Austenitic stainless steel cold-rolled sheet with high cold formability and production method thereof
By rationally designing the composition and process of austenitic stainless steel cold-rolled plates, the problems of prone to cracking and unstable tissue performance of traditional austenitic stainless steel cold-rolled plates are solved, and high-cold moldability and stable tissue performance are achieved to meet the thin films Processing requirements for low-temperature storage tanks.
Patent Information
- Application Number
- CN202411417367.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-11
AI Technical Summary
Traditional austenitic stainless steel cold-rolled plates are prone to cracking during the forming process, and the structural performance after forming is unstable, and the production process control is difficult, making it difficult to achieve a good match between cold forming, hot workability and service performance.
By rationally designing the components of austenitic stainless steel cold-rolled plates, including the content of elements such as C, Si, Mn, Cr, Ni, N, Cu, Mo, etc., and controlling the cold rolling and heat treatment processes to ensure grain size and deformation texture. The stability of the cold forming performance is improved.
It significantly improves the cold forming performance of the cold rolled plate and the stability of the tissue performance after forming, meets the processing requirements of thin-film-type low-temperature storage tanks, reduces cracking rate, and ensures the hot workability and corrosion resistance of the material.
Smart Images

Figure CN119020695A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of stainless steel production and processing, and particularly relates to a high cold formability austenitic stainless steel cold-rolled plate and a production method thereof. Background Art
[0002] Traditional fossil energy has played an indispensable role in promoting the development of the world economy, but it has also caused increasingly severe environmental pollution problems. In response to global climate deterioration and sustainable development issues, the research, development and utilization of new energy sources have rapidly heated up around the world, and countries have accelerated the popularization of green and low-carbon energy technologies. Compared with traditional fossil energy, natural gas and hydrogen energy have the technical advantages of clean, efficient and sustainable utilization, and are an important path to achieve the "dual carbon" goal.
[0003] In the natural gas and hydrogen energy industry chain, storage and transportation are the most critical links, and among all storage and transportation methods, low-temperature liquefied gas storage and transportation is the most efficient method. The future advanced storage and transportation direction of LNG and liquid hydrogen storage tanks is membrane tanks, and the inner layer of this type of tank needs to use austenitic stainless steel cold-rolled plates after complex forming processing. Due to the complex process of cold-rolled plate forming, multiple pressing passes, and large and frequent deformation in the forming area, stainless steel is required to have excellent deformation ability, and the deformation area requires stainless steel to have excellent metal fluidity.
[0004] Austenitic stainless steel cold-rolled sheets with traditional components and processes have the following problems in product design, production, preparation, and forming:
[0005] (1) The composition design is unreasonable, making it difficult to achieve a good match between the product's cold formability, hot workability, and service performance. The forming process is prone to cracking, and the structure and performance of the formed steel plate are unstable during use;
[0006] (2) The production process is difficult to control, and it is difficult to accurately control microstructures such as grain size and deformation texture, and the product formability is unstable. Summary of the invention
[0007] In order to solve all or part of the above problems, the purpose of the present invention is to provide a high cold formability austenitic stainless steel cold-rolled plate and a production method thereof, by rationally designing the composition of the cold-rolled plate and controlling the key process points of the cold rolling, heat treatment and other processes, so as to effectively improve the cold forming performance of the cold-rolled plate and ensure the stability of the organizational performance of the cold-rolled plate after forming.
[0008] In the first aspect, the present invention provides a high cold formability austenitic stainless steel cold-rolled plate, the composition of the high cold formability austenitic stainless steel cold-rolled plate includes, by mass percentage: C: 0.035-0.045%, Si: 0.25-0.3%, Mn: 2-3%, Cr: 14-14.5%, Ni: 9-9.5%, N: 0.17-0.20%, Cu: 1.3-1.6%, Mo: 0.5-0.7%, and the rest is Fe and unavoidable impurity elements.
[0009] Optionally, the microstructure properties of the high cold formability austenitic stainless steel cold-rolled sheet are:
[0010] Grain size 8-9;
[0011] Grain size range <2 level;
[0012] Full austenite structure, no precipitation phase.
[0013] Optionally, the room temperature mechanical properties of the high cold formability austenitic stainless steel cold-rolled sheet are:
[0014] Tensile strength R m : 535~565MPa;
[0015] Yield Strength R p2.0 : 220~250MPa;
[0016] Elongation A≥50%.
[0017] In a second aspect, the present invention provides a method for producing a high cold formability austenitic stainless steel cold-rolled sheet, comprising the following steps:
[0018] S1, obtaining a continuous casting billet through smelting, refining and slab continuous casting;
[0019] S2, cold rolling the continuous casting slab to obtain a strip;
[0020] S3, heat treating the strip to obtain a steel strip;
[0021] S4, the steel strip is coiled by a coiler.
[0022] Optionally, in S2, during the cold rolling of the continuous casting billet, the deformation amount of the first pass is controlled to be 30-35%, the deformation amount of the last pass is controlled to be 5-6%, and the total deformation amount is controlled to be 75-80% to ensure that the grains of the steel plate are fully broken.
[0023] Optionally, in S3, heat treating the strip includes:
[0024] In the first stage, the strip temperature is controlled at 920-940°C and the holding time is 9-10min / mm;
[0025] In the second stage, the strip temperature is controlled at 1050-1070°C and the holding time is 4-5min / mm;
[0026] In the third stage, the strip temperature is controlled at 1150-1170°C and the holding time is 0.5-1min / mm;
[0027] In the fourth stage, the strip temperature is controlled at 1100-1120°C and the holding time is 1-2 min / mm.
[0028] It can be seen from the above technical scheme that the high cold formability austenitic stainless steel cold-rolled sheet and the production method thereof provided by the present invention have the following advantages:
[0029] By rationally designing the composition of the cold-rolled sheet and controlling the key process points of the cold rolling, heat treatment and other processes, the cold forming performance of the cold-rolled sheet can be effectively improved, ensuring the stability of the organizational performance of the cold-rolled sheet after forming.
[0030] Other features and advantages of the present invention will be set forth in the description which follows. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings are used to provide a further understanding of the technical solution of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the technical solution of the present invention and do not constitute a limitation on the technical solution of the present invention.
[0032] Figure 1 The flowchart of the production method of austenitic stainless steel cold-rolled sheet with high cold formability in an embodiment of the present invention. DETAILED DESCRIPTION
[0033] To make the purpose, technical solution and advantages of the present invention more clear, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other arbitrarily without conflict.
[0034] like Figure 1 An embodiment of the present invention is shown, in which a high cold formability austenitic stainless steel cold-rolled plate is disclosed. The composition of the high cold formability austenitic stainless steel cold-rolled plate includes, by mass percentage: C: 0.035-0.045%, Si: 0.25-0.3%, Mn: 2-3%, Cr: 14-14.5%, Ni: 9-9.5%, N: 0.17-0.20%, Cu: 1.3-1.6%, Mo: 0.5-0.7%, and the rest are Fe and unavoidable impurity elements.
[0035] The reasons for limiting the chemical elements in this embodiment are as follows:
[0036] It has been found in practice that C is an austenite stabilizing element. Properly increasing the C content can improve the stability of the cold forming process and prevent processing cracking caused by martensitic phase transformation. 23 C6 carbide affects the corrosion resistance of the material, therefore, the C content is limited to 0.035-0.045%.
[0037] It has been found in practice that Si is added as a deoxidizer in smelting, but too high Si content will reduce the stability of the austenite structure during the processing process. Therefore, the Si content is limited to 0.25-0.3%.
[0038] It has been found in practice that the main function of Mn is to stabilize the austenite phase and to increase the solubility of N in steel. However, if the amount of Mn added is too large, MnS inclusions are easily formed, which seriously affects the processing performance of the product. Therefore, the Mn content is limited to 2-3%.
[0039] It has been found in practice that Cr is the most important alloying element for forming a stainless steel passivation film. In order to improve the stability of the structure, the Cr content is appropriately reduced. Therefore, the Cr content is limited to 14-14.5%.
[0040] It has been found in practice that Ni is the main element for improving the stability of austenite in stainless steel, but excessive addition of Ni will lead to excessively high costs. Therefore, the Ni content is limited to 9-9.5%.
[0041] It has been found in practice that N is an element that stabilizes austenite, inhibits the generation of intermetallic phases, and can also improve low-temperature strength and pitting resistance. In this application, N is increased to more than 0.17%, but excessive N will reduce toughness, so the N content is limited to 0.17-0.20%.
[0042] It has been found in practice that the Cu element can reduce the cold hardening tendency of austenitic stainless steel, improve the deep drawing performance and forming performance of stainless steel, and also improve the corrosion resistance in reducing media. In this application, more than 1.3% Cu is added, but too high a Cu content will seriously reduce the hot working performance of the material, so the Cu content is limited to 1.3-1.6%.
[0043] It has been found in practice that Mo can improve the pitting corrosion resistance. In order to compensate for the loss of corrosion resistance caused by the reduction of Cr content, 0.5-0.7% Mo is added to the steel of the present invention.
[0044] In this embodiment, the microstructure properties of the high cold formability austenitic stainless steel cold rolled sheet are: grain size 8-9, grain size range <2, full austenite structure, no precipitation phase. The room temperature mechanical properties of the high cold formability austenitic stainless steel cold rolled sheet are: tensile strength R m : 535~565MPa, yield strength R p2.0: 220~250MPa, elongation A≥50%.
[0045] like Figure 1 The embodiment of the present invention is shown in the figure. The embodiment also discloses a method for producing a high cold formability austenitic stainless steel cold-rolled sheet, comprising the following steps:
[0046] S1, obtaining a continuous casting billet through smelting, refining and slab continuous casting;
[0047] S2, cold rolling the continuous casting slab to obtain a strip;
[0048] S3, heat treating the strip to obtain a steel strip;
[0049] S4, the steel strip is coiled by a coiler.
[0050] In S2, during the cold rolling of the continuous casting billet, the deformation amount of the first pass is controlled to be 30-35%, the deformation amount of the last pass is controlled to be 5-6%, and the total deformation amount is controlled to be 75-80% to ensure that the grains of the steel plate are fully broken.
[0051] In S3, the strip is heat treated including:
[0052] In the first stage, the strip temperature is controlled at 920-940°C and the holding time is 9-10min / mm;
[0053] In the second stage, the strip temperature is controlled at 1050-1070°C and the holding time is 4-5min / mm;
[0054] In the third stage, the strip temperature is controlled at 1150-1170°C and the holding time is 0.5-1min / mm;
[0055] In the fourth stage, the strip temperature is controlled at 1100-1120°C and the holding time is 1-2 min / mm.
[0056] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the embodiments. The experimental methods without specific conditions in the following examples can be carried out according to conventional methods and conditions.
[0057] Example 1: Finished product specification is 1.2*1219mm cold roll
[0058] The deformation of the first cold rolling pass is 33%, the deformation of the last cold rolling pass is 5.5%, and the total deformation is 78%.
[0059] The first stage of heat treatment: steel plate temperature 930°C, holding time 9.5min / mm.
[0060] The second stage of heat treatment: steel plate temperature 1050°C, holding time 4.5min / mm.
[0061] The third stage of heat treatment: steel plate temperature 1160°C, holding time 0.7min / mm.
[0062] The fourth stage of heat treatment: steel plate temperature 1100°C, holding time 1.5min / mm.
[0063] Example 2: Finished product specification is 1.2*1250mm cold roll
[0064] The deformation of the first cold rolling pass is 32%, the deformation of the last cold rolling pass is 6%, and the total deformation is 75%.
[0065] The first stage of heat treatment: steel plate temperature 920℃, holding time 10min / mm.
[0066] The second stage of heat treatment: steel plate temperature 1060°C, holding time 4.5min / mm.
[0067] The third stage of heat treatment: steel plate temperature 1150°C, holding time 1min / mm.
[0068] The fourth stage of heat treatment: steel plate temperature 1120℃, holding time 1min / mm.
[0069] Example 3: Finished product specification is 1.2*1300mm cold roll
[0070] The first cold rolling deformation is 35%, the last cold rolling deformation is 6%, and the total deformation is 80%. The first stage of heat treatment: the steel plate temperature is 940℃, and the holding time is 9min / mm.
[0071] The second stage of heat treatment: steel plate temperature 1060℃, holding time 5min / mm.
[0072] The third stage of heat treatment: steel plate temperature 1160°C, holding time 0.8min / mm.
[0073] The fourth stage of heat treatment: steel plate temperature 1110°C, holding time 1.5min / mm.
[0074] Example 4: Finished product specification is 1.2*1800mm cold roll
[0075] The first cold rolling deformation is 33%, the last cold rolling deformation is 5%, and the total deformation is 78%. The first stage of heat treatment: steel plate temperature is 930℃, and the holding time is 10min / mm;
[0076] The second stage of heat treatment: steel plate temperature 1070℃, holding time 4min / mm;
[0077] The third stage of heat treatment: steel plate temperature 1170℃, holding time 0.5min / mm;
[0078] The fourth stage of heat treatment: steel plate temperature 1110°C, holding time 1min / mm.
[0079] Example 5: Finished product specification is 1.2*1500mm cold roll
[0080] The first cold rolling deformation is 32%, the last cold rolling deformation is 6%, and the total deformation is 75%. The first stage of heat treatment: the steel plate temperature is 940℃, and the holding time is 9min / mm.
[0081] The second stage of heat treatment: steel plate temperature 1050℃, holding time 5min / mm;
[0082] The third stage of heat treatment: steel plate temperature 1160°C, holding time 0.8min / mm.
[0083] The fourth stage of heat treatment: steel plate temperature 1120℃, holding time 1min / mm.
[0084] Comparative example: finished product specification is 1.2*1500mm cold roll
[0085] The first cold rolling deformation is 20%, the last cold rolling deformation is 10%, and the total deformation is 65%. Heat treatment stage: steel plate temperature is 1080℃, and the holding time is 6min / mm.
[0086] The chemical composition and failure rate of the examples and comparative examples are shown in Tables 1 and 2:
[0087] Table 1 lists the chemical compositions of the examples and comparative examples (weight percentage)
[0088] C Si Mn Cr Ni N Fe Example 1 0.035 0.25 2.0 14.0 9.0 0.17 margin Example 2 0.037 0.27 2.2 14.3 9.2 0.18 margin Example 3 0.045 0.30 2.5 14.5 9.1 0.20 margin Example 4 0.040 0.28 2.8 14.2 9.3 0.17 margin Example 5 0.042 0.26 2.7 14.1 9.5 0.20 margin Comparative Example 0.020 0.25 1.1 17.3 8.3 0.06 margin
[0089] Table 2 shows the defective rate of the examples and comparative examples
[0090]
[0091] It can be seen from Tables 1 and 2 that the cold formability of austenitic stainless steel cold-rolled sheets is greatly improved, which can meet the processing requirements of thin-film type low-temperature storage tanks, and the proportion of cracking or unusability after cold forming is controlled below 1%.
[0092] From the above, we can see that by designing an excellent alloy composition system and controlling the content of key elements, the basic cold formability of the material can be guaranteed while also ensuring the hot workability and corrosion resistance of the material. In addition, by matching and optimizing the cold rolling and heat treatment processes, the cold formability can be improved by precisely controlling the microstructures such as grain size and deformation texture.
[0093] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in the present invention should have the common meanings understood by those skilled in the art to which the present invention belongs.
[0094] In addition, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. In the description of the present invention, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention. In particular, as long as there is no structural conflict, the various technical features mentioned in each embodiment can be combined in any way. The present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A high cold formability austenitic stainless steel cold-rolled sheet, characterized in that: The composition of the high cold formability austenitic stainless steel cold-rolled sheet includes, by mass percentage, C: 0.035-0.045%, Si: 0.25-0.3%, Mn: 2-3%, Cr: 14-14.5%, Ni: 9-9.5%, N: 0.17-0.20%, Cu: 1.3-1.6%, Mo: 0.5-0.7%, and the rest is Fe and unavoidable impurity elements.
2. The high cold formability austenitic stainless steel cold-rolled sheet according to claim 1, characterized in that: The microstructure properties of the high cold formability austenitic stainless steel cold-rolled sheet are: Grain size 8-9; Grain size range <2 level; Full austenite structure, no precipitation phase.
3. The high cold formability austenitic stainless steel cold-rolled sheet according to claim 2, characterized in that: The room temperature mechanical properties of the high cold formability austenitic stainless steel cold rolled sheet are: Tensile strength R m : 535~565MPa; Yield Strength R p2.0 : 220~250MPa; Elongation A≥50%.
4. A method for producing austenitic stainless steel cold-rolled sheet with high cold formability according to any one of claims 1 to 3, characterized in that: The steps include: S1, obtaining a continuous casting billet through smelting, refining and slab continuous casting; S2, cold rolling the continuous casting slab to obtain a strip; S3, heat treating the strip to obtain a steel strip; S4, the steel strip is coiled by a coiler.
5. The method for producing austenitic stainless steel cold-rolled sheet with high cold formability according to claim 4, characterized in that: In S2, during the cold rolling of the continuous casting billet, the deformation amount of the first pass is controlled to be 30-35%, the deformation amount of the last pass is controlled to be 5-6%, and the total deformation amount is controlled to be 75-80% to ensure that the grains of the steel plate are fully broken.
6. The method for producing austenitic stainless steel cold-rolled sheet with high cold formability according to claim 4, characterized in that: In S3, the strip is heat treated including: In the first stage, the strip temperature is controlled at 920-940°C and the holding time is 9-10min / mm; In the second stage, the strip temperature is controlled at 1050-1070°C and the holding time is 4-5min / mm; In the third stage, the strip temperature is controlled at 1150-1170°C and the holding time is 0.5-1min / mm; In the fourth stage, the strip temperature is controlled at 1100-1120°C and the holding time is 1-2 min / mm.
Citation Information
Patent Citations
Austenitic stainless steel sheet and method for producing same
CN105452505A
Austenitic stainless-steel sheet and process for producing high-elastic-limit nonmagnetic steel material therefrom
CN108754333A
Austenitic stainless steel and preparation method thereof
CN111270147A
Critical solid solution, critical cooling aging and annealing heat treatment method
CN112779394A
Preparation method of austenitic stainless steel band for deep drawing
CN115354129A