Processing method of polycrystalline diamond composite blade
The internal stress is released in the polycrystalline diamond composite blade through heat treatment, which solves the residual internal stress problem caused by the difference in the thermal expansion coefficient of the material, improves the processing quality and reduces production costs.
Patent Information
- Application Number
- CN202411007460.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-26
AI Technical Summary
The residual internal stress caused by the difference in the thermal expansion coefficient of the polycrystalline diamond composite blade affects the processing quality, resulting in defects such as processing cracks and arches, reducing product quality and increasing production costs.
The heat treatment method is adopted, including performing the first insulation treatment and the second insulation treatment of 500 to 800°C in an oxygen-free environment of 350 to 750°C. Combined with cooling and heating rate control, releasing internal stress and reducing residual heat caused by differences in thermal expansion coefficients. Stress, reduce the arcuate.
Effectively reduce the residual internal stress of polycrystalline diamond composite blades, reduce processing defects, improve product quality grade, and reduce high-quality product manufacturing costs.
Smart Images

Figure CN119020575A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for processing a polycrystalline diamond composite blade, and belongs to the field of preparation of polycrystalline diamond composite blades. Background Art
[0002] Polycrystalline diamond composite blades are a new type of functional material, known as the teeth of industry. They are made of diamond powder and cemented carbide substrate, and are sintered under high temperature and high pressure (HTHP). They have the high hardness, high wear resistance and thermal conductivity of diamond, as well as the strength and impact toughness of cemented carbide. They are mainly used for precision processing of non-ferrous metals, wood furniture and other non-metallic materials.
[0003] As we all know, the larger the diameter of the diamond composite blade, the more selectivity and utilization rate of laser processing will be significantly improved, and the production cost will be significantly reduced. Due to the different thermal expansion coefficients of cemented carbide and diamond, there is a large residual internal stress inside the diamond composite blade after high temperature and high pressure sintering. As the diameter of the diamond composite blade product continues to increase, the residual internal stress value also continues to increase. The existence of residual internal stress has a great impact on defects such as cracks in the processing of diamond composite blades and arch after flat grinding. Summary of the invention
[0004] The object of the present invention is to provide a method for processing a polycrystalline diamond composite blade, which can significantly reduce the camber degree of the polycrystalline diamond composite blade and improve the product quality grade.
[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0006] A method for processing a polycrystalline diamond composite blade comprises the following steps: subjecting the polycrystalline diamond composite blade to a heat treatment; the heat treatment method comprises the following steps: subjecting the polycrystalline diamond composite blade to a first heat preservation treatment in an oxygen-free environment and cooling; the temperature of the first heat preservation treatment is 350-750°C and the time is 3-15 hours.
[0007] The processing method of the polycrystalline diamond composite blade of the present invention can fully relax the differences between the crystal structures and the lattice distortion characteristics in the polycrystalline diamond composite blade by keeping the polycrystalline diamond composite blade at 350-750°C for 3-15h, release the internal stress between the crystal structures and the lattice distortion in the polycrystalline diamond composite blade, achieve the effect of reducing the residual internal stress, and can also reduce the residual thermal stress generated by the large difference in physical parameters such as the thermal expansion coefficient between the cemented carbide substrate and the diamond layer. The processing method of the present invention can effectively reduce the residual internal stress of the polycrystalline diamond composite blade, improve the processing and manufacturing process, reduce the processing crack defects of the diamond composite blade and reduce the size of the arch degree of flat grinding, improve the product quality level, and reduce the manufacturing cost of high-quality products.
[0008] In order to further enhance the treatment effect, the temperature of the first insulation treatment is 400-600°C, and the time is 4-12h. For example, the temperature of the first insulation treatment is 400°C, 515°C, 550°C, 480°C or 600°C, and the time is 4h, 6h, 8h, 10h or 15h.
[0009] When the heating rate is too high, it is easy to cause the internal thermal stress of the polycrystalline diamond composite blade to increase. In order to reduce the increase of internal stress during the treatment process, the heating rate to the temperature of the first insulation treatment is ≤10°C / min. Furthermore, the heating rate to the temperature of the first insulation treatment is 2 to 8°C / min, for example, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min or 8°C / min.
[0010] Furthermore, the heat treatment method also includes the following steps: subjecting the cooled polycrystalline diamond composite blade to a second heat preservation treatment in an oxygen-free environment for cooling; the temperature of the second heat preservation treatment is 500-800°C and the time is 0.5-3h. After the first heat preservation treatment, the second heat preservation treatment can further relax the differences between the crystal structures and the lattice distortion characteristics in the polycrystalline diamond composite blade, release the internal stress generated by their interaction; and further reduce the residual thermal stress generated due to the large difference in physical parameters such as the thermal expansion coefficient between the cemented carbide substrate and the diamond layer, as well as the residual internal stress generated during the manufacturing process, and further reduce the residual stress of the polycrystalline diamond composite blade.
[0011] In order to further reduce the residual stress of the polycrystalline diamond composite blade and improve the effect of improving the camber, the polycrystalline diamond composite blade cooled after the first heat preservation treatment is further subjected to flat grinding and then subjected to the second heat preservation treatment. The oxygen-free environment is a vacuum environment or a nitrogen atmosphere or an inert gas atmosphere.
[0012] In order to further enhance the treatment effect, the temperature of the second heat preservation treatment is 580-720° C., and the time is 0.6-2.5 hours. For example, the temperature of the second heat preservation treatment is 660° C. or 690° C., and the time is 1 or 1.5 hours.
[0013] When the heating rate is too high, it is easy to cause the internal thermal stress of the polycrystalline diamond composite blade to increase. In order to reduce the increase of internal stress during the treatment process, the heating rate to the temperature of the second insulation treatment is ≤12°C / min. The heating rate to the temperature of the second insulation treatment is 3 to 10°C / min, for example, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min or 8°C / min.
[0014] Furthermore, before the polycrystalline diamond composite blade is subjected to heat treatment, the polycrystalline diamond composite blade is first subjected to cold treatment at -200 to -140° C. The cold treatment can form a compressive stress state on the surface of the polycrystalline diamond composite blade, effectively reducing the residual tensile stress at the cemented carbide substrate and the interface between the cemented carbide substrate and the diamond layer.
[0015] For cemented carbide with a bonding metal containing Co as the matrix, cold treatment can also promote the transformation of the residual high-temperature phase (FCC structure) of the Co element in the alloy substrate and the diamond composite layer into a low-temperature phase (HCP structure), thereby improving the organizational stability and the dimensional stability of the polycrystalline diamond composite blade.
[0016] Furthermore, the cold treatment time is 3 to 8 hours, and the temperature is raised to 100 to 160°C after the cold treatment and then cooled. The residual high temperature phase (FCC structure) and low temperature phase (HCP structure) of cemented carbide have a density of 0.74, but the FCC structure has more slip systems and better toughness. After the FCC structure is transformed into the HCP structure, the overall toughness of the polycrystalline diamond composite blade deteriorates, the brittleness increases, and the internal stress generated by the crystal structure and organizational transformation increases. In order to avoid the deterioration of the improvement effect of reducing the internal stress, the temperature is first raised to 100 to 160°C and then cooled after the cold treatment is completed. The cooling after heating to 100 to 160°C is preferably air cooling. The rate of heating to 100 to 160°C is 2 to 8°C / min, for example, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min or 8°C / min.
[0017] In order to further enhance the treatment effect, the temperature of the cold preservation treatment is -190 to -150°C, and the time is 3 to 8 hours. For example, the temperature of the cold preservation treatment is -160°C, -170°C or -180°C, and the time is 4 hours, 5 hours, 6 hours or 7 hours.
[0018] When the cooling rate is too high, it is easy to cause the crystal structure and organization to change violently and too quickly, and the internal stress increases significantly. In order to reduce the increase of internal stress of the polycrystalline diamond composite blade during the cooling process, the cooling rate to the cold treatment temperature is ≤15℃ / min, for example, 4℃ / min, 8℃ / min or 10℃ / min. The cooling rate to the cold treatment temperature is 6-12℃ / min.
[0019] Furthermore, the polycrystalline diamond composite blade is made of diamond powder and cemented carbide; the bonding metal of the cemented carbide contains Co. Furthermore, the cemented carbide is mainly composed of Co and WC, for example, the mass percentage of WC in the cemented carbide is 70-95%. The phase transition temperature of pure Co element is 633K (about 360°C), but due to the pinning effect of the WC phase and the Co phase interface and the solid solution of fine WC particles into the Co phase, the two work together to increase the phase transition temperature of the Co phase (about 600°C to 1000°C). When the heating temperature of the polycrystalline diamond composite blade reaches the phase transition temperature, the low temperature phase (HCP structure) of the Co element will transform into the high temperature phase (FCC structure), and vice versa, the high temperature phase (FCC structure) of the Co element will transform into the low temperature phase (HCP structure).
[0020] Furthermore, the polycrystalline diamond composite blade to be processed in the present invention is obtained by assembling diamond micropowder and cemented carbide, sintering at high temperature and high pressure, and then trimming and PCD surface processing. A flat polycrystalline diamond composite blade surface can be obtained by trimming. The purpose of PCD surface processing is to meet the PCD layer thickness required by customers.
[0021] Furthermore, the cooling after the first insulation treatment is first cooled to 200-300°C in the furnace, and then air-cooled out of the furnace, for example, first cooled to 250°C in the furnace, and then air-cooled out of the furnace. Further, the cooling after the second insulation treatment is first cooled to 200-300°C in the furnace, and then air-cooled out of the furnace, for example, first cooled to 250°C in the furnace, and then air-cooled out of the furnace. Compared with other cooling methods, the above cooling process can reduce or reduce the increase in residual thermal stress of the polycrystalline diamond composite blade caused by the excessively high furnace temperature, thereby avoiding the deterioration of the overall improvement effect. In addition, the cooling after the first insulation treatment and the cooling after the second insulation treatment can be cooled by air cooling throughout the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope microscopic morphology image of the polycrystalline diamond composite blade after treatment in Example 1 of the present invention;
[0023] Figure 2 This is a scanning electron microscope microscopic morphology image of the polycrystalline diamond composite blade after treatment in Example 6 of the present invention;
[0024] Figure 3 This is a scanning electron microscope microscopic morphology image of the polycrystalline diamond composite blade after treatment in Example 11 of the present invention;
[0025] Figure 4 Schematic diagram of the detection position of the polycrystalline diamond composite blade arch in the experimental example;
[0026] Figure 5This is a schematic diagram of using a dial indicator to detect the arch degree of a polycrystalline diamond composite blade in an experimental example. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further described below in conjunction with specific implementation methods.
[0028] The polycrystalline diamond composite blade used for processing in each embodiment is obtained by a method including the following steps: diamond powder is placed in a high temperature resistant cup and placed in a vacuum furnace for pretreatment at 980°C under vacuum conditions for 0.5h, and then the mixture obtained by mixing the diamond powder and the metal powder of the combination of Co and WC (wherein the diamond particle size is 0.5μm to 35μm) is compacted and assembled with a cemented carbide matrix by a press, and then placed in a high temperature resistant cup, and then the cup is placed in a sintered block for high temperature and high pressure (HTHP) sintering to form a polycrystalline diamond composite blade, and then the blade is trimmed and PCD surface processing is performed. The mass ratio of diamond powder to the metal powder of the combination of Co and WC during mixing is 9:1. The temperature of high temperature and high pressure sintering is 1500°C, the pressure is 6.5GPa, and the time is 18min.
[0029] The cemented carbide matrix used in the preparation of the polycrystalline diamond composite blades in Examples 1 to 15 is composed of WC and Co, and the mass percentage of WC is 85%. The cemented carbide used in the preparation of the polycrystalline diamond composite blade in Example 16 is a Ni-Cr-Co based cemented carbide, with a mass percentage of Ni of 70%, a mass percentage of Cr of 10%, and the balance of Co.
[0030] During the high temperature and high pressure sintering process of cemented carbide substrate and diamond powder, the original crystal structure is constantly changing. For example, the Co element changes from solid phase to liquid phase, and the WC phase (part of the WC phase dissolves into the liquid phase of Co) diffuses into the diamond powder layer along with the Co liquid. In the subsequent sintering and cooling process, the WC phase recrystallizes, precipitates and grows, and forms a new WC phase (hexagonal lattice). A small amount of WC particles are dissolved into the solid phase Co element, and the solid phase Co element has both FCC structure and HCP structure. For another example, the surface of the diamond powder particles after pretreatment is partially graphitized. During the high temperature and high pressure sintering process, the carbon in the graphite dissolves into the diffused Co liquid. Relying on the Co liquid as a catalyst, the graphite on the surface of the diamond particles begins to transform into diamond (regular tetrahedron) again, and connects with the adjacent diamond particles (forming DD bonds). During the entire high temperature and high pressure (HTHP) sintering process, the internal crystal structure of the cemented carbide substrate and diamond powder continues to change, eventually forming new WC phase, Co phase and diamond phase. The crystal structures of the new phases are different and are accompanied by lattice distortion. In the sintered polycrystalline diamond composite blade, they squeeze and pull each other, forming large residual internal stress, especially at the interface between the cemented carbide substrate and the diamond layer, where the local residual stress is the largest.
[0031] In addition, during the high temperature and high pressure (HTHP) sintering process, due to the thermal expansion coefficient of the cemented carbide substrate and the diamond layer (WC / Co is 6×10 -6 K, PCD is 2.36×10 -6 The physical parameters such as K) and elastic modulus (517GPa~655GPa for WC / Co and 827GPa~896GPa for PCD) are quite different, so the reaction rates to pressure relief and cooling are different, which inevitably produces severe residual stress (thermal stress) at the interface, resulting in weakened adhesion between polycrystalline diamond and cemented carbide substrate, poor impact resistance of diamond layer, and easy cracking, falling off and other defects.
[0032] The polycrystalline diamond composite blades processed by the following processing methods of Examples 1 to 15 are all polycrystalline diamond composite blades after the PCD surface processing described above. The processed polycrystalline diamond composite blades can be repaired or polished as needed, and then flat-ground to the required size and thickness.
[0033] Example 1
[0034] The processing method of the polycrystalline diamond composite blade of this embodiment includes the following steps: placing the polycrystalline diamond composite blade after PCD surface processing into a vacuum heat treatment furnace, heating it to 550°C at a rate of 3°C / min under vacuum conditions and keeping it warm for 6 hours, then cooling it to 200°C with the furnace, and then air cooling it to room temperature.
[0035] Example 2
[0036] The processing method of the polycrystalline diamond composite blade of this embodiment includes the following steps: placing the polycrystalline diamond composite blade after PCD surface processing into a vacuum heat treatment furnace, heating it to 400°C at a rate of 2°C / min under vacuum conditions and keeping it warm for 10 hours, then cooling it to 250°C with the furnace, and then air cooling it to room temperature.
[0037] Example 3
[0038] The processing method of the polycrystalline diamond composite blade of this embodiment includes the following steps: placing the polycrystalline diamond composite blade after PCD surface processing into a vacuum heat treatment furnace, heating it to 600°C at a rate of 6°C / min under vacuum conditions and keeping it warm for 8 hours, then cooling it to 300°C with the furnace, and then air cooling it to room temperature.
[0039] Example 4
[0040] The processing method of the polycrystalline diamond composite blade of this embodiment includes the following steps: placing the polycrystalline diamond composite blade after PCD surface processing into a vacuum heat treatment furnace, heating it to 750°C at a rate of 10°C / min under vacuum conditions and keeping it warm for 3 hours, then cooling it to 250°C with the furnace, and then air cooling it to room temperature.
[0041] Example 5
[0042] The processing method of the polycrystalline diamond composite blade of this embodiment includes the following steps: placing the polycrystalline diamond composite blade after PCD surface processing into a vacuum heat treatment furnace, heating it to 350°C at a rate of 8°C / min under vacuum conditions and keeping it warm for 15 hours, then cooling it to 200°C with the furnace, and then air cooling it to room temperature.
[0043] Example 6
[0044] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0045] 1) Place the PCD surface processed polycrystalline diamond composite blade into a box-type cold treatment furnace and cool it down to -180°C at a rate of 6°C / min for 5 hours, then heat it up to 135°C at a rate of 3°C / min, and then take it out of the furnace and air cool it to room temperature;
[0046] 2) The polycrystalline diamond composite blade cooled in step 1) is placed in a vacuum heat treatment furnace, heated to 515°C at a rate of 5°C / min under vacuum conditions and kept at this temperature for 8 hours, then cooled to 200°C in the furnace, and then air-cooled to room temperature.
[0047] Example 7
[0048] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0049] 1) Place the PCD surface processed polycrystalline diamond composite blade into a box-type cold treatment furnace and cool it down to -160°C at a rate of 8°C / min for 8 hours, then heat it up to 150°C at a rate of 4°C / min, and then take it out of the furnace and air cool it to room temperature;
[0050] 2) placing the polycrystalline diamond composite blade cooled in step 1) into a vacuum heat treatment furnace, heating to 550°C at a rate of 6°C / min under vacuum conditions and keeping the temperature for 6 hours, then cooling to 250°C in the furnace, and then air cooling to room temperature.
[0051] Example 8
[0052] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0053] 1) Place the PCD surface processed polycrystalline diamond composite blade into a box-type cold treatment furnace and cool it to -190°C at a rate of 12°C / min for 4 hours, then heat it to 120°C at a rate of 2°C / min, and then take it out of the furnace and air cool it to room temperature;
[0054] 2) placing the polycrystalline diamond composite blade cooled in step 1) into a vacuum heat treatment furnace, heating to 480°C at a rate of 4°C / min under vacuum conditions and keeping the temperature for 10 hours, then cooling to 300°C in the furnace, and then air cooling to room temperature.
[0055] Example 9
[0056] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0057] 1) Place the PCD surface machined polycrystalline diamond composite blade into a box-type cold treatment furnace and cool it down to -200°C at a rate of 15°C / min for 3 hours, then heat it up to 160°C at a rate of 6°C / min, and then take it out of the furnace and air cool it to room temperature;
[0058] 2) placing the polycrystalline diamond composite blade cooled in step 1) into a vacuum heat treatment furnace, heating it to 600°C at a rate of 6°C / min under vacuum conditions and keeping it at that temperature for 4 hours, then cooling it to 300°C in the furnace, and then air cooling it to room temperature.
[0059] Example 10
[0060] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0061] 1) Place the PCD surface processed polycrystalline diamond composite blade into a box-type cold treatment furnace and cool it to -140°C at a rate of 4°C / min for 8 hours, then heat it to 100°C at a rate of 8°C / min, and then take it out of the furnace and air cool it to room temperature;
[0062] 2) placing the polycrystalline diamond composite blade cooled in step 1) into a vacuum heat treatment furnace, heating to 400°C at a rate of 8°C / min under vacuum conditions and keeping the temperature for 15 hours, then cooling to 250°C in the furnace, and then air cooling to room temperature.
[0063] Embodiment 11
[0064] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0065] 1) Place the PCD surface processed polycrystalline diamond composite blade into a vacuum heat treatment furnace, heat it to 515°C at a rate of 3°C / min under vacuum conditions and keep it for 8 hours, then cool it to 200°C with the furnace, and then air cool it to room temperature;
[0066] 2) The polycrystalline diamond composite blade cooled in step 1) is flat-ground and placed in a vacuum heat treatment furnace, heated to 660°C at a rate of 3°C / min under vacuum conditions and kept warm for 1 hour, then cooled to 200°C in the furnace, and then air-cooled to room temperature.
[0067] Example 12
[0068] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0069] 1) Put the PCD surface processed polycrystalline diamond composite blade into a vacuum heat treatment furnace, heat it to 480℃ at a rate of 2℃ / min under vacuum conditions, keep it at that temperature for 10h, then cool it to 250℃ with the furnace, and then air cool it to room temperature;
[0070] 2) The polycrystalline diamond composite blade cooled in step 1) is flat-ground and placed in a vacuum heat treatment furnace, heated to 690°C at a rate of 4°C / min under vacuum conditions for 0.5 h, then cooled to 250°C in the furnace, and then air-cooled to room temperature.
[0071] Example 13
[0072] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0073] 1) Put the PCD surface processed polycrystalline diamond composite blade into a vacuum heat treatment furnace, heat it to 550℃ at a rate of 8℃ / min under vacuum conditions and keep it for 6h, then cool it to 300℃ with the furnace, and then air cool it to room temperature;
[0074] 2) The polycrystalline diamond composite blade cooled in step 1) is flat-ground and placed in a vacuum heat treatment furnace, heated to 690°C at a rate of 8°C / min under vacuum conditions and kept warm for 1.5 hours, then cooled to 300°C in the furnace, and then air-cooled to room temperature.
[0075] Embodiment 14
[0076] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0077] 1) Put the PCD surface processed polycrystalline diamond composite blade into a vacuum heat treatment furnace, heat it to 600℃ at a rate of 10℃ / min under vacuum conditions and keep it for 4h, then cool it to 250℃ with the furnace, and then air cool it to room temperature;
[0078] 2) The polycrystalline diamond composite blade cooled in step 1) is flat-ground and placed in a vacuum heat treatment furnace, heated to 800°C at a rate of 10°C / min under vacuum conditions and kept at that temperature for 0.5h, then cooled to 250°C in the furnace, and then air-cooled to room temperature.
[0079] Embodiment 15
[0080] The processing method of the polycrystalline diamond composite blade of this embodiment comprises the following steps:
[0081] 1) Place the PCD surface processed polycrystalline diamond composite blade into a vacuum heat treatment furnace, heat it to 400°C at a rate of 4°C / min under vacuum conditions, keep it warm for 15 hours, then cool it to 200°C with the furnace, and then air cool it to room temperature;
[0082] 2) The polycrystalline diamond composite blade cooled in step 1) is flat-ground and placed in a vacuum heat treatment furnace, heated to 500°C at a rate of 12°C / min under vacuum conditions and kept at that temperature for 3 hours, then cooled to 200°C in the furnace, and then air-cooled to room temperature.
[0083] Example 16
[0084] The polycrystalline diamond composite blade of this embodiment adopts a Ni-Cr-Co based cemented carbide substrate, and the processing method of the polycrystalline diamond composite blade comprises the following steps:
[0085] 1) Place the PCD surface machined polycrystalline diamond composite blade into a box-type cold treatment furnace and cool it down to -190°C at a rate of 10°C / min for 4 hours, then heat it up to 120°C at a rate of 5°C / min, and then take it out of the furnace and air cool it to room temperature;
[0086] 2) placing the polycrystalline diamond composite blade cooled in step 1) into a vacuum heat treatment furnace, heating to 480°C at a rate of 5°C / min under vacuum conditions and keeping the temperature for 10 hours, then cooling to 300°C in the furnace, and then air cooling to room temperature.
[0087] Comparative Example
[0088] The processing method of the polycrystalline diamond composite blade of this comparative example is different from that of Example 1 only in that the temperature of this comparative example is raised to 250°C at a rate of 3°C / min under vacuum conditions and kept at this temperature for 10 minutes, then cooled to 200°C in the furnace, and then air-cooled to room temperature.
[0089] Experimental example
[0090] The polycrystalline diamond composite blades after sintering were treated by the treatment methods of Examples 1 to 16. After processing, the PCD composite blade is flat-ground to detect the range of the camber of the PCD composite blade. The camber of the PCD composite blade is detected using a dial indicator. During the detection, the PCD composite blade is placed on the dial indicator detection device (PCD side facing up), the center position of the blade is aligned with the dial indicator probe, and then the dial indicator value is reset to zero, and the blade position is moved to Figure 4 6 different positions are shown, and the value shown by the dial indicator is recorded at each position (the detection process is as follows Figure 5 The test result range and average value of six positions of the samples of each embodiment are shown in Table 1.
[0091] The scanning electron microscope microscopic morphology of the polycrystalline diamond composite blade (diameter 58 mm) after treatment in the above Examples 1, 6, and 11 is shown in FIG. Figures 1 to 3 ,Depend on Figures 1 to 3 It can be seen that metal elements such as W and Co are evenly distributed at the diamond grain boundaries, the diamond particles are uniform in size and relatively round, and the DD bonds between the diamond particles are complete and firm.
[0092] Table 1 Camber test results
[0093]
[0094]
[0095] It can be seen from the data in Table 1 that the polycrystalline diamond composite blade treated by the treatment method of the present invention meets the use requirements after various performance tests.
Claims
1. A method for processing a polycrystalline diamond composite blade, Features: The following steps are involved: The polycrystalline diamond composite blade is subjected to heat treatment; the heat treatment method comprises the following steps: the polycrystalline diamond composite blade is subjected to a first heat preservation treatment in an oxygen-free environment, and then cooled; The temperature of the first heat preservation treatment is 350-750° C., and the time is 3-15 hours.
2. The method for processing a polycrystalline diamond composite blade according to claim 1, Features: The temperature of the first heat preservation treatment is 400-600° C., and the time is 4-12 hours.
3. The method for processing a polycrystalline diamond composite blade according to claim 1, Features: The rate of heating to the temperature of the first insulation treatment is ≤10°C / min.
4. The method for processing a polycrystalline diamond composite blade according to claim 1, Features: The heat treatment method further comprises the following steps: subjecting the cooled polycrystalline diamond composite blade to a second heat preservation treatment in an oxygen-free environment and cooling the blade; the temperature of the second heat preservation treatment is 500-800° C. and the time is 0.5-3 hours.
5. The method for processing a polycrystalline diamond composite blade according to claim 4, Features: The temperature of the second heat preservation treatment is 580-720° C., and the time is 0.6-2.5 h.
6. The method for processing a polycrystalline diamond composite blade according to claim 4, Features: The rate of heating to the temperature of the second insulation treatment is ≤12°C / min.
7. The method for processing a polycrystalline diamond composite blade according to any one of claims 4 to 6, Features: After the second heat preservation treatment, the steel is first cooled in the furnace to 200-300°C and then air-cooled out of the furnace.
8. The method for processing a polycrystalline diamond composite blade according to any one of claims 1 to 6, Features: Before the polycrystalline diamond composite blade is subjected to heat treatment, the polycrystalline diamond composite blade is first subjected to cold preservation treatment at -200 to -140°C.
9. The method for processing a polycrystalline diamond composite blade according to claim 8, Features: The temperature of the cold preservation treatment is -190 to -150°C, and the time is 3 to 8 hours.
10. The method for processing a polycrystalline diamond composite blade according to claim 8, Features: The rate of cooling to the cold treatment temperature is ≤15℃ / min.
11. The method for processing a polycrystalline diamond composite blade according to any one of claims 1 to 6, Features: The polycrystalline diamond composite blade is made of diamond powder and cemented carbide; the bonding metal of the cemented carbide contains Co.
12. The method for processing a polycrystalline diamond composite blade according to any one of claims 1 to 6, Features: After the first heat preservation treatment, the steel is first cooled in the furnace to 200-300°C and then air-cooled out of the furnace.