Silicone rubber insulator repairing method and used repairing material
By using polar group-modified room-temperature vulcanized coating material on the surface of silicone rubber insulating material for repair, the problems of surface energy increase and poor compatibility caused by aging are solved, effective repair results are achieved, and the resistance of insulating material is improved Cracking and service life.
Patent Information
- Application Number
- CN202411285032.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
AI Technical Summary
Silicone rubber insulating materials age due to long-term exposure to external factors, resulting in increased surface energy, making it difficult to form an effective bonding interface with traditional RTV coatings, resulting in poor repair results and affecting the long-term and stable operation of the equipment.
The matrix resin and curing agent are mixed in a specific proportion, and the polar group-modified silicone resin is added to form a room-temperature vulcanized coating material. The surface of the silicone rubber insulating material is repaired by spraying, pouring or brushing to overcome the phase Poor capacitance and low bonding strength.
It effectively repairs cracks on the surface of silicone rubber insulating material, restores its water repellency and resists external erosion, improves the crack resistance and service life of the material, and reduces maintenance costs and energy consumption.
Smart Images

Figure SMS_1 
Figure HDA0005042885240000011 
Figure HDA0005042885240000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of power insulation materials, and in particular to a method for repairing surface aging of silicone rubber insulators. Background Art
[0002] In recent years, silicone rubber materials have been widely used in external insulation of power systems due to their excellent high and low temperature resistance, hydrophobicity, hydrophobic migration, weather resistance and anti-pollution flashover performance. However, due to the long-term influence of external factors, silicone rubber insulation materials are prone to breakage of silicone rubber macromolecular chains, which causes silicone rubber insulation materials to degrade or over-crosslink, and inevitably lead to local cracking phenomena such as powdering, cracking, and hardening, resulting in reduced performance of insulation materials and shortened service life. This poses a huge threat to the long-term stable operation of power transmission and transformation equipment, and the overall replacement of locally cracked composite insulation equipment requires a long maintenance cycle and high replacement cost. Summary of the invention
[0003] The present invention provides a silicone rubber insulator repair method for repairing aging of the surface of a silicone rubber insulator and a room temperature vulcanized coating material, aiming to solve the technical problems mentioned in the above background technology.
[0004] The inventors have found through research that an ideal method is to use RTV coating to locally repair the surface of aged silicone rubber insulation materials so that it can achieve the operating performance of new equipment. In comparison, this method has short maintenance time and low cost. However, under the oxidation of various factors such as oxygen and ultraviolet rays in the air, the outer surface of the silicone rubber insulator will produce a large number of strong polar groups, and the surface energy will increase rapidly. This makes the compatibility between the aged surface of the silicone rubber insulator and the general RTV coating extremely poor, making it difficult to form an effective and stable bonding interface, which in turn leads to poor repair effects and difficulty in maintaining the normal operation of the equipment. Based on this, studying a suitable method and material for repairing the surface aging of silicone rubber insulators is an economical and fast way to maintain the safe, stable operation of UHV transmission and transformation systems.
[0005] The technical solution adopted by the present invention is as follows: A method for repairing a silicone rubber insulator, the steps are as follows: S1. After uniformly mixing a base resin and a curing agent in a mass ratio of 2 to 10:1, a solvent is added to dilute the mixture to obtain a repair material; the base resin is an organic silicone resin obtained by copolymerization and modification of polysiloxane and a polymer prepolymer with a polar group; the polar group is an epoxy group or an acrylate group; S2. Apply the repair material prepared in S1 to the cracked parts on the surface of the aged silicone rubber insulator, and react at room temperature until it is completely cured.
[0006] The coating method in step S2 is one or more of brushing, spraying, dipping and pouring; the coating thickness is 0.5 mm to 2 mm.
[0007] In step S2, the reaction temperature is 20-30° C. and the reaction time is 96-72 h.
[0008] The curing agent in step S1 is one or more of polyisocyanate, melamine formaldehyde, and alkoxy-containing methylamino resin.
[0009] The solvent is ethyl acetate or butyl acetate; the amount of the solvent added is 50%-80% of the mass of the base resin.
[0010] The polysiloxane is 2-hydroxy-dimethylsiloxane, 2-hydroxy-methylvinylsiloxane or 2-hydroxy-methylphenylsiloxane.
[0011] The polymer prepolymer with polar groups is bisphenol A epoxy resin and polybutyl methacrylate; The base resin in step S1 is prepared by the following steps: The coupling agent and the polymer prepolymer with polar groups are reacted at 80±3°C for 3±0.3h to obtain a modifier; the mass ratio of the coupling agent to the polymer prepolymer with polar groups is (1~2):5; The modifier, polysiloxane and catalyst are mixed in a mass ratio of (2-1):1:0.1 to obtain a modified silicone resin; The polymer prepolymer with polar groups is bisphenol A epoxy resin and polybutyl methacrylate; The polysiloxane is 2-hydroxy-dimethylsiloxane, 2-hydroxy-methylvinylsiloxane or 2-hydroxy-methylphenylsiloxane.
[0012] The coupling agent is γ-aminopropyl triacetoxysilane or γ-glycidyloxypropyl trimethoxysilane.
[0013] The catalyst is dibutyltin dilaurate.
[0014] Preferably, the mass ratio of the base resin to the curing agent is 2-3:1.
[0015] The mass ratio of the base resin to the curing agent is 2:1 or 5:1 or 10:1. When the mass ratio is 2:1, the tensile strength of the material can reach more than 4.5MPa, and the elongation at break can reach 40%; when the mass ratio is 5:1, the tensile strength of the material can reach more than 3.3MPa, and the elongation at break can reach 100%; when the mass ratio is 10:1, the intrinsic tensile strength of the material can reach more than 2.1MPa, and the elongation at break can reach 160%. The specific ratio can be adjusted according to the actual use and selected according to the specific use scenario of the insulator. When used in outdoor areas with many birds, in order to prevent bird pecking, a ratio that is more favorable to improving the tensile strength can be selected, such as a mass ratio of the base resin to the curing agent of 2:1; when the use scenario requires the material to have a certain toughness, a ratio that is more favorable to improving the elongation at break can be selected, such as a mass ratio of the base resin to the curing agent of 10:1.
[0016] The present invention also provides a repair material used in the above-mentioned silicone rubber insulator repair method, and its components in parts by weight are as follows: Base resin 100; Curing agent 10~50; Solvent 50~80; The base resin is an organic silicon resin obtained by copolymerization and modification of polysiloxane and a high molecular prepolymer with polar groups; the polar groups are epoxy groups or acrylate groups.
[0017] The high molecular prepolymer with polar groups is bisphenol A epoxy resin and polybutyl methacrylate.
[0018] The polysiloxane is 2-hydroxy-dimethylsiloxane, 2-hydroxy-methylvinylsiloxane or 2-hydroxy-methylphenylsiloxane.
[0019] The curing agent is one or more of polyisocyanate and melamine formaldehyde.
[0020] The solvent is ethyl acetate or butyl acetate.
[0021] The beneficial effects of the present invention are: 1) The repair material used in the present invention includes two components: a base resin and a curing agent. The main component of the base resin is a polar group-modified organic silicon resin. When used, it can be applied to the aged surface of the silicone rubber insulator by spraying, pouring or brushing, etc. after being mixed evenly in a certain proportion, and then placed at room temperature for a certain period of time to cure. Due to the presence of polar segments, the repair material used can well overcome the problems of increased surface energy of the silicone rubber insulator due to aging and poor compatibility with organic silicon molecules, and can form a stable and firm bonding interface with it, while repairing the cracks on the surface of the silicone rubber insulator and restoring its hydrophobicity and ability to resist external erosion.
[0022] 2) The silicone rubber aged surface repair coating material used in the present invention is a modified room temperature vulcanized silicone rubber coating, which introduces polar groups into the chemical structure of the silicone material. The principle of similar polarity compatibility of chemical groups is used to overcome the poor compatibility between the aged surface of the insulating material with polar groups and the traditional RTV coating, low bonding strength and other problems, so that a good bonding interface can be formed between the substrate and the coating. At the same time, the non-polar silicone chain segments diffuse at the gas-solid interface, greatly reducing its surface energy, effectively solving the problems of increased surface energy and loss of hydrophobicity caused by surface aging of silicone rubber materials.
[0023] 3) The repair method provided by the present invention uses the aged silicone rubber surface repair coating material to greatly repair the aged cracks on the surface of the silicone rubber insulating material, thereby restoring the density of its outer surface to a great extent, and can greatly improve the ability of the silicone rubber insulating material surface to resist external erosion.
[0024] 4) The silicone rubber aged surface repair coating material used in the present invention can be cured at room temperature. Compared with traditional HTV coatings, it not only reduces the energy consumption and cost of the curing process, but also reduces the construction difficulty of high-altitude operations, which is of great significance to the repair work of insulating materials for high-voltage power transmission. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the surface morphology of the aged silicone rubber insulation material in Example 1.
[0026] Figure 2 This is a surface morphology of the repaired silicone rubber insulation material of Example 1.
[0027] Figure 3 This is a surface morphology of the repaired silicone rubber insulation material of Example 2.
[0028] Figure 4 This is a surface morphology of the repaired silicone rubber insulation material of Example 3.
[0029] Figure 5 This is the surface morphology of the repaired silicone rubber insulation material of Comparative Example 1. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without carrying out creative work are within the scope of protection of the present invention.
[0031] Technologies, methods, and apparatus known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, such technologies, methods, and apparatus should be considered part of the authorization specification. Example 1
[0032] The base resin is prepared in the following steps: γ-aminopropyl triacetoxysilane and bisphenol A epoxy resin are reacted at 80° C. for 3 hours to obtain a modifier. The modifier is mixed with 2-hydroxy-dimethylsiloxane resin and dibutyltin diisocyanate in a mass ratio of 2:1:0.1 to obtain a modified silicone resin, namely the base resin.
[0033] The method for repairing the surface aging of a silicone rubber insulator provided in this embodiment comprises the following steps: 10g of base resin and 5g of melamine formaldehyde were mixed evenly, and 5g of butyl acetate was added to dilute it. After placing it in a vacuum drying oven to remove internal bubbles, the repair material was obtained. The repair material was applied to the cracked part of the upper surface of the silicone rubber insulation material sample prepared in advance by pouring, and the pouring thickness was controlled to be about 1mm. It was fully cured after fully reacting at 25°C for 80h. During the curing process of the repair material, it will further react so that the modifier in the base resin is combined with dimethylsiloxane.
[0034] The results of scanning electron microscope tests show that there are a lot of cracks and defects on the surface of aged silicone rubber insulators, such as Figure 1 As shown; the surface cracks of the insulators repaired with the repair material are well restored, as shown Figure 2 As shown. According to the standard DL / T 376-2010, the hydrophobic contact test results show that the static water contact angle of the repaired aged silicone rubber surface can reach 107°. According to the GB / T 9286-1998 test, its adhesion level can reach level 0. Example 2
[0035] The base resin is prepared in the following steps: γ-glycidyloxypropyltrimethoxysilane and bisphenol A epoxy resin are reacted at 80° C. for 3 hours to obtain a modifier. The modifier is mixed with 2-hydroxy-dimethylsiloxane resin and dibutyltin diisocyanate in a mass ratio of 2:1:0.1 to obtain a modified silicone resin, i.e., the base resin.
[0036] The method for repairing the surface aging of a silicone rubber insulator provided in this embodiment comprises the following steps: 10g of base resin and 2.5g of triphenylmethane triisocyanate were mixed evenly, and 6g of ethyl acetate was added to dilute it. The repair material was placed in a vacuum drying oven to remove internal bubbles and then coated on the upper surface of the silicone rubber insulating material sample prepared in advance by dip coating. The coating thickness was controlled to be about 0.5mm, and the material was fully cured after fully reacting for 72h at room temperature of 25°C.
[0037] The results of the scanning electron microscope test showed that the surface cracks of the insulators repaired with the repair material were well restored, such as Figure 3 As shown. According to the standard DL / T 376-2010, the hydrophobic contact test results show that the static water contact angle of the repaired aged silicone rubber surface can reach 103°. According to the GB / T 9286-1998 test, its adhesion level can reach level 0. Example 3
[0038] The base resin is prepared in the following steps: γ-aminopropyl triacetoxysilane and polybutyl methacrylate are reacted at 80° C. for 3 hours to obtain a modifier. The modifier is mixed with 2-hydroxy-methylphenylsiloxane and dibutyltin diisocyanate in a mass ratio of 2:1:0.1 to obtain a modified silicone resin, namely the base resin.
[0039] The method for repairing the surface aging of a silicone rubber insulator provided in this embodiment comprises the following steps: 10g of base resin and 1g of melamine formaldehyde were mixed evenly, and 8g of butyl acetate was added to dilute it. After placing it in a vacuum drying oven to remove internal bubbles, it was applied to the upper surface of the silicone rubber insulating material sample prepared in advance by brushing, and the coating thickness was controlled to be about 0.5mm. It was fully cured after fully reacting at room temperature of 25°C for 96 hours.
[0040] The results of the scanning electron microscope test showed that the surface cracks of the insulators repaired with the repair material were well restored, such as Figure 4 As shown. According to the standard DL / T 376-2010, the hydrophobic contact test results show that the static water contact angle of the repaired aged silicone rubber surface can reach 109°. According to the GB / T 9286-1998 test, its adhesion level can reach level 0. Comparative Example 1
[0041] This comparative example provides a use effect of a commercially available RTV room temperature vulcanized silicone rubber coating, and the repair method thereof is as follows: Mix 10g of commercially available silicone resin and 2g of curing agent evenly, add appropriate amount of solvent to dilute, place in a vacuum drying oven to remove internal bubbles, and apply it to the upper surface of the prepared silicone rubber insulation material sample by pouring coating. The coating thickness is controlled at about 1mm, and fully reacted at room temperature for 85h before curing.
[0042] The results of the scanning electron microscope test showed that the surface cracks of the insulators were restored after being repaired with the repair material. Figure 5 As shown. According to the standard DL / T 376-2010, the hydrophobic contact test results show that the static water contact angle of the repaired aged silicone rubber surface can reach 115°. However, according to GBT 9286-1998, its adhesion level only reaches level 3.
[0043] The test results of the above three specific embodiments are compared as shown in the following table:
[0044] As can be seen from the above table, the repair material used in the present invention can form an effective bonding interface with the surface of the silicone rubber insulating material, while the commercially available RTV coating has poor compatibility with the aged surface and the adhesion cannot meet the use requirements. The inventors found that the main reason is that under the action of long-term high pressure and oxygen in the air, the side chain methyl of the polysiloxane is oxidized and removed, forming a hydrophilic hydroxyl group. The hydrogen atoms on the hydroxyl group can form hydrogen bonds with the oxygen atoms on the acrylate / epoxy group (polar group), strengthening the interaction between molecules, thereby forming a good bonding interface.
[0045] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for repairing a silicone rubber insulator, characterized in that: Here are the steps: S1. After uniformly mixing a base resin and a curing agent in a mass ratio of 2 to 10:1, a solvent is added to dilute the mixture to obtain a repair material; the base resin is an organic silicone resin obtained by copolymerization and modification of polysiloxane and a polymer prepolymer with a polar group; the polar group is an epoxy group or an acrylate group; S2. Apply the repair material prepared in S1 to the cracked parts on the surface of the aged silicone rubber insulator, and react at room temperature until it is completely cured.
2. The method for repairing a silicone rubber insulator according to claim 1, characterized in that: The coating method in step S2 is one or more of brushing, spraying, dipping and pouring; the coating thickness is 0.5 mm to 2 mm.
3. The method for repairing a silicone rubber insulator according to claim 1, characterized in that: In step S2, the reaction temperature is 20-30° C. and the reaction time is 96-72 h.
4. The method for repairing a silicone rubber insulator according to claim 1, characterized in that: The curing agent in step S1 is one or more of polyisocyanate, melamine formaldehyde, and alkoxy-containing methylamino resin; the solvent is ethyl acetate or butyl acetate; and the amount of solvent added is 50%-80% of the mass of the base resin.
5. The method for repairing a silicone rubber insulator according to claim 1, characterized in that: The polysiloxane is 2-hydroxy-dimethylsiloxane, 2-hydroxy-methylvinylsiloxane or 2-hydroxy-methylphenylsiloxane.
6. The method for repairing a silicone rubber insulator according to claim 1, characterized in that: The high molecular prepolymer with polar groups is bisphenol A epoxy resin and polybutyl methacrylate.
7. The method for repairing a silicone rubber insulator according to claim 1, characterized in that: The base resin in step S1 is prepared by the following steps: The coupling agent and the polymer prepolymer with polar groups are reacted at 80±3°C for 3±0.3h to obtain a modifier; the mass ratio of the coupling agent to the polymer prepolymer with polar groups is (1~2):5; The modifier, polysiloxane and catalyst are mixed in a mass ratio of (2-1):1:0.1 to obtain a modified silicone resin; The polymer prepolymer with polar groups is bisphenol A epoxy resin and polybutyl methacrylate; The polysiloxane is 2-hydroxy-dimethylsiloxane, 2-hydroxy-methylvinylsiloxane or 2-hydroxy-methylphenylsiloxane.
8. The method for repairing a silicone rubber insulator according to claim 7, characterized in that: The coupling agent is γ-aminopropyl triacetoxysilane and γ-glycidyloxypropyl trimethoxysilane; and the catalyst is dibutyltin dilaurate.
9. A repair material used in the silicone rubber insulator repair method according to claim 1, characterized in that: Its components are calculated by weight as follows: Base resin 100; Curing agent 10~50; Solvent 50~80; The base resin is an organic silicon resin obtained by copolymerization and modification of polysiloxane and a high molecular prepolymer with polar groups; the polar groups are epoxy groups or acrylate groups.
10. The repair material according to claim 9, characterized in that: The polymer prepolymer with polar groups is bisphenol A epoxy resin or polybutyl methacrylate; the polysiloxane is 2-hydroxy-dimethylsiloxane, 2-hydroxy-methylvinylsiloxane or 2-hydroxy-methylphenylsiloxane; the curing agent is one or more of polyisocyanate and melamine formaldehyde; and the solvent is ethyl acetate or butyl acetate.