Method for rapidly detonating tempered glass containing nickel sulfide impurities
Through microwave irradiation technology, the detonation treatment of tempered glass containing nickel sulfide is solved, and the problems of low processing efficiency, high energy consumption and safety hazards in the existing technology are achieved, and the rapid and safe tempered glass treatment is achieved, which improves the application safety and Processing efficiency.
Patent Information
- Application Number
- CN202411510354.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, tempered glass has low processing efficiency, high energy consumption and high cost, and it is difficult to effectively avoid the risk of self-destruction, especially in high-rise buildings.
The microwave irradiation technology is used to detonate tempered glass containing nickel sulfide. The microwave irradiation frequency is 0.915-2.45GHz and the microwave generation power is 0.5-1000kW, achieving rapid and selective detonation of tempered glass containing nickel sulfide impurities.
It improves the safety of tempered glass, realizes rapid, automated and continuous processing, saves energy, and reduces energy consumption and costs.
Smart Images

Figure CN119023943A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of quality and safety application of tempered glass, and in particular to a method for quickly detonating tempered glass containing nickel sulfide impurities. Background Art
[0002] Tempered glass is widely used in the fields of construction, transportation, and household appliances. During the application process, the self-explosion of tempered glass is the most common and difficult to solve problem, especially if it occurs in high-rise buildings, it poses a serious safety hazard. Therefore, how to prevent the self-explosion of tempered glass has become a research hotspot and an important topic.
[0003] The main reason for tempered glass to explode is the presence of nickel sulfide impurities inside the glass. This is because nickel sulfide undergoes phase change and volume expansion, which creates a large extrusion stress on the tempered glass. Based on the current flat glass production technology, it is difficult to completely prevent nickel sulfide impurities from being mixed into the glass. If flat glass containing nickel sulfide impurities is selected for tempering, the tempered glass produced will be at risk of self-explosion during subsequent use.
[0004] At present, there are two main ways to prevent tempered glass from self-explosion: the first is to detect whether the tempered glass contains nickel sulfide impurities before use, and to prevent the further use of tempered glass containing nickel sulfide impurities; the second is to detonate tempered glass with self-explosion risks before use. The common method of early detonation is the homogenization furnace detonation treatment.
[0005] CN101852769A discloses a method for detecting nickel sulfide in glass. The method comprises: setting a strong magnetizing device in the advancing direction of the glass conveyor belt; when the glass passes through the magnetizing device, the nickel sulfide in the glass will be magnetized; when the glass passes through the magnetizing device and moves along the conveyor belt, it will be detected by a magnetic detection device arranged above the conveyor belt. This method is difficult to detect nickel sulfide with small particle size inside tempered glass, and there are no relevant application cases in the market.
[0006] CN108328913A discloses a tempered glass homogenization method, which comprises: S1: providing a glass sheet, cutting, edge grinding and tempering the glass sheet; S2: providing a homogenization furnace, placing the glass sheet in the homogenization furnace for homogenization, wherein the homogenization consists of a heating stage, a constant temperature stage and a cooling stage; S3: setting the heating rate of the heating stage to 1.5°C / s to 4°C / s, setting the temperature of the constant temperature stage to be maintained at 240°C to 300°C, setting the duration of the constant temperature stage to 1.5h to 2.5h, and setting the cooling rate of the cooling stage to 0.02°C / s to 0.04°C / s; S4: removing the glass sheet cooled to 60°C to 70°C from the homogenization furnace and continuing to cool to room temperature. This method takes about 8 hours from the entire process of tempered glass entering the furnace - heating - heat preservation - cooling - exiting the furnace, and has low processing efficiency, high energy consumption and high cost. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of low processing efficiency, poor processing effect, high processing energy consumption and high cost in the prior art.
[0008] In order to achieve the above object, a first aspect of the present invention provides a method for rapidly detonating tempered glass containing nickel sulfide impurities, the method comprising: detonating the tempered glass containing nickel sulfide under microwave irradiation; The conditions for the detonation treatment at least meet the following requirements: microwave irradiation frequency is 0.915-2.45 GHz, and microwave generation power is 0.5-1000 kW.
[0009] The method for rapidly detonating tempered glass containing nickel sulfide impurities provided by the present invention also has at least the following beneficial effects: (1) The method provided by the present invention can selectively detonate tempered glass containing nickel sulfide, effectively detonate tempered glass with a risk of self-explosion, eliminate tempered glass with a high risk of self-explosion, and improve the safe application of tempered glass; (2) The method provided by the present invention can realize the rapid detonation of tempered glass containing nickel sulfide. The method has the characteristics of energy saving and high processing efficiency, and can realize automated and continuous processing.
[0010] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 It is a schematic diagram of the structure of the microwave irradiation detonation device in Embodiments 1 to 8 of the present invention; Figure 2 It is a schematic diagram of the structure of the microwave irradiation detonation device in Example 9 of the present invention.
[0012] Description of reference numerals: . DETAILED DESCRIPTION
[0013] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0014] As mentioned above, the first aspect of the present invention provides a method for rapidly detonating tempered glass containing nickel sulfide impurities, the method comprising: detonating the tempered glass containing nickel sulfide under microwave irradiation; The conditions for the detonation treatment at least meet the following requirements: microwave irradiation frequency is 0.915-2.45 GHz, and microwave generation power is 0.5-1000 kW.
[0015] Preferably, the average particle diameter of the nickel sulfide is greater than 0.1 mm.
[0016] Preferably, the distance between the nickel sulfide and the upper surface of the tempered glass is 2-3 mm.
[0017] In the present invention, there is no special requirement for the source of the tempered glass, which can be obtained from commercial sources or prepared by determining a suitable synthesis route by combining the present invention with the known knowledge in the prior art. The present invention will not be described in detail here, and those skilled in the art should not be construed as limiting the present invention.
[0018] According to a preferred specific implementation manner, the tempered glass is prepared by the following method: drilling a hole on ordinary flat glass to obtain a hole, then placing nickel sulfide into the hole, filling the hole with glass powder obtained during the drilling, transferring the hole to a mold, and placing the mold in a high-temperature furnace for sequential melting treatment and annealing treatment, and then further reducing the temperature to room temperature to obtain flat glass containing nickel sulfide impurities; and tempering the flat glass to obtain the tempered glass; the tempered glass has a length of 200-300 mm, a width of 200-300 mm, and a thickness of 5-6 mm.
[0019] Preferably, the ordinary flat glass has a length of 200-400 mm, a width of 200-400 mm, and a thickness of 5-8 mm.
[0020] Further preferably, the diameter of the hole is 2-4 mm.
[0021] Preferably, the average particle diameter of the nickel sulfide is 0.1-0.3 mm.
[0022] Preferably, the mold has a length of 300-310 mm, a width of 300-310 mm, and a depth of 6-10 mm.
[0023] More preferably, the conditions of the melting treatment at least meet the following requirements: temperature of 1000-1200° C., heating rate of 1.5-2° C. / s, and time of 30-60 min.
[0024] Preferably, the annealing treatment conditions at least meet the following requirements: temperature of 500-600° C. and time of 2-4 h.
[0025] Further preferably, the tempering treatment conditions at least meet the following requirements: temperature of 600-700° C. and time of 30-60 s.
[0026] Preferably, the detonation process is carried out in a microwave irradiation detonation device; the microwave irradiation detonation device comprises: A box body, wherein a transmission device for conveying the tempered glass is disposed at the bottom of the box body, and a window for the tempered glass to enter and exit is also disposed on the side of the box body; A microwave generating component is arranged inside the box and is used for emitting microwaves that can promote the phase change and expansion of nickel sulfide.
[0027] In the present invention, there is no special requirement for the size of the microwave irradiation and detonation device, which only needs to be able to accommodate the tempered glass. Exemplarily, the microwave irradiation and detonation device has a length of 1.5-15m, a width of 1-2.5m, and a height of 0.5-1.5m. Those skilled in the art should not understand this as a limitation to the present invention.
[0028] In the present invention, there is no special requirement for the type of the microwave irradiation and detonation device. Exemplarily, the microwave irradiation and detonation device is a microwave oven, which should not be construed as a limitation to the present invention by those skilled in the art.
[0029] The present invention has no special requirements for the type of the transmission device, which only needs to transport the tempered glass to the microwave irradiation and detonation device. Exemplarily, the transmission device is a conveyor belt, which should not be construed as a limitation to the present invention by those skilled in the art.
[0030] Preferably, the transmission speed of the transmission device is 0.5-1.5 m / min.
[0031] Preferably, after the tempered glass completely enters the microwave irradiation and detonation device, the speed of the transmission device is adjusted so that the transmission speed of the tempered glass is 0-1.5 m / min.
[0032] According to a preferred specific implementation manner, when the tempered glass completely enters the microwave irradiation and detonation device, the power supply for controlling the transmission device is turned off.
[0033] The present invention has no special requirements on the size and specific setting position of the window, it only needs to ensure that the tempered glass passes through. Exemplarily, the window is set in the middle position of the side of the box, that is, the distance between the top wall of the window and the top of the box is equal to the distance between the bottom wall of the window and the bottom of the box; the width of the window is 1-2.5m, and the height is 0.5-1.5m, wherein the width of the window refers to the length of the window extending along the width direction of the box, and the height of the window refers to the shortest distance between the top wall of the window and the bottom wall of the window.
[0034] The present invention has no particular limitation on the specific location of the microwave generating assembly, which should not be considered as a limitation to the present invention by those skilled in the art.
[0035] According to a preferred specific implementation manner, the microwave generating assembly is arranged on the top of the box body, and the distance between the center of the microwave generating assembly and the center of the transmission device is 0.3-1.2 m.
[0036] In the present invention, microwave irradiation frequency is an important technical feature. The inventors of the present invention have found that when the microwave irradiation frequency is 0.915-2.45 GHz, combined with other technical features of the present invention, the time required to detonate tempered glass is shorter and the energy consumption of the equipment is lower.
[0037] More preferably, the conditions for the detonation treatment at least meet: the microwave irradiation frequency is 0.915 or 2.45 GHz.
[0038] In the present invention, microwave power is an important technical feature. The inventors of the present invention have found that when the microwave power is 0.5-1000kW, combined with other technical features of the present invention, the time required to detonate tempered glass is shorter and the energy consumption of the equipment is lower.
[0039] Further preferably, the conditions for the detonation treatment at least meet: the microwave generating power is 0.5, 1, 20 or 1000 kW.
[0040] The following combination Figure 1A preferred specific embodiment of the method for detonating tempered glass containing nickel sulfide impurities provided by the present invention is described in detail, comprising: placing the tempered glass 2 horizontally on the transmission device 3, turning on the power supply for controlling the transmission device 3, and transporting the tempered glass 2 to the microwave irradiation and detonation device through the transmission device 3; when the tempered glass 2 completely enters the microwave irradiation and detonation device, turning off the power supply for controlling the transmission device 3, and then turning on the microwave generating component 1, and detonating the tempered glass 2 under microwave irradiation; the conditions for the detonation treatment at least meet the following conditions: the microwave irradiation frequency is 2.45 or 0.915 GHz, and the microwave generating power is 0.5, 1 or 1000 kW.
[0041] Further preferably, the transmission device 3 is a conveyor belt.
[0042] Preferably, the transport speed of the transmission device 3 is 0.5-1 m / min.
[0043] Preferably, the microwave irradiation and detonation device is a microwave oven, and the microwave oven has a length of 1.5 m, a width of 1 m, and a height of 0.5 m.
[0044] More preferably, in the microwave oven, a microwave generating assembly 1 is arranged on the top of the microwave oven, a conveyor belt 3 for conveying the tempered glass 2 is arranged on the bottom of the microwave oven, a window for the conveyor belt 3 and the tempered glass 2 to pass through is arranged on the side of the microwave oven, and the width of the window is 1m and the height is 0.5m; the distance between the center of the microwave generating assembly 1 and the center of the conveyor belt 3 is 0.3m.
[0045] The following combination Figure 2 A preferred embodiment of the method for detonating tempered glass containing nickel sulfide impurities provided by the present invention is described in detail, comprising: Each tempered glass in the tempered glass assembly 4 is placed horizontally on the transmission device 3 in sequence, and the power supply for controlling the transmission device 3 is turned on, and each tempered glass in the tempered glass assembly 4 is transported to the microwave irradiation and detonation device at a speed of 1.5 m / min through the transmission device 3, and the microwave generating component 1 is turned on at the same time, and the tempered glass assembly 4 is detonated under microwave irradiation; The conditions for the detonation treatment are as follows: the microwave irradiation frequency is 2.45 GHz and the microwave generation power is 20 kW.
[0046] Further preferably, the transmission device 3 is a conveyor belt.
[0047] Preferably, the microwave irradiation and detonation device is a microwave oven, and the length of the microwave oven is 15m, the width is 2.5m, and the height is 1.5m.
[0048] More preferably, in the microwave oven, a microwave generating assembly 1 is arranged on the top of the microwave oven, a conveyor belt 3 for conveying the tempered glass combination 4 is arranged on the bottom of the microwave oven, a window for the conveyor belt 3 and the tempered glass combination 4 to pass through is arranged on the side of the microwave oven, and the width of the window is 2.5m and the height is 1.5m; the distance between the center of the microwave generating assembly 1 and the center of the conveyor belt 3 is 1.2m.
[0049] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the raw materials described are all commercially available products.
[0050] Microwave irradiation detonation device: A microwave oven 1 is 1.5 m long, 1 m wide and 0.5 m high; a microwave generating assembly is disposed on the top of the microwave oven 1, a conveyor belt for conveying the tempered glass is disposed on the bottom of the microwave oven 1, a window for the conveyor belt and the tempered glass to pass through is disposed on the side of the microwave oven 1, the width of the window is 1 m and the height is 0.5 m; the distance between the center of the microwave generating assembly and the center of the conveyor belt is 0.3 m; Microwave oven II has a length of 15 m, a width of 2.5 m and a height of 1.5 m; a microwave generating assembly is arranged on the top of the microwave oven II, a conveyor belt for conveying the tempered glass is arranged on the bottom of the microwave oven II, a window for the conveyor belt and the tempered glass to pass through is arranged on the side of the microwave oven II, and the width of the window is 2.5 m and the height is 1.5 m; the distance between the center of the microwave generating assembly and the center of the conveyor belt is 1.2 m.
[0051] In the following examples, unless otherwise specified, tempered glass I, tempered glass II, tempered glass combination and tempered glass DI are obtained by the following method: Preparation of the tempered glass I: Use a glass drilling machine to drill a hole with a diameter of 3 mm on an ordinary flat glass with a length of 300 mm, a width of 300 mm and a thickness of 6 mm; Putting nickel sulfide with a particle diameter of 0.25 mm into the hole, filling the hole with glass powder obtained during drilling, and then transferring it to a graphite mold with a length of 305 mm, a width of 305 mm, and a depth of 10 mm, and placing it in a high-temperature furnace, heating it to 1200° C. at a rate of 1.5° C. / s, heating and melting it at this temperature for 30 minutes, then reducing the temperature to 550° C. and maintaining it at this temperature for 2 hours to fully anneal the glass, and then further reducing the temperature to room temperature to obtain a flat glass containing nickel sulfide impurities; The flat glass is placed in a tempering furnace for tempering treatment to obtain the tempered glass I; the tempered glass I has a length of 300 mm, a width of 300 mm, and a thickness of 6 mm; The tempering treatment conditions are as follows: temperature is 630°C and time is 30s; The surface stress of the tempered glass I obtained by using a tempered glass surface stress meter is 108 MPa; and the distance between the nickel sulfide impurity and the upper surface of the tempered glass I is 2.5 mm according to GB / T30020-2023.
[0052] Preparation of the tempered glass II: The method for preparing tempered glass I is followed, except that the diameter of the hole is 2 mm, and nickel sulfide particles with a diameter of 0.15 mm are placed in the hole. The remaining steps and parameters are the same as those for preparing tempered glass I; Using the same detection method as that of the tempered glass I, it was found that the surface stress of the tempered glass II was 108 MPa, and the distance between the nickel sulfide impurity and the upper surface of the tempered glass I was 2.6 mm.
[0053] The tempered glass combination is 500 pieces of tempered glass randomly selected from a certain project, and it is impossible to determine which tempered glass contains nickel sulfide impurities, and the length of each tempered glass in the tempered glass combination is 0.5-2m, the width is 0.5-2m, and the thickness is 5-8mm.
[0054] Preparation of the tempered DI glass: The preparation method of tempered glass I is followed, except that the tempered glass DI does not contain nickel sulfide impurities, and the remaining steps and parameters are the same as those of the preparation of tempered glass I.
[0055] Embodiment 1: This example is used to provide a method for quickly detonating tempered glass containing nickel sulfide impurities, and the method is Figure 1 The method is performed in the device shown, and comprises: The tempered glass 12 is horizontally placed on the conveyor belt 3, and the power supply for controlling the conveyor belt 3 is turned on, and the tempered glass 12 is transported to the microwave oven 1 at a speed of 0.5 m / min through the conveyor belt. When the tempered glass 12 completely enters the microwave oven 1, the power supply for controlling the conveyor belt 3 is turned off, and the microwave generating assembly 1 is turned on to perform an explosion treatment on the tempered glass 12 under microwave irradiation; The conditions for the detonation treatment are as follows: the microwave irradiation frequency is 2.45 GHz, and the microwave generation power is 0.5 kW; After 5 minutes of microwave irradiation, the tempered glass I2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurities.
[0056] Embodiment 2: In this example, the tempered glass containing nickel sulfide impurities is detonated according to the method of Example 1, except that the conditions for the detonation treatment meet the following conditions: the microwave irradiation frequency is 0.915 GHz, the microwave generation power is 0.5 kW, and the remaining steps and parameters are the same as those of Example 1; After 6.5 minutes of microwave irradiation, the tempered glass I 2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurities.
[0057] Embodiment 3: In this example, the tempered glass containing nickel sulfide impurities is detonated according to the method of Example 1, except that the conditions for the detonation treatment meet the following conditions: the microwave irradiation frequency is 2.45 GHz, the microwave generation power is 1 kW, and the remaining steps and parameters are the same as those of Example 1; After 3 minutes of microwave irradiation, the tempered glass I2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurities.
[0058] Embodiment 4: In this example, the tempered glass containing nickel sulfide impurities is detonated according to the method of Example 1, except that the conditions of the detonation treatment meet the following conditions: the microwave irradiation frequency is 0.915 GHz, the microwave generation power is 1000 kW, and the remaining steps and parameters are the same as those of Example 1; After 4.5 minutes of microwave irradiation, the tempered glass I2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurities.
[0059] Embodiment 5: This example is used to provide a method for quickly detonating tempered glass containing nickel sulfide impurities, and the method is Figure 1 The method is performed in the device shown, and comprises: Place the tempered glass II 2 horizontally on the conveyor belt 3, turn on the power supply for controlling the conveyor belt 3, and transport the tempered glass II 2 into the microwave oven I at a speed of 1 m / min through the conveyor belt 3. When the tempered glass II 2 completely enters the microwave oven I, turn off the power supply for controlling the conveyor belt 3, and then turn on the microwave generating assembly 1 to detonate the tempered glass II 2 under microwave irradiation; The conditions for the detonation treatment are as follows: the microwave irradiation frequency is 2.45 GHz, and the microwave generation power is 0.5 kW; After microwave irradiation for 6.5 minutes, the tempered glass II 2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurity.
[0060] Embodiment 6: In this example, the tempered glass containing nickel sulfide impurities was detonated according to the method of Example 5, except that the conditions for the detonation treatment met the following requirements: the microwave irradiation frequency was 0.915 GHz, the microwave generation power was 0.5 kW, and the remaining steps and parameters were the same as those of Example 5; After microwave irradiation for 8 minutes, the tempered glass II 2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurity.
[0061] Embodiment 7: In this example, the tempered glass containing nickel sulfide impurities was detonated according to the method of Example 5, except that the conditions for the detonation treatment were as follows: the microwave irradiation frequency was 2.45 GHz, the microwave generation power was 1 kW, and the remaining steps and parameters were the same as those of Example 5; After microwave irradiation for 4.5 minutes, the tempered glass II 2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurity.
[0062] Embodiment 8: In this example, the tempered glass containing nickel sulfide impurities was detonated according to the method of Example 5, except that the conditions for the detonation treatment were as follows: the microwave irradiation frequency was 0.915 GHz, the microwave generation power was 1 kW, and the remaining steps and parameters were the same as those of Example 5; After 6 minutes of microwave irradiation, the tempered glass II 2 burst. By observing and analyzing the cracking point of the glass where the bursting occurred, it was detected that nickel sulfide impurity components were contained near the bursting point, that is, the bursting point was the location of the nickel sulfide impurity.
[0063] Embodiment 9: This example is used to provide a method for quickly detonating tempered glass containing nickel sulfide impurities, and the method is Figure 2 The method is performed in the device shown, and comprises: Each tempered glass in the tempered glass assembly 4 is placed horizontally on the conveyor belt 3 in sequence, and the power supply for controlling the conveyor belt 3 is turned on, and each tempered glass in the tempered glass assembly 4 is transported to the microwave oven II at a speed of 1.5 m / min through the conveyor belt 3, and the microwave generating assembly 1 is turned on at the same time, and the tempered glass assembly 4 is detonated under microwave irradiation; The conditions for the detonation treatment are as follows: the microwave irradiation frequency is 2.45 GHz, and the microwave generation power is 20 kW; When all the tempered glasses in the tempered glass combination 4 were transported out of the microwave oven II, the timing was stopped, and the results were as follows: after 10 minutes of microwave irradiation, 3 tempered glasses in the tempered glass combination 4 burst, and by observing and analyzing the cracking points of the glasses that burst, it was detected that nickel sulfide impurity components were contained near the bursting points, that is, the bursting points were the locations of the nickel sulfide impurities; the tempered glasses in the tempered glass combination 4 that did not burst continued to be irradiated with microwaves, and they still did not burst after 120 minutes.
[0064] Comparative Example 1: This example is carried out according to the method of Example 1, except that tempered glass DI is used instead of tempered glass I2, and the remaining steps and parameters are the same as those of Example 1.
[0065] After 120 minutes of microwave irradiation, the tempered glass DI did not explode.
[0066] Comparative Example 2 In this example, the tempered glass containing nickel sulfide impurities is detonated according to the method of Example 1, except that the conditions for the detonation treatment meet the following requirements: the microwave irradiation power is 300 W, and the remaining steps and parameters are the same as in Example 1.
[0067] After 120 min of microwave irradiation, the tempered glass I 2 did not explode.
[0068] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for rapidly detonating tempered glass containing nickel sulfide impurities, characterized in that: The method comprises: detonating tempered glass containing nickel sulfide under microwave irradiation; The conditions for the detonation treatment at least meet the following requirements: microwave irradiation frequency is 0.915-2.45 GHz, and microwave generation power is 0.5-1000 kW.
2. The method according to claim 1, wherein: The detonation process is carried out in a microwave irradiation detonation device; the microwave irradiation detonation device comprises: A box body, wherein a transmission device for conveying the tempered glass is disposed at the bottom of the box body, and a window for the tempered glass to enter and exit is also disposed on the side of the box body; A microwave generating component is arranged inside the box and is used for emitting microwaves that can promote the phase change and expansion of nickel sulfide.
Citation Information
Patent Citations
Detection method of nickel sulfide in glass
CN101852769A
Homogenization processing method for tempered glass and tempered glass
CN108328913A
Screening device used before glass tempering
CN106483165A
Method and apparatus for detecting foreign matter in glass
JP2005098905A
Apparatus for detecting nis in glass
KR101229179B1