C and P of the final sample are analyzed, and the final C: 0.10-0.20%, the final P ≤ 0.015%, the steel tapping temperature: 1580-1600℃, and the converter smelting target is achieved; (8) After stopping oxygen blowing, the bottom blowing argon flow rate is reduced from 1200Nm 3 / h increased to 1800Nm 3 / h, pure bottom blowing argon stirring, stirring time controlled at 4.5-5.5min, further reducing the oxygen content of molten steel to 200-300ppm; (9) Steel tapping: The steel tapping process is normally carried out after the furnace alloying. An alloy baking device is installed after the converter to bake the alloyed alloy after the furnace. The baking time is controlled at 20-25 minutes and the baking temperature is 300-400℃. Alloy baking is beneficial to control the temperature of the molten steel in the ladle above 1530℃ after lowering the steel tapping temperature of the converter, preventing the blockage of the ladle transparent bricks and ensuring the normal smelting operation of the subsequent steps.

[0017] The converter used in each embodiment of the present invention is a 130t top and bottom blown converter.

[0018] In the above method, the molten iron in step (1) contains the following chemical components in percentage by weight: C: 4.0-4.5%, Mn: 0.20-0.40%, Si: 0.35-0.60%, P≤0.140%, S≤0.035%.

[0019] In the above method, the quality requirements of lime in step (2) are: the mass fraction of CaO ≥ 90%, the activity ≥ 380ml; the quality requirements of magnesium balls are: the mass fraction of MgO ≥ 70%, the mass fraction of SiO2 ≤ 5%; the sodium-containing slagging agent contains the following chemical components in mass percentage: F: 3-8%, CaO: 3-8%, Al2O3: 15-20%, Fe2O3: 35-45%, Na2O: 20-30%, and the rest are impurities.

[0020] Table 1 Chemical composition test list of molten iron in various embodiments of the present invention (unit: %) Table 2 List of molten iron consumption, scrap steel consumption, steel production, etc. in various embodiments of the present invention

[0021] Table 3 Results of solvent consumption in various embodiments of the present invention

[0022] Table 4 List of main production process parameter values ​​of various embodiments of the present invention Table 5 List of test results at the end point of the molten steel converter in various embodiments of the present invention

[0023] It can be seen from Table 5 above that when the method of the present invention is used to produce cold heading steel, the C content at the converter end point reaches more than 0.10%, achieving the purpose of the present invention. This shows that the method of the present invention is feasible for smelting cold heading steel and increasing the C content at the converter end point.

[0024] The above embodiments are only specific examples for explaining the present invention and do not limit the present invention in any form. Any non-substantial changes made by anyone based on the above contents and forms without departing from the protection scope of the claims of the present invention shall be deemed to fall within the protection scope of the claims of the present invention. The present invention is not limited to the above specific implementation examples.

Claims

1. A smelting method for producing cold heading steel in a low iron consumption mode to increase the C content at the converter end point, characterized in that The steps include: (1) Blast furnace iron tapping: Scrap steel is added to the empty molten iron tank after the converter is ironed in time, with the added amount being 50-70kg / t steel. After the molten iron tank is added with scrap steel, it is transported to the bottom of the blast furnace for online baking for 1.0-2.0h to ensure that the surface temperature of the scrap steel is ≥400℃. The molten iron temperature of the blast furnace is ≥1500℃, and the amount of molten iron per tank is accurately controlled at 725-732kg / t steel. After the blast furnace is tapped, a high turnover rate heat preservation mode is used to transport the molten iron tank to ensure that the molten iron temperature is ≥1340℃ when entering the converter. (2) Converter smelting: After the converter is put into the furnace and the steel is tapped, the whole slag is retained. After the slag is splashed to protect the furnace, the remaining scrap steel is added to reduce the lime consumption. The target lime consumption for converter smelting is ≤32kg / t, the amount of magnesium balls is controlled at 3.0-3.5kg / t, and the sodium-containing slag-reducing agent is controlled at 1-1.5kg / t; (3) After the converter starts to blow steadily, lime and magnesium balls are added in 8-10 batches, 500-800 kg per batch. After 2 minutes of blowing, sodium-containing slagging agent is added. The above three fluxes are added within 8-10 minutes of smelting, thereby improving the slagging effect in the early stage of the converter. (4) After the oxygen lance under the converter is ignited normally, the oxygen flow rate in the early stage of smelting is 36000-38000Nm 3 / h control, the gun position is controlled at 1400-1600mm, rapid heating and slag melting, ensuring the slag is thoroughly melted; (5) According to the real-time monitoring system of the smelting process, when the temperature of the molten steel in the furnace reaches 1400℃, the oxygen lance position is raised to 1700-2000mm and the oxygen flow rate is reduced to 28000-30000Nm 3 / h, ensuring that the temperature of the molten steel in the furnace is maintained at 1400-1450℃ for 4-5min; (6) When the monitoring system shows that the temperature of the molten steel in the furnace rises to 1500-1520℃, the lower auxiliary lance measures the temperature. The heating time is determined according to the actual measured temperature of the molten steel in the furnace, usually calculated at 30-40℃ / min. The oxygen lance position is pressed to 1200-1400mm, and the oxygen flow rate is 36000-38000Nm 3 / h control, rapid heating; (7) When the final temperature of the molten steel reaches the requirement, the oxygen lance is raised to stop blowing oxygen, and the auxiliary lance is lowered to measure the temperature, so that both the temperature and the final carbon are hit to prevent re-blowing. The C and P of the final sample are analyzed, and the final C: 0.10-0.20%, the final P ≤ 0.015%, the steel tapping temperature: 1580-1600℃, to achieve the purpose of converter smelting; (8) After stopping oxygen blowing, the bottom blowing argon flow rate is reduced from 1200Nm 3 / h increased to 1800Nm 3 / h, pure low-pressure argon stirring is carried out, and the stirring time is controlled at 4.5-5.5min to further reduce the oxygen content of the molten steel to 200-300ppm; (9) The post-furnace alloying is carried out normally during the steel-making process. An alloy baking device is installed after the converter to bake the post-furnace alloying alloy to 300-400℃.

2. The smelting method for producing cold heading steel in a low iron consumption mode to increase the C content at the converter end point according to claim 1, characterized in that: The converter is a 130t top and bottom blown converter.

3. The smelting method for producing cold heading steel in a low iron consumption mode to increase the C content at the converter end point according to claim 1, characterized in that: The molten iron in step (1) contains the following chemical components in percentage by weight: C: 4.0-4.5%, Mn: 0.20-0.40%, Si: 0.35-0.60%, P≤0.140%, S≤0.035%, and the remainder is Fe and other inevitable impurities.

4. The smelting method for producing cold heading steel in a low iron consumption mode to increase the C content at the converter end point according to claim 1, characterized in that: The quality requirements of lime in step (2) are: the mass fraction of CaO ≥ 90%, the activity ≥ 380 ml; the quality requirements of magnesium balls: the mass fraction of MgO ≥ 70%, the mass fraction of SiO2 ≤ 5%; the sodium-containing slagging agent contains the following chemical components in mass percentage: F: 3-8%, CaO: 3-8%, Al2O3: 15-20%, Fe2O3: 35-45%, Na2O: 20-30%, and the rest are impurities.