Aluminum ash denitrification composition and application thereof

By using the composition of CaCO3, CaO and secondary aluminum ash, the particle size and proportion are controlled, and the denitrification of aluminum ash slag is promoted, and the problem of low denitrification rate of aluminum ash slag in the prior art is solved, and high efficiency is achieved The aluminum ash slag is harmlessly treated.

CN119016490APending Publication Date: 2024-11-26NANTONG INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411311717.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the aluminum nitride nitrogen removal rate in aluminum ash slag. The ignition nitrogen removal process consumes a large energy and has a low nitrogen removal rate, and the effect of adding CaO and CaCO3 alone is not obvious.

Method used

采用CaCO3、CaO和二次铝灰的组合物,通过控制颗粒大小和比例,促进CaCO3在高温下分解生成活性[CaO]和CO2,疏松二次铝灰结构,增加空气进入,促进AlN的氧化,从而提高脱氮率。

Benefits of technology

The denitrification rate of aluminum ash slag was significantly improved to 98.37%, achieving efficient and harmless treatment of aluminum ash, surpassing the effects of the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005050855900000041
    Figure BDA0005050855900000041
Patent Text Reader

Abstract

The invention discloses an aluminum ash denitrification composition and application thereof. The composition comprises CaCO3, CaO and secondary aluminum ash, the average particle size of the CaCO3 does not exceed 1 / 2 of the average particle size of the secondary aluminum ash, the proportion of particles smaller than the average particle size of the secondary aluminum ash in the CaCO3 is at least 75%, the average particle size of the secondary aluminum ash does not exceed 1 / 2 of the average particle size of the CaO, and the proportion of particles smaller than the average particle size of the CaO in the secondary aluminum ash is at least 75%. The aluminum ash denitrification composition is further applied to aluminum ash denitrification. The specific method comprises the following steps: uniformly mixing CaCO3, CaO and secondary aluminum ash to obtain a reaction system; and roasting the reaction system under an aerobic condition to complete aluminum ash denitrification. The nitrogen removal rate of the aluminum ash can be increased to 98.37%, the nitrogen removal effect of the nitrogen removal agent is obviously higher than that of an existing nitrogen removal agent, and efficient harmless treatment of the aluminum ash can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for denitrifying aluminum ash, and in particular to an aluminum ash denitrification composition and application thereof. Background Art

[0002] As a by-product of the aluminum industry, aluminum ash is mainly composed of Al, AlN, oxides and salts, with an annual production of more than 5 million tons. Aluminum ash is usually disposed of by landfill and stacking. Due to the presence of harmful substances such as aluminum nitride (AlN), the "National List of Hazardous Wastes (2021 Edition)" lists aluminum ash produced during the processing of recycled aluminum and aluminum materials as Class R hazardous solid waste (waste code: 321-026-48). The pyrometallurgical denitrification process is mainly to remove AlN and O in aluminum ash. 2 Reacts to generate Al 2 O 3 However, due to the AlN in the aluminum ash being 2 O 3 It is difficult for the package to come into contact with the air, so the key to pyrolysis nitrogen removal is to break the membrane. In addition, the pyrolysis nitrogen removal process has a long roasting time, high temperature and high energy consumption.

[0003] Previous studies have shown that the addition of CaO and CaCO separately during pyrometallurgy can 3 , CaO and CaCO 3 The role of is to form calcium aluminate, which does not play a role in removing nitrogen. In addition, some people believe that the formed CaO is wrapped on the surface of AlN, affecting the removal of nitrogen. Some studies believe that in Na 2 In the O-CaO system, CaO only plays a role in removing Si. For example, the literature (Huan Shuxing, Wang Yaowu, Di Yuezhong, You Jing, Peng Jianping, Hong Yiming. Experimental study on the extraction of alumina by secondary calcination of aluminum ash [J]. Mineral Protection and Utilization, 2020, (3): 34-39.) believes that AlN is relatively stable and does not react with CaO even at very high temperatures. When the calcination temperature is 1000°C, the calcium oxide generated by the decomposition of calcium carbonate basically reacts completely with the alumina in the aluminum ash; for example, the literature (He Liuqing. Optimization of aluminum extraction process from aluminum ash and research on the synthesis of calcium sulfonate from its leaching residue [M]. South China University of Technology, 2021.) believes that in the Na 2 Under the action of O, calcium oxide can fix silicon oxide.

[0004] Experimental study on the removal of nitrogen from secondary aluminum ash by calcination roasting method [J]. Nonferrous Metals Engineering, 2021, 11(4): 63-69. (Li Songyuan et al.) The study found that CaO added to secondary aluminum ash can play a film-breaking role. Under certain process conditions, AlN and Al in secondary aluminum ash can be removed. 2 O 3 Transformed into 12CaO·7Al 2 O 3and N 2 However, the roasting time is long and the denitrification rate is only 85.25%. The main reason is that the research on the characteristics and theoretical analysis of CaO is not systematic enough, and a reasonable denitrification system has not yet been established. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide an aluminum ash denitrification composition to solve the problem of how to improve the denitrification rate of aluminum ash. Another purpose of the present invention is to propose the application of the aluminum ash denitrification composition in aluminum ash denitrification to solve the problem of how to denitrify aluminum ash.

[0006] Technical solution: The aluminum ash denitrification composition of the present invention comprises CaCO 3 , CaO and secondary aluminum ash, the CaCO 3 The average particle size of the secondary aluminum ash is no more than 1 / 2 of the average particle size of the secondary aluminum ash and the CaCO 3 The particles smaller than the average particle size of the secondary aluminum ash account for at least 75%, the average particle size of the secondary aluminum ash does not exceed 1 / 2 of the average particle size of CaO, and the particles smaller than the average particle size of CaO account for at least 75% of the secondary aluminum ash.

[0007] CaCO 3 -Basic principle of nitrogen removal in the CaO-aluminum ash system:

[0008] In the early stage of temperature rise (CaCO 3 When the AlN and Al in the aluminum ash are not completely decomposed, 2 O 3 Transformed into 12CaO·7Al 2 O 3 and N 2 , promoting the denitrification process, with 12CaO·7Al 2 O 3 Increase, wrap on the AlN surface, and affect the further removal of N;

[0009] CaCO 3 Decomposes at high temperature to generate active [CaO] and CO 2 .CO 2 The escape process can make the secondary aluminum ash loose, which is beneficial to the O 2 Entering, the AlN exposed outside in the secondary aluminum ash will be more easily oxidized, and the active [CaO] will play a better effect.

[0010] CaCO 3 After mixing, CaO and secondary aluminum ash, the three are evenly distributed, and some CaCO 3 The mixture of the two is evenly filled in the gaps between the particles of CaO.3 CO produced by decomposition 2 In the process of escaping from the inside to the outside, the secondary aluminum ash is made loose and porous. 2 The contact area with AlN can be increased, and the by-product N 2 Taking it out of the reaction system and promoting the forward progress of the denitrification reaction can greatly increase the denitrification rate of secondary aluminum ash.

[0011] Preferably, the CaCO 3 The average particle size of the secondary aluminum ash is 7-9 μm, and the particles with a particle size less than 15-19 μm account for 75%, the average particle size of the secondary aluminum ash is 15-19 μm, and the particles with a particle size less than 37-40 μm account for 75%, and the average particle size of the CaO is 37-40 μm.

[0012] Preferably, the CaCO 3 The average particle size is 8.752μm, of which 90% are particles with a particle size less than 22.570μm; the average particle size of the secondary aluminum ash is 16.951μm, of which 90% are particles with a particle size less than 82.510μm; the average particle size of CaO is 38.863μm, of which 90% are particles with a particle size less than 93.938μm.

[0013] The present invention further applies the aluminum ash denitrification composition to the aluminum ash denitrification, and the specific method comprises the following steps:

[0014] (1) CaCO 3 , CaO and secondary aluminum ash are uniformly mixed to obtain a reaction system;

[0015] (2) Denitrification of aluminum ash is completed after the reaction system is calcined under aerobic conditions.

[0016] Preferably, in step (1), CaCO 3 The mass ratio of CaO: secondary aluminum ash is 0.6:0.2-1:1.

[0017] Preferably, in step (2), the calcination reaction conditions are: heating the reaction system from room temperature to 900-1200° C. at a heating rate of 2-6° C. / min, calcining at this temperature for 2-6 h, and then cooling to room temperature.

[0018] Preferably, in step (2), the aerobic condition is air condition or oxygen condition.

[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0020] The invention can improve the denitrification rate of aluminum ash to 98.37%, which is significantly higher than the denitrification effect of the existing denitrifier, and can achieve efficient and harmless treatment of aluminum ash. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described below.

[0022] Example 1: A denitrification composition for aluminum ash, comprising CaCO 3 , CaO and secondary aluminum ash, the CaCO 3 The average particle size is 8.752μm, of which 90% are particles with a particle size less than 22.570μm, and 75% are particles with a particle size less than 16.472μm; the average particle size of the secondary aluminum ash is 16.951μm, of which 75% are particles with a particle size less than 32.529μm; 90% are particles with a particle size less than 82.510μm; the average particle size of CaO is 38.863μm, of which 90% are particles with a particle size less than 93.938μm.

[0023] The aluminum ash denitrification composition is subjected to denitrification treatment as follows:

[0024] (1) CaCO 3 , CaO and secondary aluminum ash are uniformly mixed in mass ratios of 0.6:0.2:1, 0.6:0.4:1, 0.6:0.6:1, 0.6:0.8:1, and 0.6:1:1 to obtain a reaction system;

[0025] (2) Under air conditions, the reaction system was heated from room temperature to 1100°C at a heating rate of 4°C / min, calcined at this temperature for 3 h, and then cooled to room temperature to complete the denitrification of aluminum ash slag.

[0026] Embodiment 2: The rest is the same as Embodiment 1, except that:

[0027] In mass ratio m CaCO3 :m CaO :m 二次铝灰 =0.6:0.6:1, and the roasting time is 180 min, the roasting temperatures are set to 900°C, 1000°C, 1100°C, and 1200°C respectively.

[0028] Embodiment 3: The rest is the same as Embodiment 1, except that:

[0029] In mass ratio m CaCO3 :m CaO :m 二次铝灰 =0.6:0.6:1. When the roasting temperature is 1100°C, the roasting times are set to 120min, 150min, 180min, 210min, and 240min respectively.

[0030] Comparative Example 1: The rest is the same as Example 1, except that:

[0031] The CaCO 3 The average particle size of is 38.545 μm, of which particles with a particle size less than 95.883 μm account for 90%, and particles with a particle size less than 66.726 μm account for 75%; the average particle size of CaO is 8.813 μm, of which particles with a particle size less than 16.318 μm account for 90%.

[0032] m CaCO3 :m CaO :m 二次铝灰 =0.6:0.6:1.

[0033] Comparative Example 2: The rest is the same as Example 1, except that:

[0034] The average particle size of the secondary aluminum ash is 39.331 μm, and the particles with a particle size less than 72.765 μm account for 75%; the particles with a particle size less than 90.263 μm account for 90%.

[0035] The average particle size of CaO is 18.235 μm, of which particles with a particle size less than 29.786 μm account for 90%.

[0036] m CaCO3 :m CaO :m 二次铝灰 =0.6:0.6:1.

[0037] Comparative Example 3: The rest is the same as Example 1, except that:

[0038] The CaCO 3 The average particle size is 18.964 μm, of which particles with a diameter less than 35.493 μm account for 90% and particles with a diameter less than 27.532 μm account for 75%;

[0039] The average particle size of the secondary aluminum ash is 9.023 μm, and the particles with a particle size less than 15.757 μm account for 75%; the particles with a particle size less than 22.672 μm account for 90%.

[0040] m CaCO3 :m CaO :m 二次铝灰 =0.6:0.6:1.

[0041] The denitrification rates of aluminum ash of Examples 1-3 and Comparative Examples 1-3 were measured. The results are as follows:

[0042] Table 1 Effect of roasting conditions and particle size configuration of denitrification system on denitrification rate.

[0043]

[0044] The results of Example 1 in Table 1 show that the denitrification rate of secondary aluminum ash increases first and then decreases with the increase of the batching mass ratio. The reason is that when the batching ratio is small, the two additives can react with the secondary aluminum ash and play a role, so the denitrification rate of secondary aluminum ash will increase. When the batching ratio increases, the 12CaO·7Al 2 O 3 The CaO that does not participate in the reaction will be wrapped in the secondary aluminum ash and CaCO 3 On the surface of the mixture, the higher the proportion of CaO, the stronger the coating of the mixture. 2 The more difficult it is for the secondary aluminum ash to participate in the reaction, the lower the denitrification rate of the secondary aluminum ash will be. The best ratio is: m CaCO3 :m CaO :m 二次铝灰 =0.6:0.6:1.

[0045] The results of Examples 2 and 3 show that when the calcination temperature is 1100°C and the calcination time is 3 hours, the denitrification rate of the secondary aluminum ash is the highest and the [CaO] activity is the highest.

[0046] Comparison of Examples 1-3 with Example 1 shows that when CaCO 3、 After the particle size configuration of secondary aluminum ash and CaO is exchanged, the denitrification rate is greatly reduced. The present invention finds that CaCO 3 The denitrification system composed of secondary aluminum ash and CaO can successfully improve the denitrification effect only under a specific relative particle size configuration. The denitrification system formed by other particle size configurations not only cannot improve the denitrification rate, but will reduce the denitrification rate.

Claims

1. An aluminum ash denitrification composition, characterized in that: It includes CaCO3, CaO and secondary aluminum ash, the average particle size of CaCO3 does not exceed 1 / 2 of the average particle size of secondary aluminum ash, and the proportion of particles smaller than the average particle size of secondary aluminum ash in CaCO3 is at least 75%, the average particle size of secondary aluminum ash does not exceed 1 / 2 of the average particle size of CaO, and the proportion of particles smaller than the average particle size of CaO in secondary aluminum ash is at least 75%.

2. The aluminum ash denitrification composition according to claim 1, characterized in that: The average particle size of the CaCO3 is 7-9 μm, and the proportion of particles with a particle size less than 15-19 μm is 75%. The average particle size of the secondary aluminum ash is 15-19 μm, and the proportion of particles with a particle size less than 37-40 μm is 75%. The average particle size of the CaO is 37-40 μm.

3. The aluminum ash denitrification composition according to claim 2, characterized in that: The average particle size of the CaCO3 is 8.752 μm, of which 90% are particles with a diameter less than 22.570 μm. The average particle size of the secondary aluminum ash is 16.951 μm, of which 90% are particles with a diameter less than 82.510 μm. The average particle size of the CaO is 38.863 μm, of which 90% are particles with a diameter less than 93.938 μm.

4. Use of the aluminum ash denitrification composition according to any one of claims 1 to 3 in aluminum ash denitrification.

5. The use according to claim 4, characterized in that: The steps include: (1) CaCO3, CaO and secondary aluminum ash are uniformly mixed to obtain a reaction system; (2) Denitrification of aluminum ash is completed after the reaction system is calcined under aerobic conditions.

6. The use according to claim 5, characterized in that: In step (1), the mass ratio of CaCO3:CaO:secondary aluminum ash is 0.6:0.2-1:

1.

7. The use according to claim 5, characterized in that: In step (2), the calcination reaction conditions are: heating the reaction system from room temperature to 900-1200° C. at a heating rate of 2-6° C. / min, calcining at this temperature for 2-6 hours, and then cooling to room temperature.

8. The use according to claim 5, characterized in that: In step (2), the aerobic condition is air condition or oxygen condition.

Citation Information

Patent Citations

  • Green and harmless resource utilization method for aluminum ashes

    CN112453009A