Grating manufacturing method and laser chip
By using a metal mask to replace the photoresist pattern in grating structure production and using the second opening as an etching template, the problem of small duty cycle of grating structure is solved, which significantly improves the duty cycle of grating structure and satisfies higher process requirements.
Patent Information
- Application Number
- CN202411114664.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing grating structure production methods have resulted in a relatively small duty cycle of grating structures, which cannot meet the process needs of some products.
By setting a metal mask on the anti-reverse film, and after removing the photoresist and anti-reverse film, a second opening is used as an etching template to form a grating structure with a larger transverse size, the metal mask replaces the photoresist pattern. Increase the duty cycle of the grating structure.
The duty cycle of the grating structure is significantly improved, the lateral dimensional stability of the grating pattern is ensured, the impact of lateral corrosion is avoided, and the higher process needs are met.
Smart Images

Figure CN119024477A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a grating manufacturing method and a laser chip. Background Art
[0002] In order to improve the monochromaticity of the laser chip, it is usually necessary to add a grating structure inside the laser chip to utilize the frequency-selective characteristics of grating diffraction. In the related art, in order to avoid the influence of interface reflected light and standing wave effect on the process, the manufacturing process of the grating structure is usually as follows: anti-reflection glue and photoresist are coated on the upper surface of the semiconductor substrate in sequence, wherein the anti-reflection glue is insensitive to the ultraviolet light used for photolithography exposure, thereby reducing the standing wave effect, and by controlling the thickness of the anti-reflection film, the influence of interface reflected light during exposure can be reduced; after exposure and development, the grating pattern required by the process is formed on the photoresist, and then the anti-reflection glue without photoresist protection is removed by plasma oxidation, so that the grating pattern is transferred to the anti-reflection glue to complete the production of the grating mask, and finally the grating pattern structure required by the process is etched on the semiconductor substrate by wet etching or dry etching. However, the grating structure made using this technology has a small space ratio and cannot meet the process requirements of some products. Summary of the invention
[0003] In view of this, the present invention proposes a grating manufacturing method and a laser chip to solve the problem that the grating structure manufactured by the manufacturing method of the grating structure in the related art has a small duty cycle.
[0004] The technical solution of the present invention is achieved in this way:
[0005] In one aspect, the present invention provides a grating manufacturing method, comprising the following steps:
[0006] S1. providing a semiconductor substrate;
[0007] S2, providing an anti-reflection film on the semiconductor substrate;
[0008] S3, disposing a photoresist on the anti-reflective film, and etching the photoresist to form a plurality of first openings;
[0009] S4, disposing a metal mask on the surface of the anti-reflective film corresponding to the first opening;
[0010] S5, removing the photoresist and the anti-reflective film between two adjacent first openings, so as to form a plurality of second openings on the anti-reflective film;
[0011] S6, etching the upper surface of the semiconductor substrate at the second opening to form a grating structure on the upper surface of the semiconductor substrate;
[0012] S7, removing the metal mask and the anti-reflection film on both sides of the second opening to complete the grating production.
[0013] On the basis of the above technical solution, preferably, in step S4, the metal mask disposed on the surface of the anti-reflective film corresponding to the first opening is formed by a sputtering process.
[0014] Furthermore, preferably, a metal mask is formed on a side of the photoresist away from the anti-reflective film through a sputtering process.
[0015] Further, preferably, the thickness of the metal mask is smaller than the thickness of the photoresist.
[0016] On the basis of the above technical solution, preferably, in step S5, the photoresist is removed by a stripping solution, and the antireflective film between two adjacent first openings is removed by a plasma oxidation method or a reactive ion etching process.
[0017] Based on the above technical solution, preferably, in step S7, the metal mask on both sides of the second opening is removed by wet etching, and the anti-reflective film under the metal mask is removed by plasma oxidation or reactive ion etching.
[0018] On the basis of the above technical solution, preferably, the anti-reflection film has a preset thickness and a preset refractive index, the preset thickness is 35-45 nm, and the anti-reflection film is an organic or inorganic material.
[0019] On the basis of the above technical solution, preferably, in step S6, the method of etching the upper surface of the semiconductor substrate at the second opening is wet etching.
[0020] On the basis of the above technical solution, preferably, the semiconductor substrate includes a base layer, a restriction layer and a grating material layer which are stacked; the upper surface of the semiconductor substrate is etched at the second opening to form a grating structure on the upper surface of the semiconductor substrate, specifically including: etching the grating material layer at the second opening to form the grating structure.
[0021] On the other hand, the present invention further provides a laser chip, comprising a grating structure, wherein the grating structure is manufactured using the grating manufacturing method described in the first aspect.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The present invention arranges a metal mask above the anti-reflection film corresponding to the first opening, and after removing the photoresist and the anti-reflection film between two adjacent first openings, the second opening is formed with the metal mask and the anti-reflection film on both sides from top to bottom, thereby ensuring the stability of the lateral size of the grating pattern during the etching process. When the second opening is used as an etching template to etch the semiconductor substrate, the metal mask effectively prevents the influence of lateral corrosion, ensures the lateral size of the opening of the grating pattern, and significantly improves the duty cycle of the grating structure.
[0024] (2) By setting the thickness of the metal mask to be smaller than the thickness of the photoresist, the degumming melt can firstly perform a melting reaction on the photoresist leaking out of the metal mask on both sides in the first opening. When the photoresist in this part is dissolved, the metal mask on the upper part will naturally peel off. The degumming solution operation is continued to remove the photoresist between the two adjacent metal masks. At this time, after the photoresist is completely removed, a second opening is formed between the two adjacent metal masks. At the same time, the first opening disappears immediately. The role of the second opening at this time replaces the role of the first opening, which is used as the opening size of the grating pattern. At the same time, the metal mask replaces the photoresist pattern in the prior art. Since there is no photoresist, when the anti-reflection film at the second opening is etched, it will not be affected due to the high corrosion resistance of the metal mask. Therefore, when the grating structure is etched, the lateral size of the opening of the grating pattern will not be reduced, thereby improving the duty cycle of the grating structure.
[0025] (3) Since the anti-reflective film of the present invention is directly above a metal mask instead of a photoresist pattern, the size of the metal mask will not be affected by etching the anti-reflective film, which is beneficial to improving the duty cycle of the grating structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 A flowchart of the grating manufacturing method disclosed in the present invention;
[0028] Figure 2 It is a schematic diagram of a state after an anti-reflective film and a photoresist are sequentially arranged on a semiconductor substrate disclosed in the present invention;
[0029] Figure 3 It is a schematic diagram of the state after the first opening is formed on the photoresist disclosed in the present invention;
[0030] Figure 4 It is a schematic diagram of the state after a metal mask is set on the photoresist and the anti-reflective film disclosed in the present invention;
[0031] Figure 5 It is a schematic diagram of the state after the photoresist, metal mask and anti-reflective film between two adjacent first openings disclosed in the present invention are removed;
[0032] Figure 6 It is a schematic diagram of a state in which the upper surface of the semiconductor substrate is etched at the second opening to form a grating structure disclosed in the present invention;
[0033] Figure 7 It is a schematic diagram of a state after the metal mask and the anti-reflection film on both sides of the second opening disclosed in the present invention are removed;
[0034] Figure 8 It is a schematic diagram of a state after the photoresist, the metal mask and the anti-reflective film between two adjacent first openings disclosed in one embodiment of the present invention are removed;
[0035] Fig. 9 It is a schematic diagram of a state in which a grating structure is formed by etching the upper surface of a semiconductor substrate at a second opening according to an embodiment of the present invention;
[0036] Fig.10 is a schematic diagram of a grating structure disclosed in an embodiment of the present invention;
[0037] Reference numerals:
[0038] 1. Semiconductor substrate; 2. Anti-reflective film; 3. Photoresist; P1, first opening; 4. Metal mask; P2, second opening; 11. Grating structure; 13. Base layer; 12. Restriction layer; 110. Grating material layer; 111. Transparent slit; 112. Optical opaque part. DETAILED DESCRIPTION
[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] After research, it was found that after the required grating pattern is formed on the photoresist, since both the photoresist and the anti-reflective adhesive are organic materials, when the photoresist utilizes an oxidation reaction (such as plasma stripping) process, while etching the anti-reflective adhesive, it will also easily corrode the photoresist laterally, changing the lateral size of the opening of the above-mentioned grating pattern. The grating structure is formed based on the grating pattern, resulting in the final grating structure having a smaller duty cycle.
[0041] First, as Figure 1 As shown, combined Figure 2-7 The embodiment of the present invention provides a grating manufacturing method, comprising the following steps:
[0042] S1, providing a semiconductor substrate 1;
[0043] S2. Refer to the attached Figure 1 As shown, an anti-reflection film 2 is provided on the semiconductor substrate 1. The function of the anti-reflection film 2 is to reduce the reflection and standing wave effect of light. As some embodiments, the anti-reflection film 2 can be deposited on the semiconductor substrate 1 by a plasma enhanced chemical vapor deposition (PECVD, Plasma Enhanced Chemical Vapor Deposition) process, a physical vapor deposition (Physical Vapor Deposition, PVD) process, an atomic layer deposition (ALD) process or a chemical vapor deposition (CVD) process, etc., without specific limitation herein.
[0044] S3. Refer to the attached Figure 1 and 2 As shown, a photoresist 3 is disposed on the anti-reflective film 2 and the photoresist 3 is etched to form a plurality of first openings P1 to ensure the accuracy and consistency of subsequent etching steps.
[0045] Specifically, a photoresist 3 can be coated on the anti-reflective film 2 to form a photoresist layer with uniform thickness on one side, and then a photoresist pattern with multiple first openings P1 can be formed on the photoresist layer by exposure and development. The photoresist 3 layer can be exposed by ultraviolet exposure (i.e., Talbot effect exposure) to form a photoresist pattern. In this embodiment, the thickness of the photoresist 3 is controlled to be 200nm to 500nm, and these first openings P1 define the position of the grating structure 11.
[0046] S4, a metal mask 4 is disposed on the surface of the anti-reflective film 2 corresponding to the first opening P1. The metal mask 4 is used as an etching mask in subsequent steps to reduce side etching generated when removing the anti-reflective film 2.
[0047] In this embodiment, the metal mask 4 is realized by a sputtering process, and the metal used for sputtering is selected to be easy to remove, preferably, it can be titanium or nickel metal.
[0048] In some embodiments, it is difficult to set the metal mask 4 on the surface of the anti-reflective film 2 corresponding to the first opening P1 through the sputtering process, and it is difficult to control a specific area. Therefore, this embodiment adopts the sputtering process to achieve overall sputtering of the surface of the semiconductor substrate 1, which makes the photoresist 3 and the surface of the anti-reflective film 2 corresponding to the first opening P1 covered with the metal mask 4.
[0049] S5, removing the photoresist 3 and the antireflective film 2 between two adjacent first openings P1, so as to form a plurality of second openings P2 on the antireflective film 2. At this time, with the removal of the photoresist 3, the first openings P1 no longer exist, and the second openings P2 are openings formed when the antireflective film 2 is removed, and the bottom of the second openings P2 corresponds to the semiconductor substrate 1, and the two sides of the second openings P2 are the metal mask 4 and the antireflective film 2 from top to bottom.
[0050] Since in the prior art, there is a photoresist pattern above the anti-reflective film 2, the photoresist pattern will be easily corroded laterally while etching the anti-reflective film 2, thereby changing the lateral size of the opening of the above-mentioned grating pattern. The grating structure 11 is formed based on the grating pattern, resulting in a smaller occupancy rate of the final grating structure 11.
[0051] In the present invention, the metal mask 4 is located above the anti-reflective film 2, and the width of the metal mask 4 is determined by the width of the first opening P1. Relative to the photoresist pattern, the metal mask 4 has a strong corrosion resistance, so when the anti-reflective film 2 is etched, it will not affect the metal mask 4, thereby ensuring the lateral size of the opening of the grating pattern, so that the final grating structure 11 occupies a larger space.
[0052] S6. Etching the upper surface of the semiconductor substrate 1 at the second opening P2 to form a grating structure 11 on the upper surface of the semiconductor substrate 1. In this step, the semiconductor substrate 1 is etched using the second opening P2 as an etching template to form the grating structure 11. During the etching process, the metal mask 4 acts as a barrier. Although a certain amount of lateral etching will be caused to the anti-reflection film 2 during the etching process of the semiconductor substrate 1, the metal mask 4 will not be affected during the etching process. Therefore, the semiconductor substrate 1 corresponding to the second opening P2 forms a light-transmitting slit 111 after etching, and the two sides of the light-transmitting slit 111 are opaque parts 112, and the opaque parts 112 are located directly below the anti-reflection film 2. The size of the light-transmitting slit 111 directly affects the duty cycle of the grating structure 11. The method of this embodiment can reduce or avoid the increase in the size of the light-transmitting slit 111, ensure the lateral size of the opening of the grating pattern, and thus improve the duty cycle of the grating structure 11.
[0053] S7, removing the metal mask 4 and the anti-reflection film 2 on both sides of the second opening P2, and completing the grating production. Through this step, the purity and integrity of the grating structure 11 can be ensured to meet the expected grating design requirements.
[0054] The present invention arranges a metal mask 4 above the antireflection film 2 corresponding to the first opening P1, and after removing the photoresist 3 and the antireflection film 2 between two adjacent first openings P1, the second opening P2 is formed with the metal mask 4 and the antireflection film 2 on both sides from top to bottom, thereby ensuring the stability of the lateral size of the grating pattern during the etching process. When the second opening P2 is used as an etching template to etch the semiconductor substrate 1, the metal mask 4 effectively prevents the influence of lateral corrosion, ensures the lateral size of the opening of the grating pattern, and significantly improves the duty cycle of the grating structure 11.
[0055] Since the metal mask 4 is sputtered on the top surface of the photoresist 3 and the surface of the anti-reflective film 2 corresponding to the first opening P1, when removing the photoresist 3, this embodiment adopts a degumming solution to remove it, which requires that the photoresist 3 can effectively contact the degumming solution. As a preferred embodiment, the thickness of the metal mask 4 needs to be smaller than the thickness of the photoresist 3.
[0056] By adopting the above technical solution, the stripping melt can firstly perform a welding reaction on the photoresist 3 leaking out of the metal mask 4 on both sides in the first opening P1. When the photoresist 3 of this part is dissolved, the metal mask 4 on the upper part will naturally be peeled off. The stripping solution operation is continued to remove the photoresist 3 between two adjacent metal masks 4. At this time, after the photoresist 3 is completely removed, a second opening P2 is formed between two adjacent metal masks 4. At the same time, the first opening P1 disappears immediately. The role of the second opening P2 at this time replaces the role of the first opening P1, which is used as the opening size of the grating pattern. At the same time, the metal mask 4 replaces the photoresist pattern in the prior art. Since there is no photoresist 3, when the anti-reflection film 2 at the second opening P2 is etched, it will not be affected due to the high corrosion resistance of the metal mask 4. Therefore, when the grating structure 11 is etched, the lateral size of the opening of the grating pattern will not be reduced, thereby improving the duty cycle of the grating structure 11.
[0057] In this embodiment, after completely removing the photoresist 3, it is also necessary to remove the anti-reflective film 2 between two adjacent metal masks 4 so as to carry out the next step of etching the non-grating structure 11. To this end, this embodiment removes it by plasma oxidation or reactive ion etching process. Plasma oxidation is a dry etching technology that physically and chemically etches the anti-reflective film 2 by reactive ions generated in plasma.
[0058] It is worth noting that since the metal mask 4 is located directly above the antireflective film 2 of the present invention instead of a photoresist pattern, the size of the metal mask 4 will not be affected by etching the antireflective film 2 , which is beneficial to improving the duty cycle of the grating structure 11 .
[0059] As some preferred embodiments, in step S7, the metal mask 4 on both sides of the second opening P2 is removed by wet etching, which is a commonly used etching technology that selectively removes the metal layer by reacting a chemical solution with the metal mask 4. The anti-reflective film 2 under the metal mask 4 is removed by plasma oxidation or reactive ion etching.
[0060] In some embodiments, the anti-reflection film 2 has a preset thickness and a preset refractive index. When the photoresist 3 is exposed, light is irradiated onto the semiconductor substrate 1 through the photoresist 3. At the interface between the photoresist 3 and the semiconductor substrate 1, in order to prevent this part of the light from being reflected and interfering with the incident light, thereby causing uneven distribution of light intensity along the depth direction of the photoresist 3 (forming a standing wave effect), the anti-reflection film 2 can have a preset thickness and a preset refractive index to prevent the light from being reflected at the interface between the photoresist 3 and the semiconductor substrate 1 when the photoresist 3 is exposed, thereby causing a standing wave effect.
[0061] If the thickness of the anti-reflection film 2 is too large or too small, the anti-reflection effect of the anti-reflection film 2 will be affected; therefore, the thickness of the anti-reflection film 2 needs to be set within a certain range, such as 35 to 45 nm, which can effectively avoid the standing wave effect caused by the reflection of light at the interface between the photoresist 3 and the semiconductor substrate 1 when the photoresist 3 is exposed.
[0062] Optionally, the material of the anti-reflective film 2 needs to be selected according to the material of the semiconductor substrate 1, and is selected in combination with the refractive index and thickness of the anti-reflective film 2. For example, the anti-reflective film 2 includes a silicon nitride layer or a silicon oxide layer. The silicon nitride layer can be SiNX, and the silicon oxide layer can be SiOX. The silicon nitride layer and the silicon oxide layer are both inorganic materials. In the process of etching the anti-reflective film 2, an inorganic material with different properties from the photoresist pattern as an organic material is selected as the anti-reflective film 2, which is beneficial to improve the etching selectivity of the anti-reflective film 2 and the photoresist pattern, and then it is beneficial to reduce the effect of the etching process of the anti-reflective film 2 on the size of the photoresist pattern. Since the present invention uses a metal mask 4 to replace the photoresist 3 in the grating manufacturing process, there is no photoresist 3, and there is no effect on the size of the photoresist pattern when the anti-reflective film 2 is etched, so the anti-reflective film 2 can also be provided with an organic material.
[0063] As some preferred embodiments, in step S6, the method for etching the upper surface of the semiconductor substrate 1 at the second opening P2 is wet etching. By using wet etching, the height of the etched grating can be guaranteed, and then the depth of the side etching can be controlled by controlling the wet etching time, thereby obtaining gratings with different duty ratios.
[0064] As some preferred implementations, refer to the attached Figure 8-10As shown, the semiconductor substrate 1 includes a stacked base layer 13 , a limiting layer 12 and a grating material layer 110 . The step of forming the anti-reflection film 2 on the semiconductor substrate 1 specifically includes: forming the anti-reflection film 2 on the grating material layer 110 .
[0065] Etching the upper surface of the semiconductor substrate 1 at the second opening P2 to form a grating structure 11 on the upper surface of the semiconductor substrate 1 specifically includes: etching the grating material layer 110 at the second opening P2 to form the grating structure 11 .
[0066] The barrier layer can prevent the etchant used to etch the grating material layer 110 from damaging the base layer 13 .
[0067] As some embodiments, the material of the grating material layer 110 includes gallium arsenide (GaAs), the material of the barrier layer includes indium gallium phosphide (InGaP), and the etchant for etching the grating material layer 110 includes a mixed solution of sulfuric acid (H2SO4), hydrogen peroxide (H2O2) and water (H2O). Alternatively, the material of the grating material layer 110 includes indium gallium phosphide InGaP, the material of the barrier layer includes gallium arsenide GaAs, and the etchant for etching the grating material layer 110 uses a diluted solution of hydrochloric acid (HCl). Of course, the grating material layer 110, the barrier layer and the etchant for etching the grating material layer 110 may also be other materials, as long as the barrier layer can be used to prevent the etchant for etching the grating material layer 110 from damaging the base layer 13 in the process of etching the grating material layer 110 at the second opening P2.
[0068] In a second aspect, the present invention further provides a laser chip, comprising a grating structure 11, wherein the grating structure 11 is manufactured using the grating manufacturing method described in the first aspect.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A grating manufacturing method, characterized in that: The steps include: S1. providing a semiconductor substrate (1); S2, providing an anti-reflection film (2) on the semiconductor substrate (1); S3, disposing a photoresist (3) on the anti-reflective film (2), and etching the photoresist (3) to form a plurality of first openings (P1); S4, disposing a metal mask (4) on the surface of the anti-reflective film (2) corresponding to the first opening (P1); S5, removing the photoresist (3) and the anti-reflective film (2) between two adjacent first openings (P1), so as to form a plurality of second openings (P2) on the anti-reflective film (2); S6, etching the upper surface of the semiconductor substrate (1) at the second opening (P2) to form a grating structure (11) on the upper surface of the semiconductor substrate (1); S7, removing the metal mask (4) and the anti-reflection film (2) on both sides of the second opening (P2), and completing the grating production.
2. The grating manufacturing method according to claim 1, characterized in that: In step S4, the metal mask (4) disposed on the surface of the anti-reflective film (2) corresponding to the first opening (P1) is formed by a sputtering process.
3. The grating manufacturing method according to claim 1, characterized in that: A metal mask (4) is also formed on the side of the photoresist (3) away from the anti-reflective film (2) through a sputtering process.
4. The grating manufacturing method according to claim 3, characterized in that: The thickness of the metal mask (4) is smaller than the thickness of the photoresist (3).
5. The grating manufacturing method according to claim 4, characterized in that: In step S5, the photoresist (3) is removed by a stripping solution, and the anti-reflective film (2) between two adjacent first openings (P1) is removed by a plasma oxidation method or a reactive ion etching process.
6. The grating manufacturing method according to claim 1, characterized in that: In step S7, the metal mask (4) on both sides of the second opening (P2) is removed by wet etching, and the anti-reflective film (2) below the metal mask (4) is removed by plasma oxidation or reactive ion etching.
7. The grating manufacturing method according to claim 1, characterized in that: The anti-reflection film (2) has a preset thickness and a preset refractive index, the preset thickness is 35-45 nm, and the anti-reflection film (2) is made of an organic or inorganic material.
8. The grating manufacturing method according to claim 1, characterized in that: In step S6, the method of etching the upper surface of the semiconductor substrate (1) at the second opening (P2) is wet etching.
9. The grating manufacturing method according to any one of claims 1 to 8, characterized in that: The semiconductor substrate (1) comprises a base layer (13), a restriction layer (12) and a grating material layer (110) which are stacked; the upper surface of the semiconductor substrate (1) is etched at the second opening (P2) to form a grating structure (11) on the upper surface of the semiconductor substrate (1), specifically comprising: etching the grating material layer (110) at the second opening (P2) to form the grating structure (11).
10. A laser chip, characterized in that: The invention comprises a grating structure (11), wherein the grating structure (11) is manufactured by using the grating manufacturing method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Lithium tantalate micro-patterning method based on reactive ion etching
CN111627811A
Processing method of grating with high aspect ratio
CN117420626A
Semiconductor buried grating fabrication method
US20090246707A1