Electroplating solution capable of being used for insoluble anode and electrocoppering process thereof

By using quaternized copolymers of ether and imidazole compounds as leveling agents in high aspect ratio through-hole electroplating, and combining copper-soluble plating technology to supplement copper ions with ferrous sulfate, the high-thickness-to-diameter ratio through-hole electroplating is solved. The problems of unevenness and slow copper plating speed in electroplating achieve efficient uniform copper plating and deep plating capabilities, which are suitable for a variety of printed circuit boards.

CN118996552APending Publication Date: 2024-11-22GUANGDONG SHUO CHENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411225141.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art has problems of uneven electroplating and slow copper plating speed in high-thickness-biased through-hole electroplating, and traditional leveling agents have poor effect when plating through-hole electroplating at high-aspect ratio, which cannot meet the needs of industrial applications.

Method used

Quaternary ammonium copolymers made of polymerization of specific ether compounds and imidazole compounds are used as high aspect ratio through-hole leveling agents, combined with copper plating technology that supplements copper ions with ferrous sulfate, and plating is achieved through cyclic redox reactions. Purity and uniform electroplating of the liquid.

Benefits of technology

Achieve uniform copper plating with high thickness diameter ratio through holes, the TP value of deep plating capacity reaches more than 90%, and the board surface is bright, solving the problems of unevenness and slow copper plating speed in traditional electroplating technology, and is suitable for many types printed circuit board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024257540000071
    Figure BDA0005024257540000071
  • Figure BDA0005024257540000081
    Figure BDA0005024257540000081
  • Figure BDA0005024257540000101
    Figure BDA0005024257540000101
Patent Text Reader

Abstract

The invention relates to the technical field of electroplating (IPC classification number: C25D), in particular to an electroplating solution capable of being used for an insoluble anode and a copper electroplating process of the electroplating solution. The electroplating solution comprises the following components: 20-200g / L of 5H2O. CuSO4, 20-200g / L of Na2SO4, 20-200g / H2SO4: 120 to 300 g / L; 10 to 160 mg / L of Cl <->; 2 to 100 g / L of 7H2O. FeSO4; 0.1 mg / L to 10 mg / L of a brightening agent; the concentration of the inhibitor is 40 to 1600 mg / L; 2 to 500 mg / L of a high aspect ratio through hole leveling agent; and the solvent of the electroplating liquid is water. The electroplating liquid and the copper electroplating process provided by the invention can be used for electroplating through holes with different aperture sizes on various PCB support plates, even if the PCB is subjected to chemical copper plating treatment, flash copper plating treatment, black hole treatment, black shadow treatment and conductive film treatment, the through holes can be subjected to uniform copper plating, and the electroplating effect is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electroplating technology (IPC classification number: C25D), and in particular to an electroplating solution that can be used for an insoluble anode and a copper electroplating process thereof. Background Art

[0002] In recent years, printed circuit boards are one of the most important components in the electronics industry and are widely used in various fields of society. In the industry, phosphor copper anodes are the most commonly used for through-hole DC electroplating. During the dissolution process, phosphor copper anodes will still produce black insoluble substances such as cuprous phosphide, which will pollute the plating solution. Therefore, an anode bag must be installed outside the anode titanium basket to improve the purity of the plating solution. However, this method is only a temporary solution, and the coating electroplated with phosphor copper anodes is prone to defects such as burrs, pitting, and pinholes. In order to solve this problem, the industry has begun to adopt insoluble anode copper plating technology. But in this technology, the supplementation of copper ions is achieved by adding copper oxide to the solution. However, current copper plating additives often use polyethylene glycol and polyether carriers, which are easily oxidized and decomposed rapidly under the oxygen absorption of insoluble anodes, and the stability of the plating solution cannot meet the requirements of industrial applications, thus limiting its promotion and application.

[0003] On the other hand, with the continuous advancement of electronic information technology, electronic products and equipment are becoming thinner and lighter, and tend to be miniaturized and integrated. As a carrier of electronic components, the design and manufacture of circuit boards are also rapidly developing in the direction of high-density interconnection and small-hole technology. As a conductive hole connecting different layers, through-holes have gradually become one of the core technologies for achieving inter-layer interconnection. However, for the electroplating process of high aspect ratio through-holes, there are still problems such as uneven current density distribution and poor mass transfer of plating solution in the hole, which leads to a decrease in the uniformity of the plating layer and the crystallization quality of the copper layer, which cannot meet the needs of customers.

[0004] In order to solve the copper plating problem of high aspect ratio through-holes, researchers began to explore the leveling agent in depth. The leveling agent plays an important role in the copper plating leveling agent system. Its content in the through-hole copper plating solution is low, and it has little effect on the low current density area in the hole. However, there are relatively few studies on high aspect ratio through-hole electroplating leveling agents, and most of the widely used leveling agents on the market are monopolized by large foreign companies. Chinese patent CN117107310A discloses a hole-filling leveling agent, which is polymerized from nitrogen-containing heterocyclic compounds and polyol glycidyl ethers; however, the electroplating effect of this technology is still defective when applied to through-holes with high aspect ratios, and it cannot meet the use requirements.

[0005] Therefore, there is an urgent need to develop a technical solution suitable for high aspect ratio through-hole electroplating to make the plating solution purer, effectively improve the coating appearance of the circuit board, as well as the uniformity of the coating on the board surface and in the hole, and enhance the through-hole deep plating capability. Summary of the invention

[0006] The present invention provides an innovative high aperture ratio through-hole leveler for copper-dissolving electroplating copper process with an insoluble anode and its combination and application. It can electroplate through-holes with different aperture sizes on various PCB (printed circuit board) carriers. For PCB boards that have been treated with chemical copper plating, flash copper plating, black hole treatment, black shadow treatment, and conductive film treatment, it can be uniformly copper plated to make the TP value (deep plating capability) better and the board surface bright. It can copper plate circuit boards with a thickness and aperture of 8:1 or more, and the deep plating capability TP value can reach more than 90%, which has a significant effect in solving the problems of uneven electroplating and slow copper plating speed in traditional electroplating processes.

[0007] In view of some problems existing in the prior art, the first aspect of the present invention provides an electroplating solution that can be used for an insoluble anode, the components of the electroplating solution comprising:

[0008] 5H2O·CuSO4: 20-200g / L;

[0009] H2SO4: 120-300g / L;

[0010] Cl - : 10-160mg / L;

[0011] 7H2O·FeSO4: 2-100g / L;

[0012] Brightener: 0.1-10mg / L;

[0013] Inhibitor: 40-1600mg / L;

[0014] High aspect ratio through-hole leveler: 2-500mg / L;

[0015] The solvent of the plating solution is water.

[0016] Further preferably, the components of the electroplating solution include:

[0017] 5H2O·CuSO4:40-100g / L

[0018] H2SO4: 180-240g / L;

[0019] Cl - : 40-100mg / L;

[0020] 7H2O·FeSO4: 5-50g / L;

[0021] Brightener: 1-6mg / L;

[0022] Inhibitor: 100-1000mg / L;

[0023] High aspect ratio through-hole leveler: 10-200mg / L;

[0024] The solvent of the plating solution is water.

[0025] In one embodiment, the basic component range and process conditions of the electroplating solution are as follows in Table 1:

[0026] Table 1

[0027] Components or process conditions scope Standard value <![CDATA[5H2 O·CuSO4]]> 40-100g / L 60g / L <![CDATA[H2 SO4]]> 180-240g / L 220g / L <![CDATA[Cl - ]]> 40-100mg / L 80mg / L <![CDATA[7H2 O·FeSO4]]> 5-50g / L 6g / L Brightener 1~6mg / L 3mg / L Inhibitors 100~1000mg / L 400mg / L Leveling agent 10~200mg / L 50mg / L anode Insoluble Anode Iridium-Tantalum coated titanium anode Current density 1~60ASF 5~45ASF temperature 20~35℃ 22~27℃

[0028] In some preferred embodiments, the high aspect ratio through-hole leveler is a quaternized copolymer of an ether compound and an imidazole compound.

[0029] Preferably, the weight average molecular weight of the polyol glycidyl ether substance is 300-15000.

[0030] In some preferred embodiments, the ether compound includes at least one of a quaternized copolymer of propoxyglycerol triglycidyl ether, trimethylolpropane triglycidyl ether, trimethylolethane triglycidyl ether, and glycerol triglycidyl ether.

[0031] In some preferred embodiments, the imidazole compound includes at least one of imidazole-2-carboxamide, 1H-imidazole-4-carboxamide, 1H-benzimidazole-2-carboxamide, and 1H-benzimidazole-2-sulfonamide.

[0032] In some preferred embodiments, the high aspect ratio through-hole leveler is at least one of a quaternary ammonium copolymer of imidazole-2-carboxamide / propoxyglycerol triglycidyl ether, a quaternary ammonium copolymer of 1H-imidazole-4-carboxamide / trimethylolpropane triglycidyl ether, a quaternary ammonium copolymer of 1H-benzimidazole-2-carboxamide / trimethylolethane triglycidyl ether, a quaternary ammonium copolymer of 1H-benzimidazole-2-sulfonamide / glycerol triglycidyl ether, a quaternary ammonium copolymer of imidazole-2-carboxamide / glycerol triglycidyl ether, and a quaternary ammonium copolymer of 1H-imidazole-4-carboxamide / trimethylolethane triglycidyl ether.

[0033] The present invention adopts a tertiary amine polymer or a quaternized copolymer thereof formed by polymerization of a specific ether compound and an imidazole compound, and when used for electroplating a PCB through-hole plate with an aperture ratio of 8:1, it is more conducive to the deposition inhibition at the convex part of the microscopic surface, so that the through-hole TP value is greater than 90%, the board surface is bright, and it can adapt to the processing of fine circuits and meet the requirements of fine development.

[0034] Preferably, the molar ratio of the imidazole compound to the ether compound is 0.25:0.8-1.

[0035] In some preferred embodiments, the preparation steps of the electroplating solution include: S1. subjecting an ether compound and an imidazole compound to a chelating reaction under heating conditions to obtain a tertiary amine polymer, and S2. then adding an alkyl halide to carry out a quaternization reaction to further obtain a quaternized copolymer.

[0036] Preferably, in step S1, the imidazole compound and the ether compound undergo a chelating reaction at 35-105° C. to obtain a tertiary amine polymer.

[0037] Preferably, the chelating reaction time in step S1 is 2-18 hours.

[0038] Preferably, in step S2, the molar ratio of the tertiary amine polymer to the alkyl halide is 1:0.2-2.

[0039] Preferably, the alkyl halides in the present application include tert-butyl chloride, benzyl chloride, and phenyl halides containing substituted or unsubstituted C1-C4 alkyl groups.

[0040] More preferably, the halogen of the phenyl halide containing a substituted or unsubstituted C1-C4 alkyl group is chlorine, such as o-chloroanisole, m-chloroanisole, p-chloroanisole, 2,4-dichloroanisole, 2,6-dichloroanisole and the like.

[0041] Preferably, the temperature of the quaternization reaction in step S2 is 85-105°C.

[0042] Preferably, the quaternization reaction time in step S2 is 4 to 18 hours.

[0043] Preferably, the weight average molecular weight of the inhibitor is 400-20,000.

[0044] Further preferably, the inhibitor is selected from one or more of PEG1500, PEG20000, and 50HB-400.

[0045] Preferably, the brightener is a compound of sodium 3-mercaptopropane sulfonate and sodium polydisulfide propane sulfonate, and the mass concentration ratio of sodium 3-mercaptopropane sulfonate to sodium polydisulfide propane sulfonate is 0.02-0.2:1.

[0046] A second aspect of the present invention provides a copper-dissolving electroplating process for an insoluble anode, the copper-dissolving electroplating process comprising the following steps:

[0047] (1) Prepare electroplating solution;

[0048] (2) placing an insoluble anode in an electroplating solution to obtain a plating solution 1 through an electroplating reaction;

[0049] (3) returning the plating solution 1 to a copper dissolving tank containing solid copper to obtain a plating solution 2 through an oxidation-reduction reaction; (4) introducing the plating solution 2 into an electrolyte, and repeating steps (2) and (3) in sequence; and replenishing the consumed copper ions during the electroplating process through a reciprocating cycle.

[0050] Preferably, in step (1), the raw materials in the electroplating solution except 7H2O·FeSO4 are first mixed uniformly, and then 7H2O·FeSO4 is added.

[0051] The present invention adopts a copper-dissolving copper electroplating process by adding ferrous sulfate into the electroplating solution and combining it with electrolytic copper to supplement copper ions. This can avoid the aging of the bath solution caused by the introduction of excessive oxides and can also ensure the purity of the plating solution, so that industrial production can meet higher requirements.

[0052] The main idea of ​​the copper plating process of the present invention is that an adapted insoluble anode is used, ferrous sulfate is added to the plating solution, and ferrous ions are oxidized into trivalent ferrous ions on the surface of the insoluble anode; the plating solution containing the trivalent ferrous ions is returned to the pure copper block or pure copper particles in the copper dissolving tank, and the electrolysis of metallic copper is accelerated by oxidation of the trivalent ferrous ions, so that the metallic copper is converted into divalent copper ions, and the copper itself is reduced to divalent ferrous ions, and the copper ions consumed in the electroplating are replenished through a reciprocating cycle.

[0053] In some preferred embodiments, the electroplating temperature of the electroplating reaction is 20-35°C.

[0054] In some preferred embodiments, the electroplating time of the electroplating reaction is 10-240 min.

[0055] In some preferred embodiments, the electroplating reaction is specifically performed by direct current to plate copper; the current density of the direct current is 1-60ASF.

[0056] Preferably, the application scenario of the above copper electroplating process is specifically on a printed circuit board (PCB board) with multiple through holes, and copper is plated using a direct current density. The working temperature of the electroplating solution is 20-35°C.

[0057] Further preferably, the electroplating time of the PCB board is 20-180 minutes;

[0058] More preferably, the electroplating temperature is 22-27°C.

[0059] Further preferably, the current density of the DC power supply is 5-35ASF.

[0060] The method of placing the electroplating solution on the printed circuit board having a plurality of through holes in the present application is not particularly limited, and any method that can be implemented in the art can be used.

[0061] The present application does not limit the type of printed circuit board, and the thickness of the board is not limited. It can be a single-layer or multi-layer full PCB board, a graphic PCB board, an IC carrier board, a UHDI board, or other types of printed circuit boards.

[0062] The present application does not limit the specifications of the printed circuit board. For example, the thickness can be 25 to 5000 μm, the through hole diameter can be 25 to 5000 μm, and the through hole aperture ratio can be 0.5 to 10:1. Electroplating within this range can make the TP value better and the board surface glossiness high. In particular, for electroplating through holes with an aperture ratio of 8:1, the TP value is >90%, the board surface is bright, and the electroplating effect is significant.

[0063] Beneficial effects:

[0064] The present invention provides an electroplating solution that can be used for an insoluble anode and a copper electroplating process thereof, which has the following advantages:

[0065] (1) The present invention preferably uses a quaternized copolymer formed by polymerization of a specific imidazole compound and an ether compound as a high aspect ratio through-hole leveling agent, and cooperates with other components in the electroplating solution to effectively control the copper electroplating process of the through-hole, so that the entire board can be uniformly electroplated during the through-hole copper plating process, the copper plating solution has a good through-hole deep plating ability, the through-hole TP value is high, the through-hole mouth has no tailing or shoulder cutting, there is no broken copper or cracks in the hole, and the board surface is bright without pitting, copper nodules or pinholes.

[0066] (2) The electroplating solution provided by the present invention can be used to electroplate through holes of different aperture sizes on various types of PCB substrates. Even if the PCB board has been treated with chemical copper plating, flash copper plating, black hole treatment, black shadow treatment, or conductive film treatment, its through holes can be uniformly copper plated to achieve a better TP value and a bright board surface. This is something that existing leveling agents cannot do.

[0067] (3) The copper plating solution provided by the present invention can meet the more refined requirements of single-layer or multi-layer comprehensive PCB boards, graphic PCB boards, IC carrier boards and UHDI boards or other types of printed circuit boards, and has a wide range of applications and strong feasibility.

[0068] (4) The copper dissolving electroplating process provided by the present invention, through ingenious design and conception, can achieve a uniform and bright coating during the electroplating process, and can also replenish the copper ions consumed in the electroplating process through reciprocating cycles, thus achieving multiple goals at one stroke.

[0069] (5) The raw materials of the electroplating solution of the present invention are cheap and easily available, the process is simple and controllable, and it can be applied to printed circuit boards of various types and scenarios. It has strong practicality and can realize large-scale industrial production, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1: Schematic diagram of through-hole cross section; A, B, C, D are the surface copper thickness, E, F are the thinnest hole copper thickness;

[0071] Figure 2 : Electroplating section diagram of chemical copper-plated through-hole board, which is the overall effect diagram of through-hole after electroplating using the leveling agent and electroplating solution of Example 1 of the present invention;

[0072] Figure 3 : A cross-section diagram of electroplating of a chemical copper-plated through-hole board, which is a diagram showing the electroplating effect of the through-hole mouth after electroplating using the leveling agent and the electroplating solution of Example 1 of the present invention;

[0073] Figure 4 : A cross-section diagram of electroplating of a chemical copper-plated through-hole board, which is a diagram showing the electroplating effect of the middle of a through-hole after electroplating using the leveling agent and the electroplating solution of Example 1 of the present invention;

[0074] Figure 5 : The through-hole plate electroplating section diagram after black shadow treatment is the overall effect diagram of the through-hole after electroplating using the leveling agent and electroplating solution of Example 1 of the present invention;

[0075] Figure 6 : A cross-section diagram of a through-hole plate electroplated with a black shadow treatment, which is a diagram showing the electroplating effect of the through-hole mouth after electroplating using the leveling agent and the electroplating solution of Example 1 of the present invention;

[0076] Figure 7 : A cross-section diagram of a through-hole plate electroplated with a black shadow treatment, which is a diagram showing the electroplating effect of the middle of a through-hole after electroplating using the leveling agent and the electroplating solution of Example 1 of the present invention;

[0077] Figure 8 : Electroplating section diagram of through-hole flash-plated board, which is the overall effect diagram of through-hole after electroplating using the leveling agent and electroplating solution of Example 1 of the present invention;

[0078] Fig. 9 : A cross-section of a through-hole flash-plated board, which is a diagram showing the electroplating effect of the through-hole mouth after electroplating using the leveling agent and the electroplating solution of Example 1 of the present invention;

[0079] Fig.10 : A cross-section diagram of a through-hole flash-plated board, which is a diagram showing the electroplating effect in the middle of a through-hole after electroplating using the leveling agent and the electroplating solution of Example 1 of the present invention; DETAILED DESCRIPTION

[0080] Example

[0081] An electroplating solution that can be used for an insoluble anode: The components of the electrolyte are shown in Table 2 below, and the solvent of the electroplating solution is water. Unless otherwise specified, the chloride ions of the present invention are provided by hydrochloric acid.

[0082] The high aspect ratio through-hole leveler in Examples 1-8 is a quaternized copolymer of an ether compound and an imidazole compound, as shown in Table 2. The ether compound and the imidazole compound are reacted with corresponding monomers selected according to Examples 1-8.

[0083] The preparation method of the high aspect ratio through-hole leveler comprises: adding 100 mmol of an ether compound to a round-bottom reaction flask at room temperature (25°C), then adding 40 mL of deionized water, filling with nitrogen protection, and adding 100 mmol of an imidazole compound at a constant temperature and pressure (control to complete the dripping within 15 minutes) under a nitrogen environment at 95°C, and then keeping the temperature at 95°C for 10 hours. Continue to increase the temperature to 100°C, and then add 50 mmol of benzyl chloride to the reaction flask at a constant pressure (control to complete the dripping within 8 minutes), continue to heat at 100°C for 6 hours, and then stir at room temperature (25°C) for another 5 hours to finally obtain an amber reaction product, which is washed and diluted with a 0.5 wt% sulfuric acid aqueous solution. (Note: The dilution multiple is not limited, and no further purification is required; it can be added according to the required amount of leveler)

[0084] In Example 1-8, the brightener is sodium 3-mercaptopropane sulfonate (CAS No. 17636-10-1) and sodium polydisulfide propane sulfonate (CAS No. 27206-35-5), and the mass ratio of sodium 3-mercaptopropane sulfonate to sodium polydisulfide propane sulfonate is 0.3:3.

[0085] In Examples 1-8, the inhibitor is PEG20000.

[0086] Table 2

[0087]

[0088]

[0089] A copper-dissolving electroplating process for insoluble anodes, comprising the following specific steps:

[0090] (1) Inorganic drag cylinder;

[0091] (2) Organic drag cylinder;

[0092] (3) electroplating reaction to obtain plating solution 1;

[0093] (4) returning the plating solution 1 to the copper dissolving tank containing solid copper to obtain the plating solution 2 through oxidation-reduction reaction;

[0094] (5) Then, the second plating solution is introduced into the electrolyte, and steps (3) and (4) are repeated in sequence; the consumed copper ions are replenished during the electroplating process through the reciprocating cycle.

[0095] Step (1) includes: adding inorganic components in the electrolyte to the test line plating tank in sequence, and the adding order and operation are specifically as follows: adding 2 / 3 of the volume of deionized water in the formula to the test line plating tank, starting the circulation, filtering and temperature control system; slowly adding H2SO4, and the temperature in the bath cannot exceed 50°C; adding 5H2O·CuSO4; hanging an iridium-tantalum coated titanium anode wrapped in a double-layer anode bag; replenishing the water level, adjusting and analyzing H2SO4, 5H2O·CuSO4, Cl - After concentration, add 7H2O·FeSO4, add 1 / 2-2 / 3 of the volume of pure copper particles to the copper dissolving tank; install a carbon core in the filter barrel of the test line tank to filter the electroplating tank liquid to remove the organic pollutants that may remain in the tank liquid; the electroplating tank liquid is dragged at a current density of 10ASF for 2 hours; after the dragging is completed, use Hullcell sheets to confirm the contaminants in the tank liquid; electrolyze the Hullcell sheet at a current of 2A for 10 minutes, and the Hullcell sheet is required to be non-glossy after electroplating. If it is shiny, it is necessary to continue electrolysis and carbon core filtering;

[0096] (2) Adding plating solution and dragging tank: adding organic components in the plating solution in sequence, and then performing organic dragging tank, electroplating the dragging tank for 4 hours under 5ASF conditions, analyzing the plating solution, and then continuously electroplating the dragging tank at 10ASF for at least 4AH / L; after the dragging tank is completed, electroplating is performed;

[0097] (3) Electroplating conditions: working temperature: 23-25℃; operating parameters: 20ASF×60min. The anode is a Machnetal iridium-tantalum coated titanium mesh anode with low light agent consumption, and the PCB electroplating board is the cathode. The anode and cathode area ratio is 1:2; the stirring method is spray convection stirring and cathode moving stirring; the filtering method is Zhengye brand conventional 20-inch electroplating copper cylinder filter barrel with cotton core continuous filtration.

[0098] During the electroplating process, the plating solution is maintained continuously: the plating solution lost due to evaporation can be replenished with deionized water; 5H2O·CuSO4, H2 SO4, Cl are analyzed regularly - and 7H2O·FeSO4 concentration; and adjust the concentration of additive leveler / brightener / inhibitor according to the CVS analysis results. The copper source is added by adding pure copper, and the iron content is adjusted by analyzing the ferrous content and ferric iron content to adjust the plating solution.

[0099] The redox reaction in step (4) is Cu 0 +2Fe 3+ →2Fe 2+ +Cu 2+ The copper dissolving condition is 25℃ to achieve cyclic copper dissolving.

[0100] In step (5), the plating solution is circulated to dissolve copper until the line is shut down.

[0101] Performance Testing Methods

[0102] The electroplated product of Example 1 was tested using the following electroplating test board. The test results are shown in Tables 3 and Figure 2-10 Furthermore, embodiments 2 to 8 can achieve similar electroplating effects as embodiment 1.

[0103] Conventional through-hole board: board size 40.64*50.8cm 2 , with a thickness of 1.6mm, and a through hole with an aperture of 200μm, and the through hole aperture ratio is 8:1. The test board can be treated with chemical copper plating, black shadow treatment, or flash copper plating after chemical copper plating before testing.

[0104] Through hole plating capability (TP value) evaluation method: Figure 1 As shown in the figure, the ratio of the copper thickness in the center of the through hole after electroplating to the copper thickness on the board surface is the TP value, and the calculation formula is: TP=2(E+F) / (A+B+C+D)*100%.

[0105] Current efficiency n = actual copper thickness / theoretical copper thickness × 100%.

[0106] Performance test data

[0107] Table 3

[0108]

[0109] Based on the test results in Table 3 and Figure 2-10 It can be seen from the electroplating effect that the through-hole electroplating results of the electroplating solutions of Examples 1-8 are excellent. It can be seen from the test results that the average TP of the through-hole AR=8:1 is greater than 88%. The present invention has excellent electroplating effects on through-holes with different aspect ratios on PCB boards, especially high aspect ratio through-holes, and can meet actual performance requirements.

Claims

1. A plating solution for an insoluble anode, It is characterized in that The components of the electroplating solution include: 5H 2 O·CuSO 4 : 20-200g / L; H 2 I AM 4: 120-300g / L; Cl - :10-160mg / L; 7H 2 O·FeSO 4 :2-100g / L; Brightener: 0.1-10mg / L; Inhibitor: 40-1600mg / L; High aspect ratio through-hole leveler: 2-500mg / L; The solvent of the plating solution is water.

2. The electroplating solution according to claim 1, It is characterized in that The components of the electroplating solution include: 5H 2 O·CuSO 4 :40-100g / L H 2 SO 4 :180-240g / L; Cl - :40-100mg / L; 7H 2 O·FeSO 4 :5-50g / L; Brightener: 1-6mg / L; Inhibitor: 100-1000mg / L; High aspect ratio through-hole leveler: 10-200mg / L; The solvent of the plating solution is water.

3. The electroplating solution according to claim 1, It is characterized in that The high aspect ratio through-hole leveler is a quaternized copolymer of an ether compound and an imidazole compound.

4. The electroplating solution according to claim 3, It is characterized in that The ether compound includes at least one of a quaternized copolymer of propoxyglycerol triglycidyl ether, trimethylolpropane triglycidyl ether, trimethylolethane triglycidyl ether, and glycerol triglycidyl ether.

5. The electroplating solution according to claim 3, It is characterized in that The imidazole compound includes at least one of imidazole-2-carboxamide, 1H-imidazole-4-carboxamide, 1H-benzimidazole-2-carboxamide, and 1H-benzimidazole-2-sulfonamide.

6. The electroplating solution according to claim 3, It is characterized in that The high aspect ratio through-hole leveler is at least one of a quaternary ammonium copolymer of imidazole-2-carboxamide / propoxyglycerol triglycidyl ether, a quaternary ammonium copolymer of 1H-imidazole-4-carboxamide / trimethylolpropane triglycidyl ether, a quaternary ammonium copolymer of 1H-benzimidazole-2-carboxamide / trimethylolethane triglycidyl ether, a quaternary ammonium copolymer of 1H-benzimidazole-2-sulfonamide / glycerol triglycidyl ether, a quaternary ammonium copolymer of imidazole-2-carboxamide / glycerol triglycidyl ether, and a quaternary ammonium copolymer of 1H-imidazole-4-carboxamide / trimethylolethane triglycidyl ether.

7. A copper-dissolving electroplating process for insoluble anodes, It is characterized in that The copper dissolving type electroplating copper process comprises the following steps: (1) Prepare electroplating solution; (2) placing an insoluble anode in an electroplating solution to obtain a plating solution 1 through an electroplating reaction; (3) returning the plating solution 1 to the copper dissolving tank containing solid copper to obtain the plating solution 2 through oxidation-reduction reaction; (4) Then, the second plating solution is introduced into the electrolyte, and steps (2) and (3) are repeated in sequence; the consumed copper ions are replenished during the electroplating process through the reciprocating cycle.

8. The copper dissolving electroplating process according to claim 7, It is characterized in that The electroplating temperature of the electroplating reaction is 20-35°C.

9. The copper dissolving electroplating process according to claim 7, It is characterized in that The electroplating time of the electroplating reaction is 10-240 minutes.

10. The copper dissolving electroplating process according to claim 7, It is characterized in that The electroplating reaction specifically uses direct current to plate copper; the current density of the direct current is 1-60ASF.