Bump structure for solving PA layer cracks and reflow soldering cracks of Non-PI flip chip and preparation process
By setting up a tin-copper metal alloy layer and annular Ni layer on the bump copper column of the flip chip, and using the groove design, the problem of easy cracking of the Ni layer under the copper column is solved, reducing tin crawling phenomenon and enhancing welding The reliability effect significantly reduces the crack risk of PA layer and reflow soldering, and improves the packaging quality of the chip.
Patent Information
- Application Number
- CN202411115383.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the Ni layer plated under the copper column of the flip chip is prone to cracks at the solder joints, resulting in the product after reflow soldering being easily broken under the action of external forces.
Design a bump structure, including a tin copper metal alloy layer and annular Ni layer at the center of the top of the bump copper column, a tin copper metal alloy layer is formed by reflow soldering, and a groove is opened at the center of the top of the copper column to enhance The embedding effect of solder, controlling the width and cross-sectional area of the Ni layer to optimize the solder quality.
It effectively reduces the crack risk of PA layer and reflow soldering, enhances the reliability of solder joints, ensures the thickness and shape of the tin-copper metal alloy layer, and improves the packaging quality and reliability of the overall chip.
Smart Images

Figure CN119008563A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flip chip packaging, and in particular to a bump structure and a preparation process for solving cracks in a PA layer of a Non-PI flip chip and cracks in a reflow soldering process. Background Art
[0002] For flip-chip (Non-PI) chips, when the bump structure is copper pillar + solder, there will be uneven tin creeping on both sides of the copper pillar during the reflow soldering process. The uneven tin creeping phenomenon will cause the solder thickness under the copper pillar to become thinner. When the molten tin is converted into a solid state, there will be different pulling forces on both sides of the copper pillar, resulting in irreversible cracks in the PA layer on the chip surface, such as Figure 1 shown.
[0003] In order to improve the cracking caused by the uneven tin creeping phenomenon and the welding stress caused by the thin solder under the copper pillar, the current bump process is to plate a Ni layer between the copper pillar and the solder, which can effectively improve the uneven tin creeping phenomenon on both sides of the copper pillar, increase the solder thickness under the copper pillar, and have a better buffering effect on the stress of the reflow soldering cooling stage. Figure 2 However, after reflow soldering, no metal alloy layer is formed between the Ni layer and the solder (such as Figure 3 ), the Ni layer and the solder interface become the most vulnerable part of the solder joint. When the product after reflow soldering is subjected to external bending or deformation, cracks are likely to occur at the solder joint, and the fracture surface is between the Ni layer and the solder (such as Figure 4 ). Summary of the invention
[0004] In view of the problem in the prior art that cracks are easily generated at the solder joints of the Ni layer and solder plated under the copper pillars of the flip chip, the present invention provides a bump structure and a preparation process for solving cracks in the PA layer of the Non-PI flip chip and reflow cracks.
[0005] The present invention is achieved through the following technical solutions:
[0006] A bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering comprises a bump copper column, a tin-copper metal alloy layer and a Ni layer. The tin-copper metal alloy layer is arranged at the top center of the bump copper column, and the Ni layer is arranged in a ring shape on the top of the bump copper column.
[0007] Preferably, the width of the Ni layer is 1 / 3 to 1 / 2 of the radius of the copper column of the bump.
[0008] Preferably, the cross-sectional area of the Ni layer is 1 / 3 to 1 / 2 of the top surface area of the copper pillar of the bump.
[0009] Preferably, the tin-copper IMC layer is formed by solder and copper bump pillars through a reflow process.
[0010] Preferably, before reflow soldering, the height of the solder is 30-38 μm.
[0011] Preferably, before reflow soldering, the top center of the copper pillar of the bump is not plated with a Ni layer, and a groove is provided at the top center thereof; after reflow soldering, part of the tin-copper metal alloy layer is located in the groove.
[0012] Preferably, after reflow soldering, the depth of the groove is less than 1 / 2 of the thickness of the tin-copper metal alloy layer.
[0013] Preferably, after reflow soldering, the top plane of the Sn-Cu metal alloy layer is higher than the top plane of the Ni layer.
[0014] A process for preparing a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering, comprising the following steps:
[0015] S1, firstly, plating of the copper pillars of the bumps is performed;
[0016] S2, plating a Ni layer on the top surface of the bump copper column;
[0017] S3, solder is plated on the upper surface of the Ni layer to obtain a pre-product;
[0018] S4, reflow soldering is performed on the pre-product to obtain a bump structure.
[0019] A Non-PI flip chip comprises the bump structure for solving the cracks of the PA layer and the reflow cracks of the Non-PI flip chip.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention discloses a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering. By arranging a semi-Ni layer between a bump copper column and solder, after reflow soldering, not only the tin creeping on both sides of the bump copper column is reduced, but also an effective tin-copper metal alloy layer is formed, and the reliability of the solder joint is increased, and it is not easy to break.
[0022] Furthermore, the Ni layer is arranged in a ring-shaped form on the top of the copper column of the bump, and its width or cross-sectional area accounts for a certain proportion (such as 1 / 3 to 1 / 2) of the top of the copper column of the bump. Such a design not only ensures sufficient connection area, but also reduces the influence of the Ni layer on the formation of the tin-copper metal alloy layer, which helps to optimize the welding quality. The width of the Ni layer is limited. If the width of the Ni layer is large, the stress solder joint of the frame is disconnected after reflow soldering; if the width of the Ni layer is too small, the solder cannot be effectively blocked during the welding process, and tin creeping will occur on the side of the copper column.
[0023] In the preparation process of a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering, a Ni layer is plated on the top surface of the bump copper column, but avoiding the top center area. This step can be achieved by a mask or other technology that accurately controls the position of the plating layer. The Ni layer acts as a barrier layer, which can reduce the direct reaction between copper and solder, and improve the reliability of soldering. Solder is plated on the upper surface of the Ni layer (excluding the part covered by the Ni layer) to form a pre-product. The height of the solder should be controlled within a certain range to ensure that the thickness of the alloy layer after reflow soldering is moderate. The pre-product is subjected to reflow soldering treatment, so that the solder reacts with the bump copper column to generate a tin-copper metal alloy layer. During the reflow soldering process, since the top center of the bump copper column is not plated with a Ni layer and may be provided with a groove, the solder can partially penetrate into the groove to form a more secure connection. At the same time, by controlling the reflow soldering conditions, it is ensured that the top plane of the tin-copper metal alloy layer is higher than the top plane of the Ni layer, and the performance of the bump structure is further optimized. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the prior art without PI wafer + without Ni layer bump and with tin creeping;
[0025] Figure 2 It is a schematic diagram of adding a Ni layer between the copper pillar and the solder without tin creep in the prior art;
[0026] Figure 3 It is a schematic diagram of a metal alloy layer formed by welding a copper pillar without a Ni layer and a solder in the prior art;
[0027] Figure 4 It is a schematic diagram of a prior art in which there is a Ni layer bump and the Ni layer and the solder do not form a metal alloy layer after reflow;
[0028] Figure 5 is a schematic diagram of a bump structure of the present invention;
[0029] Figure 6 is a schematic diagram of a metal alloy layer in a bump structure of the present invention;
[0030] Figure 7 This is the process flow for preparing the bump structure of the present invention;
[0031] Figure 8 It is a schematic diagram of the bump structure of the present invention before reflow soldering.
[0032] In the figure, 1. copper pillar bump; 2. tin-copper metal alloy layer; 3. Ni layer; 4. solder. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0034] In the description of the present invention, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal connection of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0035] The present invention discloses a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering, referring to Figure 5 , including a bump copper pillar 1, a tin-copper metal alloy layer 2 and a Ni layer 3, wherein the tin-copper metal alloy layer 2 is arranged at the top center of the bump copper pillar 1, and the Ni layer 3 is arranged in a ring shape on the top of the bump copper pillar 1. The bump copper pillar 1 serves as the basis of the bump structure and is used to provide necessary mechanical support and electrical connection functions.
[0036] The width of the Ni layer 3 is 1 / 3 to 1 / 2 of the radius of the bump copper column 1, and the cross-sectional area of the Ni layer 3 is 1 / 3 to 1 / 2 of the top surface area of the bump copper column 1. The thickness of the Ni layer 3 in this embodiment is the same as the thickness of the Ni layer 3 of the bump in the prior art, which is 3 μm. The thickness of the Ni layer 3 is limited. If the Ni layer 3 is too thick, the production cost of the bump is higher, and if the Ni layer 3 is too thin, the Ni layer 3 cannot block the welding of tin and copper.
[0037] The tin-copper metal alloy layer 2 is formed by solder 4 and the copper pillar 1 through a reflow process. Before reflow, the height of the solder 4 is 30-38 μm. The tin-copper metal alloy layer 2 can enhance the bonding force between the copper pillar and the solder, which helps to improve the reliability of the bump structure.
[0038] Reference Figure 5Before reflow soldering, the top center of the copper pillar 1 is not plated with Ni layer 3, and a groove is provided at the top center thereof; after reflow soldering, part of the tin-copper alloy layer 2 is located in the groove. This design enables the tin-copper alloy layer 2 to be partially embedded in the groove during the reflow soldering process, further increasing the bonding strength between the solder 4 and the copper pillar 1, and reducing the risk of cracks. At the same time, after reflow soldering, the depth of the groove is less than 1 / 2 of the thickness of the tin-copper alloy layer 2, and the top plane of the tin-copper alloy layer 2 is higher than the top plane of the Ni layer 3.
[0039] The present invention discloses a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in a reflow soldering process. By arranging a semi-Ni layer 3 between a bump copper pillar 1 and a solder 4, after reflow soldering, not only the creeping tin on both sides of the bump copper pillar 1 is reduced, but also an effective tin-copper metal alloy layer is formed, and the reliability of the solder joint is increased, and it is not easy to break (such as Figure 6 shown).
[0040] The present invention effectively reduces cracks generated in the PA layer and the reflow soldering process of the Non-PI flip chip by optimizing the bump structure, especially the annular design of the Ni layer 3 and the formation of the tin-copper metal alloy layer 2. At the same time, by accurately controlling the height of the solder and the reflow soldering conditions, it is ensured that the thickness and shape of the tin-copper metal alloy layer 2 meet the design requirements, thereby optimizing the connection quality between the bump and the substrate.
[0041] The present invention also discloses a process for preparing a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in a reflow soldering process. Figure 7 , 8 , including the following steps:
[0042] S1, firstly plating the bump copper column 1;
[0043] S2, plating a Ni layer 3 on the top surface of the bump copper column 1;
[0044] S3, plating solder 4 on the upper surface of the Ni layer 3 to obtain a pre-product;
[0045] S4, reflow soldering is performed on the pre-product to make the solder react with the copper pillar of the bump to form a tin-copper metal alloy layer to obtain a bump structure. During the reflow soldering process, the solder is partially embedded in the groove to enhance the bonding force.
[0046] The present invention also discloses a Non-PI flip chip, including a bump structure for solving cracks in the PA layer and reflow soldering cracks of the Non-PI flip chip. The bump structure is applied to the Non-PI flip chip, which can significantly reduce the crack risk of the PA layer during the manufacturing process, especially in the reflow soldering stage. Due to the blocking effect of the Ni layer and the enhanced bonding effect of the groove design, the bump structure is more stable and reliable, which helps to improve the packaging quality and reliability of the overall chip.
[0047] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.
Claims
1. A bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering, characterized in that: The invention comprises a copper bump column (1), a tin-copper metal alloy layer (2) and a Ni layer (3); the tin-copper metal alloy layer (2) is arranged at the top center of the copper bump column (1); and the Ni layer (3) is arranged in a ring shape at the top of the copper bump column (1).
2. The bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering according to claim 1, characterized in that: The width of the Ni layer (3) is 1 / 3 to 1 / 2 of the radius of the bump copper column (1).
3. The bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering according to claim 1, characterized in that: The cross-sectional area of the Ni layer (3) is 1 / 3 to 1 / 2 of the top surface area of the bump copper column (1).
4. The bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering according to claim 1, characterized in that: The tin-copper IMC layer is formed by solder (4) and a bump copper column (1) through a reflow soldering process.
5. The bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering according to claim 4, characterized in that: Before reflow soldering, the height of the solder (4) is 30 to 38 μm.
6. The bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering according to claim 1, characterized in that: Before reflow soldering, the top center of the copper pillar (1) is not plated with a Ni layer (3), and a groove is provided at the top center thereof; after reflow soldering, part of the tin-copper metal alloy layer (2) is located in the groove.
7. The bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering according to claim 6, characterized in that: After reflow soldering, the depth of the groove is less than 1 / 2 of the thickness of the tin-copper metal alloy layer.
8. The bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering according to claim 6, characterized in that: After reflow soldering, the top plane of the tin-copper metal alloy layer (2) is higher than the top plane of the Ni layer (3).
9. A process for preparing a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: S1, firstly plating the copper pillar (1); S2, plating a Ni layer (3) on the top surface of the bump copper column (1); S3, plating solder (4) on the upper surface of the Ni layer (3) to obtain a pre-product; S4, reflow soldering is performed on the pre-product to obtain a bump structure.
10. A Non-PI flip chip, characterized in that: The invention comprises a bump structure for solving cracks in the PA layer of a Non-PI flip chip and cracks in reflow soldering as described in any one of claims 1 to 8.