Method for reducing silicon content in aluminum oxide product and aluminum oxide product
By adding lime milk to alumina production to produce hydrated calcium carbonate and aluminate, combined with crude sodium aluminate solution for desilica reaction, the problem of excessive silicon content of alumina products in low silicon bauxite is solved, and the silicon quantity index is achieved. Improvement and reduction of silicon content, suitable for industrial applications.
Patent Information
- Application Number
- CN202411101533.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
AI Technical Summary
The existing desiliconization technology is not suitable for low-silicon bauxite, which leads to excessive silicon content in alumina products. The existing methods are prone to alumina losses when increasing the silicon quantity index.
By adding lime milk to sodium aluminate semen, hydrated calcium carboaluminate is generated, and it reacts with silicon impurities, combined with a large amount of crude sodium aluminate solution for desilication reaction, forming a filter aid to enhance the desiliconization effect and increase the amount of silicon Index and reduce the silicon content in alumina products.
The silicon quantity index of sodium aluminate refined liquid is effectively improved, and the silica content in alumina products is reduced to less than 0.015%. This method has little change to the existing process, has little investment, and is easy to use in industrial applications.
Smart Images

Figure CN119018920A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of alumina production, and in particular to a method for reducing the silicon content in an alumina product and an alumina product. Background Art
[0002] Alumina is the raw material for electrolytic aluminum production, and its product quality seriously affects the current efficiency of the electrolytic cell and the purity of the original aluminum. The SiO2 in alumina will precipitate at the cathode during the electrolysis process and enter the aluminum, reducing the grade of aluminum. Therefore, the national standard for alumina (GB / T-24487-2022) stipulates that the SiO2 content in first-grade alumina should not exceed 0.02%. The SiO2 content in alumina products is closely related to the SiO2 content in semen. Therefore, the Bayer process alumina production process requires the silicon content index of semen to be greater than 200 as much as possible.
[0003] In recent years, the import volume of Guinea ore has increased year by year, and more and more alumina plants use Guinea ore for alumina production. Guinea ore has the characteristics of high iron and low silicon, with SiO2 content less than 3% and kaolinite content less than 3%. Only through the traditional pre-desiliconization and dilution desiliconization process, the silicon content index of the semen is generally low. An alumina plant uses Guinea ore as raw material. After pre-desiliconization, low-temperature dissolution and dilution desiliconization, the silicon content index of the semen is only about 160, causing the silicon content in the alumina product to reach more than 0.035%, which is seriously exceeded. Therefore, it is necessary to find a method to effectively increase the silicon content index of the semen and reduce the silicon content in the alumina product. Summary of the invention
[0004] The present application provides a method for reducing the silicon content in an alumina product and an alumina product to solve the following technical problem: how to reduce the silicon content in an alumina product.
[0005] In a first aspect, the present application provides a method for reducing the silicon content in an alumina product, the method comprising:
[0006] Get the Na2O C Sodium aluminate semen of concentration and set temperature;
[0007] Adding lime milk to the sodium aluminate semen to react at the set temperature and set time to obtain a first mixture;
[0008] adding the first mixture to a crude sodium aluminate solution to perform a desiliconization reaction to obtain a second mixture;
[0009] filtering the second mixture to obtain a refined sodium aluminate liquid;
[0010] Decomposing the sodium aluminate refined liquid by seed crystal decomposition to obtain aluminum hydroxide; and
[0011] The aluminum hydroxide is calcined to obtain an aluminum oxide product.
[0012] Optionally, the setting of Na2O C Concentration ≥10g / L.
[0013] Optionally, the set temperature is 60°C to 80°C.
[0014] Optionally, the set time is 30 minutes to 60 minutes.
[0015] Optionally, the lime milk is prepared using red mud washing water or aluminum hydroxide washing water, and the solid content of the lime milk is 250 g / L to 300 g / L.
[0016] Optionally, the volume ratio of the lime milk to the sodium aluminate semen is 1:(1-4).
[0017] Optionally, the temperature of the desiliconization reaction is 80° C. to 95° C., and the time of the desiliconization reaction is 60 min to 120 min.
[0018] Optionally, the solid content of the filter aid in the second mixture is 5 g / L to 20 g / L.
[0019] Optionally, the silicon content index of the refined sodium aluminate solution is ≥250.
[0020] In a second aspect, the present application provides an alumina product prepared by the method described in any one of the embodiments of the first aspect, wherein the SiO2 content in the alumina product is ≤0.015% by mass.
[0021] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0022] The present application provides a method for reducing the silicon content in an alumina product, comprising: obtaining a product having a set Na2O C concentration and a set temperature of sodium aluminate concentrate; adding lime milk to the sodium aluminate concentrate to react at the set temperature and set time to obtain a first mixture; adding the first mixture to the sodium aluminate crude liquid to perform a desiliconization reaction to obtain a second mixture; filtering the second mixture to obtain a sodium aluminate refined liquid; performing seed crystal decomposition on the sodium aluminate refined liquid to obtain aluminum hydroxide; and roasting the aluminum hydroxide to obtain an alumina product. C Lime milk is added to the concentrated sodium aluminate solution, which reacts at a set temperature to produce hydrated calcium aluminate. At the same time, hydrated calcium aluminate reacts with sufficient Na2O CThe reaction continues to occur, and unstable hydrated calcium aluminate is generated. The hydrated calcium aluminate is not easily converted into hydrated calcium aluminate at a set temperature, thereby obtaining hydrated calcium aluminate that can react with silicon impurities. Subsequently, the mixture of lime milk and sodium aluminate semen is mixed with a large amount of sodium aluminate crude liquid to carry out a removal reaction of silicon impurities in the sodium aluminate crude liquid. The solid calcium formed in the above process can all be used as a filter aid. Therefore, the present application adjusts the preparation conditions of the filter aid, strengthens the desiliconization effect of the crude liquid, effectively improves the silicon content index of the semen, and reduces the silicon dioxide content in the alumina product. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0025] Figure 1 A schematic flow chart of a method for reducing silicon content in an alumina product provided in an embodiment of the present application. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0027] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0028] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0029] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0030] The creative ideas of this application are:
[0031] Existing desiliconization technology is not suitable for low-silicon bauxite such as Guinea ore, resulting in low silicon content index of the semen and excessive silicon content in the alumina product. At the same time, although the existing method can increase the silicon content index of the sodium aluminate solution, the calcium-containing compounds will react with the sodium aluminate solution to cause alumina loss. At present, there is no economical and efficient method to increase the silicon content index of the semen in the process of producing alumina from Guinea ore.
[0032] In order to solve the above technical problems, the present application provides a method for increasing the silicon content index in semen and reducing the silicon content in alumina products. The present application cools the sodium aluminate semen from the alumina production site to 60°C to 80°C, then adds lime milk, and reacts at a temperature of 60°C to 80°C. The reaction equation is as follows: 3CaO+2NaAl(OH)4+3H2O→3CaO·Al2O3·6H2O+2NaOH. Since the present application controls the Na2O in the sodium aluminate semen, the sodium aluminate semen is reduced to 100% by weight. C When the concentration is not less than 10g / L, hydrated calcium aluminate (CaO·Al2O3·6H2O) will continue to react, and the reaction equation is as follows: 3CaO·Al2O3·6H2O+mCO3 2- +CaO(OH)2 2-→4CaO·Al2O3·mCO2·nH2O+(2+2m)OH - At the same time, at a temperature of 60°C to 80°C, the unstable hydrated calcium aluminate (CaO·Al2O3·mCO2·nH2O) generated is not easily converted into hydrated calcium aluminate, thereby obtaining hydrated calcium aluminate that can react with silicon impurities. Subsequently, the mixture of lime milk and sodium aluminate concentrate is mixed with a large amount of sodium aluminate crude liquid to remove silicon impurities from the sodium aluminate crude liquid. The specific reaction equation is as follows: 4CaO·Al2O3·mCO2·nH2O+x[SiO4] 4- →3CaO·Al2O3·xSiO2·(6-2x)H2O+CaCO3+4xOH - The solid calcium formed in the above process can be used as a filter aid. The preparation conditions of the filter aid are adjusted, and then a sodium aluminate refined liquid with a silicon content index of more than 250 is obtained by filtration, thereby efficiently removing silicon impurities in the sodium aluminate crude liquid.
[0033] The method of the present application can effectively increase the silicon content index of the sodium aluminate refined liquid to above 250, meet the requirements of seed decomposition, and reduce the silicon dioxide content in the alumina product; at the same time, the method does not cause much change to the existing process, requires little investment, and is easy to apply industrially.
[0034] Figure 1 A schematic flow chart of a method for reducing silicon content in an alumina product provided in an embodiment of the present application.
[0035] See also Figure 1 The present application provides a method for reducing the silicon content in an alumina product, the method comprising:
[0036] S1, get the set Na2O C Sodium aluminate semen of concentration and set temperature;
[0037] In some embodiments, the setting of Na2O C Concentration ≥10g / L.
[0038] In the above embodiment, the Na2O in the sodium aluminate semen is controlled C concentration, thereby facilitating the formation of hydrated calcium aluminate. For example, Na2O in sodium aluminate semen C The concentration can be 10g / L, 12g / L, 15g / L, 18g / L, 20g / L, 23g / L, 25g / L, 30g / L, etc.
[0039] S2, adding lime milk to the sodium aluminate semen to react at the set temperature and set time to obtain a first mixture;
[0040] In some embodiments, the set temperature is 60°C to 80°C.
[0041] In the above embodiment, controlling the temperature of the reaction between sodium aluminate semen and lime milk can, on the one hand, avoid the precipitation of aluminum hydroxide at low temperatures, and on the other hand, facilitate the formation of hydrated calcium aluminate. Exemplarily, the temperature of the reaction between sodium aluminate semen and lime milk can be 60°C, 65°C, 70°C, 75°C, 80°C, etc.
[0042] In some embodiments, the set time is 30 min to 60 min.
[0043] In the above embodiment, controlling the reaction time of sodium aluminate semen and lime milk can increase the amount of hydrated calcium aluminate on the one hand, and avoid the conversion of synthesized hydrated calcium aluminate into hydrated calcium aluminate on the other hand. Exemplarily, the reaction time of sodium aluminate semen and lime milk can be 30min, 35min, 40min, 45min, 50min, 55min, 60min, etc.
[0044] In some embodiments, the lime milk is prepared using red mud wash water or aluminum hydroxide wash water, and the solid content of the lime milk is 250 g / L to 300 g / L.
[0045] In some embodiments, the volume ratio of the lime milk to the sodium aluminate semen is 1:(1-4).
[0046] In the above embodiment, when the volume ratio of lime milk to semen is greater than 1:1, it is difficult to convert all the lime into hydrated calcium aluminate; when the volume ratio of lime milk to semen is less than 1:4, the amount of hydrated calcium aluminate prepared is small or more semen is required. Exemplarily, the volume ratio of lime milk to the sodium aluminate semen can be 1:1, 1:1.5, 1:2, 1:3, 1:4, etc.
[0047] S3, adding the first mixture to the crude sodium aluminate solution to perform a desiliconization reaction to obtain a second mixture;
[0048] It should be noted that step S3 may specifically be: sending the first mixture to a crude liquid tank with a temperature of 80-95° C., mixing it evenly with the sodium aluminate crude liquid, and staying in the crude liquid tank for 60 min to 120 min to perform a desiliconization reaction.
[0049] In some embodiments, the temperature of the desiliconization reaction is 80° C. to 95° C., and the time of the desiliconization reaction is 60 min to 120 min.
[0050] In the above embodiment, if the temperature of the desiliconization reaction is lower than 80°C, the desiliconization reaction rate of hydrated calcium aluminate is slow; if the temperature of the desiliconization reaction is higher than 95°C, hydrated calcium aluminate is easily decomposed, which is not conducive to desiliconization. If the desiliconization reaction time is less than 60 minutes, the desiliconization reaction is not fully reacted; if the desiliconization reaction time is more than 120 minutes, the desiliconization reaction is fully reacted, and the silicon content index of semen does not change much by extending the reaction time. Exemplarily, the temperature of the desiliconization reaction can be 80°C, 82°C, 85°C, 90°C, 92°C, 95°C, etc., and the time of the desiliconization reaction can be 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes, 120 minutes, etc.
[0051] In some embodiments, the solid content of the filter aid in the second mixture is 5 g / L to 20 g / L.
[0052] It should be noted that in actual production, the volume ratio of the first mixture to the crude sodium aluminate solution is difficult to determine, but most of the solids in the second mixture come from the first mixture. Therefore, by determining the solid content of the filter aid in the second mixture, the volume ratio of the first mixture to the crude sodium aluminate solution can be indicated to a certain extent.
[0053] In the above embodiment, the filter aid is solid calcium (calcium carbonate, hydrated garnet, hydrated calcium aluminate, hydrated calcium carbon aluminate, etc.). If the solid content of the filter aid is lower than 5 g / L, the desiliconization range is small. If the solid content of the filter aid is higher than 20 g / L, the amount of slag is too large and the loss of alumina increases. Exemplarily, the solid content of the filter aid can be 5 g / L, 8 g / L, 10 g / L, 12 g / L, 15 g / L, 18 g / L, 20 g / L, etc.
[0054] S4, filtering the second mixture to obtain a refined sodium aluminate solution;
[0055] In some embodiments, the silicon content index of the refined sodium aluminate solution is ≥250.
[0056] The present application strengthens the desiliconization effect of the crude liquid by adjusting the preparation conditions of the filter aid, effectively increases the silicon content index of the refined liquid to above 250, and reduces the silicon dioxide content in the alumina product. For example, the silicon content index of the sodium aluminate refined liquid can be 250, 255, 260, 270, 280, 285, 290, etc.
[0057] S5, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0058] S6. calcining the aluminum hydroxide to obtain an aluminum oxide product.
[0059] Based on a general inventive concept, the present application provides an alumina product prepared by the method described in any one of the above embodiments, wherein the SiO2 content in the alumina product is ≤0.015% by mass.
[0060] The alumina product is realized based on the preparation method of the alumina product mentioned above. The specific steps of the preparation method of the alumina product can refer to the above embodiment. Since the alumina product adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.
[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0062] Example 1
[0063] This embodiment provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0064] S11, take the sodium aluminate semen from the alumina production site and cool it to 60℃. The concentration of sodium aluminate semen is Na2O T 162g / L, Na2O k 140g / L, Al2O3 155g / L, Na2O C 22g / L, SiO2 0.95g / L, a K 1.48, silicon content index 163;
[0065] S21, preparing lime milk with red mud washing water, the lime milk having a solid content of 250 g / L, and uniformly mixing the lime milk with sodium aluminate semen at a volume ratio of 1:1, and reacting at 60° C. for 60 min to obtain a first mixture;
[0066] S31, sending the first mixture to a crude liquid tank with a temperature of 90° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 90° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 10 g / L;
[0067] S41, filtering the second mixture by leaf filtration to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 255;
[0068] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0069] S61. calcining the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.012%.
[0070] Example 2
[0071] This embodiment provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0072] S11, take the sodium aluminate semen from the alumina production site and cool it to 70℃. The concentration of sodium aluminate semen is Na2O T 162g / L, Na2O k 140g / L, Al2O3 155g / L, Na2O C 22g / L, SiO2 0.95g / L, a K 1.48, silicon content index 163;
[0073] S21, preparing lime milk with red mud washing water, wherein the solid content of the lime milk is 250 g / L, and uniformly mixing the lime milk with sodium aluminate semen in a volume ratio of 1:2, and reacting at 70° C. for 60 min to obtain a first mixture;
[0074] S31, sending the first mixture to a crude liquid tank with a temperature of 90° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 90° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 10 g / L;
[0075] S41, leaf filtering the second mixture to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 270;
[0076] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0077] S61. The aluminum hydroxide is calcined to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.009%.
[0078] Example 3
[0079] This embodiment provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0080] S11, take the sodium aluminate semen from the alumina production site and cool it to 80℃. The concentration of sodium aluminate semen is Na2O T 162g / L, Na2O k 140g / L, Al2O3 155g / L, Na2O C 22g / L, SiO2 0.95g / L, aK 1.48, silicon content index 163;
[0081] S21, preparing lime milk with red mud washing water, wherein the solid content of the lime milk is 250 g / L, and uniformly mixing the lime milk with sodium aluminate semen in a volume ratio of 1:3, and reacting at 80° C. for 60 min to obtain a first mixture;
[0082] S31, sending the first mixture to a crude liquid tank with a temperature of 90° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 90° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 10 g / L;
[0083] S41, filtering the second mixture through leaf filters to obtain a refined sodium aluminate solution, wherein the silicon content index of the refined sodium aluminate solution is 250;
[0084] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0085] S61. Roasting the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.011%.
[0086] Example 4
[0087] This embodiment provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0088] S11, take the sodium aluminate semen from the alumina production site and cool it to 60℃. The concentration of sodium aluminate semen is Na2O T 160g / L, Na2O k 145g / L, Al2O3 159g / L, Na2O C 15g / L, SiO2 0.90g / L, a K 1.50, silicon content index 177;
[0089] S21, preparing lime milk with red mud washing water, the lime milk having a solid content of 300 g / L, and uniformly mixing the lime milk with sodium aluminate semen at a volume ratio of 1:2, and reacting at 60° C. for 40 min to obtain a first mixture;
[0090] S31, sending the first mixture to a crude liquid tank with a temperature of 90° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 90° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 15 g / L;
[0091] S41, leaf filtering the second mixture to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 260;
[0092] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0093] S61. calcining the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.010%.
[0094] Example 5
[0095] This embodiment provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0096] S11, take the sodium aluminate semen from the alumina production site and cool it to 70℃. The concentration of sodium aluminate semen is Na2O T 160g / L, Na2O k 145g / L, Al2O3 159g / L, Na2O C 15g / L, SiO2 0.90g / L, a K 1.50, silicon content index 177;
[0097] S21, preparing lime milk with red mud washing water, the lime milk having a solid content of 300 g / L, and uniformly mixing the lime milk with sodium aluminate semen in a volume ratio of 1:3, and reacting at 70° C. for 40 min to obtain a first mixture;
[0098] S31, sending the first mixture to a crude liquid tank with a temperature of 90° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 90° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 15 g / L;
[0099] S41, leaf filtering the second mixture to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 270;
[0100] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0101] S61. The aluminum hydroxide is calcined to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.009%.
[0102] Example 6
[0103] This embodiment provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0104] S11, take the sodium aluminate semen from the alumina production site and cool it to 70℃. The concentration of sodium aluminate semen is Na2O T 160g / L, Na2O k 145g / L, Al2O3 159g / L, Na2O C 15g / L, SiO2 0.90g / L, a K 1.50, silicon content index 177;
[0105] S21, preparing lime milk with red mud washing water, the lime milk having a solid content of 300 g / L, and uniformly mixing the lime milk with sodium aluminate semen in a volume ratio of 1:3, and reacting at 70° C. for 40 min to obtain a first mixture;
[0106] S31, sending the first mixture to a crude liquid tank with a temperature of 90° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 90° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 20 g / L;
[0107] S41, filtering the second mixture by leaf filtration to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 290;
[0108] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0109] S61. calcining the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.008%.
[0110] Comparative Example 1
[0111] This comparative example provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0112] S11, take the sodium aluminate semen from the alumina production site and cool it to 55℃. The concentration of sodium aluminate semen is Na2O T 162g / L, Na2O k 140g / L, Al2O3 155g / L, Na2O C 22g / L, SiO2 0.95g / L, a K 1.48, silicon content index 163;
[0113] S21, preparing lime milk with red mud washing water, wherein the solid content of the lime milk is 250 g / L, and uniformly mixing the lime milk with sodium aluminate semen at a volume ratio of 1:1, and reacting at 55° C. for 60 min to obtain a first mixture;
[0114] S31, sending the first mixture to a crude liquid tank with a temperature of 90° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 90° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 10 g / L;
[0115] S41, filtering the second mixture by leaf filtration to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 195;
[0116] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0117] S61. calcining the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.020%.
[0118] Comparative Example 2
[0119] This comparative example provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0120] S11, take the sodium aluminate semen from the alumina production site and cool it to 90℃. The concentration of sodium aluminate semen is Na2O T 150g / L, Na2O k 145g / L, Al2O3 159g / L, Na2O C 5g / L, SiO2 0.95g / L, a K 1.50, silicon content index 167;
[0121] S21, preparing lime milk with red mud washing water, wherein the solid content of the lime milk is 250 g / L, and uniformly mixing the lime milk with sodium aluminate semen in a volume ratio of 1:1, and reacting at 90° C. for 60 min to obtain a first mixture;
[0122] S31, sending the first mixture to a crude liquid tank with a temperature of 100° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 100° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 10 g / L;
[0123] S41, leaf filtering the second mixture to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 180;
[0124] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0125] S61. calcining the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.022%.
[0126] Comparative Example 3
[0127] A method for reducing the silicon content in an alumina product mainly comprises the following steps:
[0128] This comparative example provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0129] S11, take the sodium aluminate semen from the alumina production site and cool it to 60℃. The concentration of sodium aluminate semen is Na2O T 150g / L, Na2O k 145g / L, Al2O3 159g / L, Na2O C 5g / L, SiO2 0.95g / L, a K 1.50, silicon content index 167;
[0130] S21, preparing lime milk with red mud washing water, wherein the solid content of the lime milk is 250 g / L, and uniformly mixing the lime milk with sodium aluminate semen in a volume ratio of 1:1, and reacting at 60° C. for 15 min to obtain a first mixture;
[0131] S31, sending the first mixture to a crude liquid tank with a temperature of 95° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to perform a desiliconization reaction at a temperature of 95° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 15 g / L;
[0132] S41, filtering the second mixture by leaf filtration to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 175;
[0133] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0134] S61. calcining the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.022%.
[0135] Comparative Example 4
[0136] This comparative example provides a method for reducing the silicon content in an alumina product, comprising the following steps:
[0137] S11, take the sodium aluminate semen from the alumina production site and cool it to 70℃. The concentration of sodium aluminate semen is Na2O T 160g / L, Na2O k 145g / L, Al2O3 159g / L, Na2O C 15g / L, SiO2 0.90g / L, aK 1.50, silicon content index 177;
[0138] S21, preparing lime milk with red mud washing water, the lime milk having a solid content of 300 g / L, and uniformly mixing the lime milk with sodium aluminate semen in a volume ratio of 1:3, and reacting at 70° C. for 40 min to obtain a first mixture;
[0139] S31, sending the first mixture to a crude liquid tank at a temperature of 100° C., mixing with a crude sodium aluminate solution, and leaving the mixture in the crude liquid tank for 60 minutes to undergo a desiliconization reaction at a temperature of 100° C. for 60 minutes, to obtain a second mixture; wherein the solid content of the filter aid in the second mixture is 20 g / L;
[0140] S41, filtering the second mixture by leaf filtration to obtain a refined sodium aluminate liquid, wherein the silicon content index of the refined sodium aluminate liquid is 190;
[0141] S51, subjecting the sodium aluminate refined liquid to seed decomposition to obtain aluminum hydroxide; and
[0142] S61. calcining the aluminum hydroxide to obtain an aluminum oxide product, wherein the SiO2 content in the aluminum oxide product is 0.023%.
[0143] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0144] In the embodiment of the present invention, by adjusting the preparation conditions of the filter aid, the desiliconization effect of the crude liquid is enhanced, the silicon content index of the semen is effectively increased to above 250, and the silicon dioxide content in the alumina product is reduced to below 0.015%.
[0145] In the embodiments of the present invention, the provided method does not cause much change to the existing process, requires little investment, and is easy to apply industrially.
[0146] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for reducing the silicon content in an alumina product, characterized in that: The method comprises: Get the Na2O C Sodium aluminate semen of concentration and set temperature; Adding lime milk to the sodium aluminate semen to react at the set temperature and set time to obtain a first mixture; adding the first mixture to a crude sodium aluminate solution to perform a desiliconization reaction to obtain a second mixture; filtering the second mixture to obtain a refined sodium aluminate liquid; Decomposing the sodium aluminate refined liquid by seed crystal decomposition to obtain aluminum hydroxide; and The aluminum hydroxide is calcined to obtain an aluminum oxide product.
2. The method according to claim 1, characterized in that The setting of Na2O C Concentration ≥10g / L.
3. The method according to claim 1, characterized in that The set temperature is 60°C to 80°C.
4. The method according to claim 1, characterized in that: The set time is 30 minutes to 60 minutes.
5. The method according to claim 1, characterized in that The lime milk is prepared by using red mud washing water or aluminum hydroxide washing water, and the solid content of the lime milk is 250g / L to 300g / L.
6. The method according to claim 1, characterized in that The volume ratio of the lime milk to the sodium aluminate semen is 1:(1-4).
7. The method according to claim 1, characterized in that The temperature of the desiliconization reaction is 80° C. to 95° C., and the time of the desiliconization reaction is 60 min to 120 min.
8. The method according to claim 1, characterized in that The solid content of the filter aid in the second mixture is 5 g / L to 20 g / L.
9. The method according to claim 1, characterized in that: The silicon content index of the sodium aluminate refined liquid is ≥250.
10. An alumina product prepared by the method according to any one of claims 1 to 9, characterized in that: Calculated by mass fraction, the SiO2 content in the alumina product is ≤0.015%.