Fluid self-assembly method applied to micro-nano device
By performing surface energy treatment and designing solution media for micro-nano devices and assembled substrates, high precision and high efficiency of fluid self-assembly are achieved, and the problems of poor assembly accuracy and complex substrate preparation in the prior art are solved.
Patent Information
- Application Number
- CN202310605115.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
The existing fluid self-assembly technology has problems such as poor assembly accuracy, complex assembly substrate preparation, and difficult to take into account both assembly efficiency and accuracy.
By surface treatment of micro-nano devices and assembled substrates, the surface energy difference is achieved, the interface between solution A and solution B is used for primary assembly, and the solution C in the second assembly container is used to regulate the dissolution or volatility of the liquid bridge, and the second assembly container is used to achieve the second Second alignment to form the final stable assembly.
The self-assembly accuracy of fluids is improved, the preparation process of assembling substrates and micro-nano devices is simplified, the contradiction between assembly accuracy and efficiency is solved, and high-precision and high-efficiency assembly is achieved.
Smart Images

Figure CN119018841A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a fluid self-assembly method applied to micro-nano devices. Background Art
[0002] With the development and progress of science and technology, microelectronic systems have gradually developed, and a large number of micro-sized component arrays are integrated at high density on the driver circuit board to achieve functions such as display, sensing, and photoelectric conversion. For example, the micro-LED display technology that integrates tens of millions of micro-LED chips to achieve display has the advantages of high energy conversion rate, fast response speed, long service life, and high contrast compared to traditional display technology. In the preparation process of these microelectronic systems, a large number of microelectronic devices need to be integrated with high density and high precision on the driver circuit board to achieve the corresponding functions. In the face of the above needs, a high-efficiency, high-precision, high-density, and low-cost microelectronic integration technology is needed. Mass transfer technology has also come into being.
[0003] Mass transfer technology refers to the process of arranging millions or even tens of millions of small-sized micro-nano devices on the driving panel in a reasonable and orderly manner. Due to the development and progress of micro-nano manufacturing technology, high requirements are put forward for the transfer accuracy, transfer efficiency, transfer yield, cost and other aspects of mass transfer technology.
[0004] Among the existing mass transfer technology routes, fluid self-assembly technology has attracted the attention of researchers with its advantages of low cost and high efficiency. Fluid self-assembly technology uses mechanical principles such as fluid force and shape matching to allow micro-nano devices to fall into a pre-made special structure to achieve the effect of self-assembly. After the micro-nano devices are dispersed in the fluid, they achieve random movement with the help of fluid movement, and are filled and arranged by matching the shape of the groove structure on the receiving panel. Since fluid self-assembly technology does not rely on precision instruments to achieve the capture, positioning, and assembly of micro-nano devices, and the filling process is fast, efficient, and low-cost, it is considered to be the most promising mass transfer technology.
[0005] However, the existing fluid self-assembly technology has the following main disadvantages:
[0006] 1) Poor assembly precision of fluid self-assembly. In the existing fluid self-assembly based on the principle of minimizing surface free energy, the disappearance process of the liquid bridge between the micro-nano device and the assembly substrate is uncontrollable, which makes it difficult to control the process of the micro-nano device falling and assembling with the assembly substrate. The rapid removal of the liquid bridge does not allow the micro-nano device to have enough time for fine adjustment, which may cause horizontal displacement and assembly deviation. Although the absolute error generated by this process is not large, the relative error is large compared to the smaller size of the micro-nano device, which affects the subsequent bonding process.
[0007] 2) It is difficult to achieve both assembly accuracy and assembly efficiency during fluid self-assembly. In existing fluid self-assembly, the assembly process is mostly achieved by capturing micro-nano devices using grooves. In this process, when the size of the micro-nano devices is the same, the larger the groove size, the higher the efficiency of capturing the micro-nano devices. However, after the micro-nano devices fall into the groove structure, they can still move inside the structure, resulting in poor assembly accuracy. Reducing the groove size can effectively improve assembly accuracy, but it will also reduce assembly efficiency. Therefore, it is difficult for existing strategies to reconcile the contradiction between assembly accuracy and assembly efficiency.
[0008] 3) The assembly substrate needs to construct a complex three-dimensional structure. In the existing fluid self-assembly, in order for the assembly substrate to capture the micro-nano devices that move randomly in the fluid, most of the three-dimensional structures of grooves or protrusions are set on the assembly substrate to realize the assembly of the micro-devices and the assembly substrate. The preparation process of this three-dimensional structure is complicated, which greatly increases the preparation process and difficulty of the assembly substrate.
[0009] 4) Micro-nano devices need to be set up with complex structures to achieve surface selectivity during the assembly process. During the fluid self-assembly process, micro-nano devices need to be assembled on the assembly position of the assembly substrate with a specific surface to achieve specific functions. There are two main methods to achieve the surface selectivity of micro-nano devices: first, construct a special three-dimensional structure on the surface; second, adjust the center of gravity of the micro-nano device. However, these strategies require additional processes, which increases the complexity of preparation.
[0010] In view of this, the existing fluid self-assembly technology still has the problems of poor assembly accuracy, complex preparation of micro-nano devices and assembly substrates, and difficulty in balancing assembly efficiency and assembly accuracy. It is urgent for technicians in this field to provide a new strategy to solve the above problems. Summary of the invention
[0011] To this end, the present invention provides a fluid self-assembly method for microelectronic devices to solve the problems existing in the prior art.
[0012] In order to achieve the above object, the present invention provides the following technical solutions:
[0013] A fluid self-assembly method for micro-nano devices comprises the following steps:
[0014] S1. The micro-nano device and the assembly substrate are subjected to surface treatment respectively, different surfaces of the micro-nano device have different surface energies, the assembly position and the non-assembly position of the assembly substrate also have different surface energies, and the surface of the micro-nano device to be assembled and the preset assembly position of the assembly substrate have similar surface energies;
[0015] S2. In the first assembly container, the modified micro-nano device and the assembly substrate are dropped into solution B through solution A. Under external disturbance, the assembly surface of the micro-nano device and the droplets composed of solution A attached to the assembly position of the assembly substrate contact and fuse with each other to form a liquid bridge, completing one alignment and forming a primary assembly of the micro-nano device and the assembly substrate;
[0016] S3. The primary assembly is transferred to a second assembly container, and the liquid bridge composed of solution A between the micro-nano device in the primary assembly and the assembly substrate is controllably dissolved or volatilized into fluid C to complete the secondary alignment and form a final assembly;
[0017] S4. The final assembly is taken out from the second assembly container, and the final assembly consisting of the micro-nano device and the assembly substrate is post-processed to form a stable bond between the two, achieve the conduction of various physical and chemical properties, and complete the packaging process.
[0018] In some embodiments, the micro-nano device has a size ranging from nanometers to centimeters, has a columnar structure, a bottom surface of the columnar structure is a first surface, and is made of at least one of gallium nitride, silicon dioxide, metal or polymer, and has a density greater than the density of solution B.
[0019] In some embodiments, the first surface of the micro-nano device has a different surface energy from other surfaces. The surface energy of the first surface enables it to be wetted by solution A but not by solution B, and the surface energy of other surfaces enables it to be wetted by solution B but not by solution A.
[0020] In some embodiments, the shape of the assembly substrate is a plane or a curved surface, the material of the assembly substrate is metal, silicon dioxide or polydimethylsiloxane, and the assembly position on the surface of the assembly substrate is a patterned protrusion, a patterned groove or a planar structure.
[0021] In some embodiments, the surface of the assembly substrate is patterned and specifically modified so that different positions on the surface have different surface energies, the size and shape of the assembly position are consistent with the size and shape of the first surface of the micro-nano device, the surface energy of the assembly position on the assembly substrate allows it to be wetted with solution A but not with solution B, and the surface energy of the non-assembly position on the assembly substrate allows it to be wetted with solution B but not with solution A.
[0022] In some embodiments, the fluid disturbance method is a plunger pump, a circulation pump, a peristaltic pump, a brush, a shaker, an oscillation or a centrifugal method.
[0023] In some embodiments, step S2 is replaced by the following steps:
[0024] S201. The modified micro-nano devices are uniformly dispersed at the interface between solution A and solution B, and the assembly substrate is slowly inserted into the solution at any angle of 30-90°. The micro-nano devices are assembled to the assembly positions on the assembly substrate based on the interface interaction, completing one alignment and forming a primary assembly of the micro-nano devices and the assembly substrate.
[0025] In some embodiments, in step S2, the upper layer of the first assembly container is solution A, and the lower layer is solution B, and a conveying mechanism leading to the second assembly container is installed at the bottom of the first assembly container, and a flow disturbance component is installed in the first assembly container for disturbing the solution B;
[0026] The modified micro-nano device and the assembly substrate are sent to solution B through solution A. During this process, droplets composed of solution A are attached to the assembly position on the surface of the assembly substrate and the first surface of the micro-nano device;
[0027] The assembly substrate is fixed on the conveying mechanism at the bottom of the first assembly container, and the patterned specific modified surface is in contact with the solution. Under the action of the spoiler, the micro-nano device moves irregularly in the solution B. In this process, the droplets at the assembly position on the assembly substrate collide and merge with the droplets on the first surface of the micro-nano device to form a liquid bridge. Based on the interfacial tension, the micro-nano device is assembled at the assembly position of the assembly substrate, completing an alignment.
[0028] The assembly status of the assembly substrate and the micro-nano device is monitored in real time by an image monitoring device. After all assembly positions of the assembly substrate are assembled with the micro-nano device, the disturbance of solution B is stopped to form a primary assembly of the assembly substrate and the micro-nano device.
[0029] In some embodiments, in step S3, after the primary assembly is completed, the primary assembly is transferred to the second assembly container via an automatic conveying mechanism;
[0030] The primary assembly enters the second assembly container, and the liquid bridge formed by solution A between the first surface of the micro-nano device and the assembly position of the assembly substrate slowly dissolves or evaporates into fluid C. As the liquid bridge gradually becomes smaller, the relative position between the assembly position of the micro-nano device and the assembly substrate is finely adjusted due to the change in interfacial tension, completing the secondary alignment and forming the final assembly.
[0031] In some embodiments, in step S4, the final assembly is taken out from the second assembly container, and the bonding between the micro-nano device and the assembly substrate is achieved by welding, and the welded assembly continues to complete the subsequent packaging process.
[0032] In some embodiments, in step S201, the upper layer of the first assembly container is solution A, the lower layer is solution B, and an automatic conveying mechanism leading to the second assembly container is installed at the bottom of the first assembly container;
[0033] Due to the combined effect of density and surface energy, the modified micro-nano device is evenly dispersed at the interface between solution A and solution B with the first surface facing solution A.
[0034] The patterned assembly substrate is slowly inserted into the solution at any angle of 30-90°, with one side facing the solution and the other side facing the side wall of the first assembly container. During the insertion process, due to the difference in surface energy, the assembly position of the assembly substrate is at the interface between solution A and solution B, causing interface deformation, so that the first surface of the micro-nano device is assembled with the assembly position of the assembly substrate, completing an alignment, and forming a primary assembly consisting of the assembly substrate and multiple micro-nano devices. After the assembly substrate with the micro-nano device assembled is completely immersed in solution B, the angle of the assembly substrate is adjusted, and the side of the assembly substrate with the assembly position faces the solution, and is fixed on the automatic conveying mechanism at the bottom of the first assembly container.
[0035] In some embodiments, solution A and solution B are immiscible with each other, solution A and fluid C are slightly soluble, solution A is deionized water, saline solution or alkaline solution; solution B is toluene, n-hexane, cyclohexane or xylene; fluid C is ethyl acetate, chloroform, ether or nitrogen.
[0036] Compared with the existing fluid self-assembly technology, the fluid self-assembly method for micro-nano devices provided by the present invention has the following technical advantages:
[0037] 1) Improved fluid self-assembly accuracy. Through the two-step alignment assembly process, the dissolution or volatilization rate of the liquid bridge between the micro-nano device and the assembly substrate is regulated, effectively solving the problem of poor assembly accuracy caused by the relative displacement of the micro-nano chip and the assembly substrate during the rapid removal of the liquid bridge and the difficulty of fine adjustment due to rapid fixation.
[0038] 2) Simplified the preparation process of the assembly substrate. The assembly position of the assembly substrate uses similar surface energy on the plane structure to capture the micro-nano devices, avoiding the preparation of the complex three-dimensional structure of the assembly substrate and simplifying the preparation process. It also fundamentally solves the contradiction between assembly accuracy and assembly efficiency in shape matching fluid self-assembly.
[0039] 3) Simplified the preparation process of micro-nano devices. The surface energies of different surfaces of micro-nano devices are significantly different, and the surface selectivity of the assembly process can be achieved without additional structures or preparation processes. This simplifies the preparation process of micro-nano devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0041] The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with the technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantial technical significance. Any structural modification, change in proportion or adjustment in size shall still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.
[0042] Figure 1 A schematic flow chart of the fluid self-assembly method for microelectronic devices provided by the present invention;
[0043] Figure 2 A schematic diagram of the structure of a specific implementation mode of the chip provided by the present invention;
[0044] Figure 3 for Figure 2 Cross-section view along the AA direction;
[0045] Figure 4 A schematic structural diagram of a specific implementation of an assembly substrate provided by the present invention;
[0046] Figure 5 for Figure 4 Cross-section along the BB direction;
[0047] Figure 6 A schematic structural diagram of a specific embodiment of a device used in the fluid self-assembly method provided by the present invention;
[0048] Figure 7 This is a schematic diagram of a chip and an assembly substrate in a correct alignment mode in the fluid self-assembly method provided by the present invention;
[0049] Figure 8 A schematic diagram of a chip and an assembly substrate in a fluid self-assembly method provided by the present invention when they are in a misaligned state;
[0050] Fig. 9 This is a schematic structural diagram of the hot pressing process in the fluid self-assembly method provided by the present invention;
[0051] Fig.10 A schematic structural diagram of another specific embodiment of the device used in the fluid self-assembly method provided by the present invention;
[0052] Fig.11 The present invention is a schematic structural diagram of another specific implementation of the device used in the fluid self-assembly method provided by the present invention.
[0053] Description of reference numerals:
[0054] 1- Chip;
[0055] 12-first electrode, 13-second electrode, 14-insulating layer;
[0056] 2- Assemble the substrate;
[0057] 22- a third electrode, 23- a fourth electrode;
[0058] 31-first assembly container, 32-second assembly container, 33-isolation plate A, 34-isolation plate B, 35-conveyor belt, 361-solution A, 362-solution B, 363-fluid C, 37-image monitoring system, 38-plunger pump, 391-discharge valve, 392-temperature and pressure regulating device;
[0059] 41-Hot-press welding plate. DETAILED DESCRIPTION
[0060] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the technology can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0061] The fluid self-assembly method for micro-nano devices provided by the present invention performs surface treatment on the micro-nano devices and the assembly substrate 2 so that the assembly surface of the micro-nano devices and the assembly position of the assembly substrate 2 have similar surface energies. The modified micro-nano devices and the assembly substrate 2 are placed in a pre-built first assembly container 31. In the disturbed fluid, the assembly surface of the micro-nano devices and the droplets attached to the assembly position of the assembly substrate 2 contact and fuse with each other to form a liquid bridge, completing an alignment to form a primary assembly of the micro-nano devices and the assembly substrate 2; the primary assembly is transferred to the second assembly container 32, and then the liquid bridge between the micro-nano devices and the assembly substrate 2 in the primary assembly slowly dissolves or evaporates to complete the secondary alignment to form a final assembly. The fluid self-assembly method for micro-nano devices provided by the present invention has the advantages of high assembly accuracy and simple structure of the micro-nano devices and the assembly substrate 2. The method can be used in Micro-LED display, flexible solar cells, microelectronics integration, flexible electronics, micro robots, automotive lighting and other fields.
[0062] In a specific embodiment, Figure 1 As shown, the fluid self-assembly method for micro-nano devices provided by the present invention comprises the following steps:
[0063] S1. The micro-nano device and the assembly substrate 2 are subjected to surface treatment respectively. Different surfaces of the micro-nano device have different surface energies, and the assembly position and the non-assembly position of the assembly substrate 2 also have different surface energies. The surface to be assembled of the micro-nano device and the preset assembly position of the assembly substrate 2 have similar surface energies.
[0064] Among them, the micro-nano device can be of nanometer to centimeter size, and its shape can be any columnar structure such as a cube, a cuboid, a cylinder, etc., and one bottom surface of the columnar structure is the first surface. Its material can be composed of a single or composite material such as gallium nitride, silicon dioxide, metal, polymer, etc. The overall density of the micro-nano device should be slightly greater than the density of solution B362. The first surface of the micro-nano device has a different surface energy from other surfaces. The surface energy of the first surface allows it to be wetted with solution A361 but not with solution B362, and the surface energy of other surfaces allows it to be wetted with solution B362 but not with solution A361.
[0065] In some embodiments, the shape of the assembly substrate 2 can be any shape such as a plane or a curved surface, and the material can be a hard material such as metal, silicon dioxide, or a soft material such as polydimethylsiloxane. The assembly position on the surface of the assembly substrate 2 can be a patterned protrusion / patterned groove / plane structure. The surface of the assembly substrate 2 is pattern-specifically modified so that different positions on the surface have different surface energies. The size and shape of the assembly position are consistent with the size and shape of the first surface of the micro-nano device. The surface energy of the assembly position on the assembly substrate 2 allows it to be wetted with solution A361 but not with solution B362, and the surface energy of the non-assembly position on the assembly substrate 2 allows it to be wetted with solution B362 but not with solution A361.
[0066] S2. In the first assembly container 31, the modified micro-nano device and the assembly substrate 2 are dropped into the solution B362 through the solution A361. Under external disturbance, the assembly surface of the micro-nano device and the droplets composed of the solution A361 attached to the assembly position of the assembly substrate 2 contact and fuse with each other to form a liquid bridge, completing an alignment and forming a primary assembly of the micro-nano device and the assembly substrate 2. The fluid disturbance method can be a plunger pump, a circulation pump, a peristaltic pump, a brush, a shaker, an oscillation, a centrifuge, and other methods.
[0067] Furthermore, in the above step S2, the upper layer of the first assembly container 31 is solution A361, the lower layer is solution B362, and the bottom of the first assembly container 31 is equipped with a conveying mechanism leading to the second assembly container 32, and the first assembly container 31 is equipped with a spoiler component for disturbing the solution B362; the modified micro-nano device and the assembly substrate 2 are sent to the solution B362 through the solution A361, and in this process, the assembly position on the surface of the assembly substrate 2 and the first surface of the micro-nano device are both attached with droplets composed of solution A361; the assembly substrate 2 is fixed on the conveying mechanism at the bottom of the first assembly container 31, and the patterned specific modified surface is in contact with the solution. Under the action of the spoiler component, the micro-nano device moves irregularly in the solution B362. In this process, the droplets at the assembly position on the surface of the assembly substrate 2 collide and merge with the droplets on the first surface of the micro-nano device to form a liquid bridge. Based on the interfacial tension, the micro-nano device is assembled at the assembly position of the assembly substrate 2, completing an alignment. The assembly status of the assembly substrate 2 and the micro-nano device is monitored in real time by an image monitoring device. After all assembly positions of the assembly substrate 2 are assembled with micro-nano devices, the disturbance of solution B362 is stopped to form a primary assembly of the assembly substrate 2 and the micro-nano device.
[0068] S3. The primary assembly is transferred to the second assembly container 32, and the liquid bridge composed of solution A361 between the micro-nano device and the assembly substrate 2 in the primary assembly is controllably dissolved or volatilized into the fluid C363 to complete the secondary alignment and form the final assembly. In step S3, after the primary assembly is completed, the primary assembly is transferred to the second assembly container 32 via the automatic conveying mechanism; the primary assembly enters the second assembly container 32, and the liquid bridge composed of solution A361 between the first surface of the micro-nano device and the assembly position of the assembly substrate 2 slowly dissolves or evaporates into the fluid C363. In the process of the liquid bridge gradually becoming smaller, the relative position between the assembly position of the micro-nano device and the assembly substrate 2 is finely adjusted due to the change in interfacial tension, completing the secondary alignment and forming the final assembly.
[0069] S4. The final assembly is taken out from the second assembly container 32, and the final assembly consisting of the micro-nano device and the assembly substrate 2 is post-processed to form a stable bond between the two, to achieve the conduction of various physical and chemical properties, and to complete the packaging process. In step S4, the final assembly is taken out from the second assembly container 32, and the micro-nano device and the assembly substrate 2 are bonded by welding or other connection methods to achieve electrical and thermal conductivity. The welded assembly continues to complete the subsequent packaging process.
[0070] In some other embodiments, step S2 is replaced by the following steps. It should be understood that the other steps are the same as those in the above embodiment:
[0071] S201. The modified micro-nano device is uniformly dispersed at the interface of solution A361 and solution B362, and the assembly substrate 2 is slowly inserted into the solution at any angle of 30-90°. The micro-nano device is assembled to the assembly position of the assembly substrate 2 based on the interface interaction, and the alignment is completed once, and the primary assembly of the micro-nano device and the assembly substrate 2 is formed.
[0072] In step S201, the upper layer of the first assembly container 31 is solution A361, and the lower layer is solution B362, and an automatic conveying mechanism leading to the second assembly container 32 is installed at the bottom of the first assembly container 31; due to the combined effect of density and surface energy, the modified micro-nano device is uniformly dispersed at the interface between solution A361 and solution B362 in a state where the first surface contacts solution A361; the patterned modified assembly substrate 2 faces the solution on one side and faces the side wall of the first assembly container 31 on the other side, and is slowly inserted into the solution at any angle of 30-90°. During the insertion process, due to the difference in surface energy, the assembly position of the assembly substrate 2 is at the interface between solution A361 and solution B362, causing interface deformation, so that the first surface of the micro-nano device is assembled with the assembly position of the assembly substrate 2, completing one alignment, and forming a primary assembly consisting of the assembly substrate 2 and multiple micro-nano devices. After the assembly substrate 2 with the micro-nano device assembled thereon is completely immersed in the solution B362, the angle of the assembly substrate 2 is adjusted and fixed on the automatic conveying mechanism at the bottom of the first assembly container 31, so that the patterned specific modified surface contacts with the solution.
[0073] Specifically, solution A361 and solution B362 are mutually immiscible, and solution A361 and fluid C363 are slightly soluble. Solution A361 is a low-viscosity aqueous solution such as deionized water, saline solution, alkaline solution, etc.; solution B362 is a low-viscosity organic solvent such as toluene, n-hexane, cyclohexane or xylene that is insoluble in water; fluid C363 can be a low-viscosity organic solvent such as ethyl acetate, chloroform or ether that is slightly soluble in water, or can be a gas such as nitrogen and air.
[0074] For ease of understanding, the implementation process of the method provided by the present invention is briefly described below using several specific embodiments as examples.
[0075] In Example 1, the fluid self-assembly process of the Micro-LED chip includes the following steps:
[0076] S110: Preparation of chip 1. The structure of Micro-LED chip 1 is as follows Figure 2 and Figure 3As shown. First, a multilayer gallium nitride structure is prepared on the surface of the growing wafer, and then an etching method is used to prepare a light-emitting micro-LED chip 1, which can be a circular, quadrilateral, hexagonal and other shapes. Here, the preparation process is described by taking a circular chip 1 as an example. Electrodes are prepared on the surface of the prepared chip 1 using magnetron metal sputtering coating technology, silver paste coating, screen printing technology, chemical deposition and other technologies to construct a complete circuit structure. The two electrodes are concentric structures and can be rotationally symmetrical shapes such as circular, quadrilateral, hexagonal, etc. The electrode material is composed of materials such as gold, silver, and aluminum. An insulating layer 14 is prepared between the prepared first electrode 12 and the second electrode 13. The insulating layer 14 is composed of insulators such as silicon dioxide, resin, and polymer. The electrodes and the insulating layer 14 are modified to have high surface energy by surface modification methods such as plasma bombardment, dip coating, reactive ion beam etching, and femtosecond laser, showing hydrophilicity, and the other parts of the light-emitting device still maintain hydrophobicity.
[0077] S120: Design of assembly substrate 2. The structure of assembly substrate 2 is as follows: Figure 4 and Figure 5 As shown. First, the surface of the assembly substrate 2 is modified as a whole by using a surface modification method such as dip coating, vapor deposition, spraying, and femtosecond laser, so that the assembly substrate 2 is a hydrophobic structure as a whole. Electrodes are also prepared on the surface of the assembly substrate 2 by using magnetron metal sputtering coating technology, silver paste coating, screen printing technology, chemical deposition and other technologies to construct a complete circuit structure. They are the third electrode 22 and the fourth electrode 23, respectively, and their shapes are consistent with the electrode shape in the micro-LED chip 1. The electrode material is composed of materials such as gold, silver, and aluminum. An insulating layer 14 is prepared between the prepared first electrode 12 and the second electrode 13. The insulating layer 14 is composed of insulators such as silicon dioxide, resin, and polymer. Then, a metal high-precision template is combined with a vapor deposition process, chemical etching, femtosecond laser, two-photon lithography and other surface modification methods to modify the electrode and the insulating layer 14 to have high surface energy and show hydrophilicity. The assembly substrate 2 is hydrophobic as a whole, and the electrode and the insulating layer 14 are partially hydrophilic.
[0078] S130: Fluid self-assembly process. Fluid self-assembly process Figure 6As shown, the entire container is divided into two grooves on the left and right. The upper layer in the left groove is solution A361, and the lower layer is solution B362. During the process of immersing the assembled substrate 2 and the micro-LED chip 1 into the solution B362 through the solution A361 layer, the metal electrodes with high surface energy and the surface of the insulating layer 14 are attached with liquid A361 to form droplets. By disturbing the fluid, the micro-LED chip 1 moves randomly in the liquid B362. In incompatible liquids, different liquids are attached to different surfaces of the micro-LED chip 1 and different areas of the surface of the assembled substrate 2. During fluid disturbance, since the electrodes of the micro-LED chip 1 and the electrodes of the assembled substrate 2 are attached with the same liquid A361, self-assembly occurs, and preliminary alignment is achieved due to the principle of minimizing interfacial energy, forming the following. Figure 7 The primary assembly shown in (a). Since there is more solution A361 between the electrode surface of the micro-LED chip 1 and the electrode position of the assembly substrate 2 at this time, the alignment accuracy is insufficient. Here, solution A361 is various low-viscosity aqueous solutions such as pure water, salt solution, alkaline solution, etc., and liquid B361 is a low-viscosity organic solvent incompatible with solution A361, such as toluene, n-hexane, cyclohexane, xylene, etc. The perturbing fluid mode includes a plunger pump, a brush drive, a circulating pump, a vertical oscillation, a centrifuge, and other methods.
[0079] During the self-assembly process of the Micro-LED chip 1 in the liquid B, the image monitoring system 37 above also monitors the assembly process in real time. After the image monitoring system 37 recognizes that a micro-LED chip 1 is assembled at each electrode position on the assembly substrate 2, the disturbance stops. When the solution B362 in the first assembly container 31 stops moving, the isolation plate A33 opens, and the bottom conveying mechanism transports the primary assembly consisting of the micro-LED chip 1 and the assembly substrate 2 to the right groove, and then the isolation plate A33 is closed. The second assembly container 32 contains fluid C363, and the solution A361 between the electrode surface of the micro-LED chip 1 and the electrode position of the assembly substrate 2 gradually diffuses and dissolves into the fluid C362. The solution A361 between the two gradually decreases, and the liquid bridge gradually becomes smaller. Because the surface energy of the electrode surface of the micro-LED chip 1 and the electrode surface of the assembly substrate 2 are similar, in the process of the liquid bridge gradually becoming smaller, due to the change in interfacial tension, the relative position between the electrode surface of the micro-LD chip 1 and the electrode position of the assembly substrate 2 is finely adjusted to complete the secondary alignment, forming the following. Figure 7The final assembly shown in (b). Compared with the existing fluid self-assembly based on the principle of minimizing interfacial free energy, this two-step alignment strategy significantly improves the assembly accuracy and can reduce the assembly error to one tenth of the original. After the final assembly is completed, open the rightmost isolation plate B34 to take out the final assembly consisting of the micro-LED chip 1 and the assembly substrate 2, and proceed to the next step. Here, the fluid C363 is a low-viscosity organic solvent that is slightly soluble in the solution A361, such as ethyl acetate, chloroform, ether, etc. Figure 8 This is an incorrect contact mode between the micro-LED chip 1 and the assembly substrate 2. In fluid disturbance, the assembly interface interaction force of the incorrect structure is weak and easy to remove, and then through multiple trials and errors, it is adjusted to the correct assembly structure and stabilized by strong interface force.
[0080] S140: bonding process and packaging of micro-LED chip 1 and assembly substrate 2. After the micro-LED chip 1 and assembly substrate 2 are properly assembled in the fluid (the structure after bonding is as shown in FIG. Fig. 9 As shown), the whole is taken out from the solution C363. The micro-LED chip 1 and the assembly substrate 2 are bonded by various methods such as hot pressing welding, eutectic welding or soldering to achieve electrical and thermal conductivity. The bonded assembly continues to complete the subsequent packaging process.
[0081] In Example 2, the fluid self-assembly process of the micro-LED chip 1 includes the following steps.
[0082] S210: The design and preparation process of the micro-LED chip 1 are consistent with those of Example 1.
[0083] S220: The design and preparation process of the assembly substrate 2 is consistent with that of Example 1.
[0084] S230: Fluid self-assembly process. Fluid self-assembly process is as follows Fig.10As shown, the entire container is divided into two grooves on the left and right. The upper layer in the left groove is solution A361, and the lower layer is solution B362. The overall density of the prepared micro-LED chip 1 is slightly greater than that of solution B362. Due to the combined effect of density and interfacial tension, all micro-LED chips 1 are dispersed at the interface between solution A361 and solution B362 in the state where the electrodes contact solution A361 and the light-emitting devices contact solution B362. The assembly substrate 2 is modified with an electrode position facing the solution on one side and facing the side wall of the left groove on the other side, and is slowly inserted into the solution at a certain angle. The angle between the assembly substrate 2 and the liquid surface is 30° to 90°, and the speed is 0.1-10cm / s. Since the electrode position on the surface of the assembly substrate 2 is hydrophilic, when the assembly substrate 2 passes through the liquid-liquid interface of solution A361 and solution B362, the liquid surface is pulled to deform, so that the electrode of the micro-LED chip 1, which is also hydrophilic, is assembled with the electrode position of the assembly substrate 2. The two realize the first step of alignment based on the principle of minimizing the interface free energy, and the electrode surface of the micro-LED chip 1 is assembled to the electrode position of the assembly substrate 2. The assembly substrate 2 continues to descend until the entire assembly substrate 2 is completely immersed in the solution B362. At this time, all the electrode positions on the assembly substrate 2 are assembled with micro-LED chips 1, forming a primary assembly. The assembly substrate 2 falls on the conveyor belt 35, and the assembly shape is similar to Figure 7 The shape presented in (a). Since there is more solution A361 between the micro-LED chip 1 and the assembly substrate 2 at this time, the droplets are larger, resulting in insufficient alignment accuracy. The isolation plate A33 is opened, and the bottom conveyor belt 35 moves to the right to transport the assembly substrate 2 assembled with the micro-LED chip 1 to the right groove, and then the isolation plate A33 is closed. The right groove contains fluid C363, and the solution A361 between the electrode surface of the micro-LED chip 1 and the electrode position of the assembly substrate 2 gradually diffuses and dissolves into the fluid C363. The solution A361 between the two gradually decreases, and the liquid bridge gradually becomes smaller. Because the surface energy of the electrode surface of the micro-LED chip 1 and the electrode position of the assembly substrate 2 are similar, in the process of the liquid bridge gradually becoming smaller, due to the change in interfacial tension, the relative position between the electrode surface of the micro-LED chip 1 and the electrode position of the assembly substrate 2 is finely adjusted to complete the secondary alignment, forming the following Figure 7The final assembly is shown in (b). Compared with the existing fluid self-assembly based on the principle of minimizing interfacial free energy, this two-step alignment strategy significantly improves the assembly accuracy and can reduce the assembly error to one tenth of the original. After the assembly is completed, open the rightmost isolation plate B34 to take out the final assembly and proceed to the next step. Here, solution A361 is various low-viscosity aqueous solutions such as pure water, salt solution, alkaline solution, etc., and liquid B362 is a low-viscosity organic solvent incompatible with solution A361, such as toluene, n-hexane, cyclohexane, xylene, etc. Fluid C363 is a low-viscosity organic solvent that is slightly soluble in solution A361, such as ethyl acetate, chloroform, ether, etc.
[0085] S240: The bonding process of the micro-LED chip 1 and the assembly substrate 2 is consistent with that in Example 1.
[0086] In Example 3, the fluid self-assembly process of the micro-LED chip 1 includes the following steps:
[0087] S310: The design and preparation process of the micro-LED chip 1 are consistent with those of Example 1.
[0088] S320: The design and preparation process of the assembly substrate 2 is consistent with that of Example 1.
[0089] S330: Fluid self-assembly process. The assembly process of the primary assembly is consistent with that of Example 1. Fig.11As shown, after the primary assembly is formed, the primary assembly consisting of the micro-LED chip 1 and the assembly substrate 2 is transported by the conveying mechanism to the second assembly container 32 containing the fluid C363. The bottom drain valve 391 is opened to discharge the excess liquid in the second assembly container 32. Due to the influence of surface tension, there is still a liquid bridge composed of solution A361 between the electrode of the micro-LED chip 1 and the electrode position of the assembly substrate 2. The temperature and pressure of the fluid C363 in the second assembly container 32 are adjusted by the temperature and pressure regulating device 392, so that the saturated vapor pressure of the solution A362 in the right groove is in a suitable state, so as to facilitate the solution A361 between the electrode surface of the micro-LED chip 1 and the electrode position of the assembly substrate 2 to gradually evaporate into the fluid C363. The solution A361 between the two gradually decreases, and the liquid bridge gradually becomes smaller. Because the surface energy of the electrode surface of the micro-LED chip 1 is similar to that of the electrode position of the assembly substrate 2, in the process of the liquid bridge gradually becoming smaller, the relative position between the electrode surface of the micro-LD chip 1 and the electrode position of the assembly substrate 2 is finely adjusted due to the change in interfacial tension, completing the secondary alignment and forming the final assembly. Compared with the existing fluid self-assembly based on the principle of minimizing interfacial free energy, this two-step alignment strategy significantly improves the assembly accuracy and can reduce the assembly error to one tenth of the original. After the assembly is completed, open the rightmost isolation plate B34 to remove the assembled assembly substrate 2 and proceed to the next step. Here, solution A361 is various low-viscosity aqueous solutions such as pure water, salt solution, alkaline solution, etc., and liquid B362 is a low-viscosity organic solvent incompatible with solution A, such as toluene, n-hexane, cyclohexane, xylene, etc. Fluid C363 is air, nitrogen and other gases.
[0090] S340: The bonding process between the chip and the assembly substrate is consistent with that in Example 1.
[0091] Compared with the existing fluid self-assembly technology, the fluid self-assembly method for micro-nano devices provided by the present invention has the following technical advantages:
[0092] 1) Improved fluid self-assembly accuracy. Through the two-step alignment assembly process, the dissolution or volatilization rate of the liquid bridge between the micro-nano device and the assembly substrate is regulated, effectively solving the problem of poor assembly accuracy caused by the relative displacement of the micro-nano chip and the assembly substrate during the rapid removal of the liquid bridge and the difficulty of fine adjustment due to rapid fixation.
[0093] 2) Simplified the preparation process of the assembly substrate. The assembly position of the assembly substrate uses similar surface energy on the plane structure to capture the micro-nano devices, avoiding the preparation of the complex three-dimensional structure of the assembly substrate and simplifying the preparation process. It also fundamentally solves the contradiction between assembly accuracy and assembly efficiency in shape matching fluid self-assembly.
[0094] 3) Simplified the preparation process of micro-nano devices. The surface energies of different surfaces of micro-nano devices are significantly different, and surface selectivity can be achieved during the assembly process without the need for additional structures or preparation processes. This simplifies the preparation process of micro-nano devices.
[0095] The above specific implementation methods further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific implementation methods of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made on the basis of the technical solutions of the present invention should be included in the scope of protection of the present invention.
Claims
1. A fluid self-assembly method for micro-nano devices, It is characterized in that The following steps are involved: S1. The micro-nano device and the assembly substrate are subjected to surface treatment respectively, different surfaces of the micro-nano device have different surface energies, the assembly position and the non-assembly position of the assembly substrate also have different surface energies, and the surface of the micro-nano device to be assembled and the preset assembly position of the assembly substrate have similar surface energies; S2. In the first assembly container, the modified micro-nano device and the assembly substrate are dropped into solution B through solution A. Under external disturbance, the assembly surface of the micro-nano device and the droplets composed of solution A attached to the assembly position of the assembly substrate contact and fuse with each other to form a liquid bridge, completing one alignment and forming a primary assembly of the micro-nano device and the assembly substrate; S3. The primary assembly is transferred to a second assembly container, and the liquid bridge composed of solution A between the micro-nano device in the primary assembly and the assembly substrate is controllably dissolved or volatilized into fluid C to complete the secondary alignment and form a final assembly; S4. The final assembly is taken out from the second assembly container, and the final assembly consisting of the micro-nano device and the assembly substrate is post-processed to form a stable bond between the two, achieve the conduction of various physical and chemical properties, and complete the packaging process.
2. The fluid self-assembly method for micro-nano devices according to claim 1, It is characterized in that The micro-nano device has a size of nanometer to centimeter level, has a columnar structure, and has a bottom surface of the columnar structure as a first surface. The material of the micro-nano device is at least one of gallium nitride, silicon dioxide, metal or polymer, and the density of the micro-nano device is greater than the density of solution B.
3. The fluid self-assembly method for micro-nano devices according to claim 1, It is characterized in that The first surface of the micro-nano device has a different surface energy from other surfaces. The surface energy of the first surface enables it to be wetted by solution A but not by solution B, and the surface energy of other surfaces enables it to be wetted by solution B but not by solution A.
4. The fluid self-assembly method for micro-nano devices according to claim 1, It is characterized in that The shape of the assembly substrate is a plane or a curved surface, the material of the assembly substrate is metal, silicon dioxide or polydimethylsiloxane, and the assembly position on the surface of the assembly substrate is a patterned protrusion, a patterned groove or a plane structure.
5. The fluid self-assembly method for micro-nano devices according to claim 1, It is characterized in that The surface of the assembly substrate is patterned and specifically modified so that different positions on the surface have different surface energies. The size and shape of the assembly position are consistent with the size and shape of the first surface of the micro-nano device. The surface energy of the assembly position on the assembly substrate allows it to be wetted with solution A but not with solution B. The surface energy of the non-assembly position on the assembly substrate allows it to be wetted with solution B but not with solution A.
6. The fluid self-assembly method for micro-nano devices according to claim 1, It is characterized in that The fluid disturbance method is a plunger pump, a circulation pump, a peristaltic pump, a brush, a shaker, an oscillation or a centrifugal method.
7. The fluid self-assembly method for micro-nano devices according to any one of claims 1 to 6, It is characterized in that Step S2 is replaced by the following steps: S201. The modified micro-nano devices are uniformly dispersed at the interface between solution A and solution B, and the assembly substrate is slowly inserted into the solution at any angle of 30-90°. The micro-nano devices are assembled to the assembly positions on the assembly substrate based on the interface interaction, completing one alignment and forming a primary assembly of the micro-nano devices and the assembly substrate.
8. The fluid self-assembly method for micro-nano devices according to claim 7, It is characterized in that In step S2, the upper layer of the first assembly container is solution A, the lower layer is solution B, and a conveying mechanism leading to the second assembly container is installed at the bottom of the first assembly container, and a flow disturbance component is installed in the first assembly container for disturbing the solution B; The modified micro-nano device and the assembly substrate are sent to solution B through solution A. During this process, droplets composed of solution A are attached to the assembly position on the surface of the assembly substrate and the first surface of the micro-nano device; The assembly substrate is fixed on the conveying mechanism at the bottom of the first assembly container, and the patterned specific modified surface is in contact with the solution. Under the action of the spoiler, the micro-nano device moves irregularly in the solution B. In this process, the droplets at the assembly position on the surface of the assembly substrate collide and merge with the droplets on the first surface of the micro-nano device to form a liquid bridge. Based on the interfacial tension, the micro-nano device is assembled at the assembly position of the assembly substrate, completing an alignment. The assembly status of the assembly substrate and the micro-nano device is monitored in real time by an image monitoring device. After all assembly positions of the assembly substrate are assembled with the micro-nano device, the disturbance of solution B is stopped to form a primary assembly of the assembly substrate and the micro-nano device.
9. The fluid self-assembly method for micro-nano devices according to any one of claims 1 to 6, It is characterized in that In step S3, after the primary assembly is completed, the primary assembly is transferred to the second assembly container via the automatic conveying mechanism; The primary assembly enters the second assembly container, and the liquid bridge formed by solution A between the first surface of the micro-nano device and the assembly position of the assembly substrate slowly dissolves or evaporates into fluid C. In the process of the liquid bridge gradually becoming smaller, the relative position between the assembly position of the micro-nano device and the assembly substrate is finely adjusted due to the action of interfacial tension, completing the secondary alignment and forming the final assembly.
10. The fluid self-assembly method for micro-nano devices according to any one of claims 1 to 6, It is characterized in that In step S4, the final assembly is taken out from the second assembly container, and the micro-nano device is bonded to the assembly substrate by welding. The welded assembly continues to complete the subsequent packaging process.
11. The fluid self-assembly method for micro-nano devices according to claim 7, It is characterized in that In step S201, the upper layer of the first assembly container is solution A, the lower layer is solution B, and an automatic conveying mechanism leading to the second assembly container is installed at the bottom of the first assembly container; Due to the combined effect of density and surface energy, the modified micro-nano device is evenly dispersed at the interface between solution A and solution B with the first surface facing solution A; The assembly substrate is patterned and modified with one side facing the solution and the other side facing the side wall of the first assembly container, and is slowly inserted into the solution at any angle of 30-90°. During the insertion process, due to the difference in surface energy, the assembly position of the assembly substrate is at the interface between solution A and solution B, causing interface deformation, so that the first surface of the micro-nano device is assembled with the assembly position of the assembly substrate, completing one alignment, and forming a primary assembly consisting of the assembly substrate and multiple micro-nano devices; After the assembly substrate with the micro-nano device assembled thereon is completely immersed in solution B, the angle of the assembly substrate is adjusted so that the side of the assembly substrate with the assembly position faces the solution and is fixed on the automatic conveying mechanism at the bottom of the first assembly container.
12. The fluid self-assembly method for micro-nano devices according to claim 7, It is characterized in that Solution A and solution B are immiscible with each other, solution A and fluid C are slightly soluble, solution A is deionized water, saline solution or alkaline solution; solution B is toluene, n-hexane, cyclohexane or xylene; fluid C is ethyl acetate, chloroform, ether or nitrogen.