Duplex stainless steel forge piece and component design method thereof

Through thermodynamic calculation and finite element simulation, the composition and process of duplex stainless steel forgings are optimized, and the problems of long development cycle and high cost of large forgings are solved, and rapid development and efficient production are achieved.

CN119028495AInactive Publication Date: 2024-11-26CHINA FIRST HEAVY IND +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411165917.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The development cycle of large duplex stainless steel forgings is long and the development cost is high. The existing methods require multiple laboratory tests and verification of intermediate test pieces, resulting in inefficiency.

Method used

Thermodynamic calculation determines the equilibrium phase, unbalanced phase and brittle phase of the material, combines the finite element simulation software to simulate the forging process, optimize the biphasic proportions and process parameters, and designs components and process flows suitable for large forgings to reduce the test volume and Verification steps.

Benefits of technology

It shortens the R&D cycle, improves product performance stability and market competitiveness, and realizes the rapid development and efficient production of large duplex stainless steel forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028495A_ABST
    Figure CN119028495A_ABST
Patent Text Reader

Abstract

The invention provides a duplex stainless steel forge piece and a component design method thereof, and relates to the technical field of alloy design. The component design method of the duplex stainless steel forge piece comprises the following steps that materials are determined; and determining material components. A large duplex stainless steel forge piece material rapid design process based on material thermodynamic calculation, finite element simulation and a small number of verification tests; the method comprises the following steps: performing preliminary evaluation on a material based on material thermodynamic calculation so as to determine important factors, including a brittle phase structure, a phase proportion and the like, influencing the performance of the forging; the optimal component range of the material is determined according to the brittle phase precipitation thermodynamics and dynamics and phase proportion control, so that the laboratory result is closer to the result of a large forge piece product, a rapid development way is provided for the large duplex stainless steel forge piece, the test quantity is reduced, the verification step of a middle test piece is omitted, and the research and development period of the product is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy design, and in particular to a duplex stainless steel forging and a composition design method thereof. Background Art

[0002] Duplex stainless steel has the advantages of both ferritic stainless steel and austenitic stainless steel. It combines the excellent toughness and weldability of austenitic stainless steel with the high strength and chloride stress corrosion resistance of ferritic stainless steel. It is these superior properties that make duplex stainless steel one of the preferred materials for offshore oil and gas development. At the same time, due to the special two-phase structure, its material properties are closely related to the two-phase ratio, and the deformation temperature range is narrow, and the heat treatment deformation law is also different from that of ordinary steel.

[0003] There have been many studies on duplex stainless steel forgings, including how to avoid forging cracks. These studies are based on laboratory test methods. For ultra-large products with a diameter of more than 2 meters, such as Figure 2 As shown, the current development method steps are: first, the composition is designed according to standards and literature, small steel ingots are refined, and physical and chemical tests are performed to verify whether its performance meets the requirements, and then it is verified through pilot samples. If the performance meets the requirements, the material is put into production. If the performance does not meet the requirements, the composition needs to be redesigned. This process makes the development cycle of large duplex stainless steel forgings long and the development cost high. Summary of the invention

[0004] The problem solved by the invention is how to solve the problem of long development cycle and high development cost of large duplex stainless steel forgings.

[0005] In order to solve the above problems, the present invention provides a duplex stainless steel forging and a composition design method thereof.

[0006] In a first aspect, the present invention provides a composition design method for a duplex stainless steel forging, comprising the following steps:

[0007] S1: Determination of materials. The equilibrium phase, non-equilibrium phase, phases that have an important influence on the performance, and precipitation phases that have an important influence on the process are determined through thermodynamic calculations, and the influence of each phase on the material performance is calculated; the factor that has an important influence on the performance in the material is determined to be the duplex ratio of duplex stainless steel. The duplex ratio is the ratio of austenite phase to ferrite phase. The duplex ratio is selected as 1:1. The factor that has an important influence on the process is determined to be the brittle phase; through thermodynamic calculations, based on the composition range of the material specified in the standard, the influence of each material on the duplex ratio, brittle phase and material strength is obtained, and the materials selected are Fe, C, Si, Mn, P, S, Cr, Ni, Mo and N;

[0008] S2: Determination of material composition, comprehensive material properties, dual-phase ratio and precipitation control of brittle phase, with dual-phase ratio of 1:1 and avoidance of precipitation of brittle phase as screening targets, through thermodynamic calculation, the material composition of duplex stainless steel forgings is determined by weight as C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr22.00-23.00%, Ni 4.50-5.50%, Mo 2.50-3.50% and N0.08-0.20%, and the rest is Fe.

[0009] Optionally, the method further includes step S0: determining the working conditions, determining the heat treatment and water-cooling quenching methods according to the workpiece size, and calculating the cooling rate that can be achieved at the slowest cooling point of the workpiece during water-cooling quenching by finite element simulation software.

[0010] Optionally, the workpiece is an annular forging, and the slowest cooling point of the workpiece is at 1 / 2 thickness of the workpiece.

[0011] Optionally, the method further includes step S3: simulating forging, refining steel ingots according to the material components in S3, forging the steel ingots, and obtaining forgings.

[0012] Optionally, the method further includes step S4: performing performance testing on the forging obtained in step S3.

[0013] Optionally, the selected biphasic ratio parameter is 1:1.

[0014] In a second aspect, the present invention provides a duplex stainless steel forging, which is designed and manufactured using the composition design method for a duplex stainless steel forging as described in any one of the above items.

[0015] Optionally, based on weight percentage, it includes C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr 22.00-23.00%, Ni 4.50-5.50%, Mo 2.50-3.50% and N0.08-0.20%, and the rest is Fe.

[0016] The beneficial effects of the duplex stainless steel forging and the composition design method thereof of the present invention are: based on the material thermodynamic calculation, the material is preliminarily evaluated to determine the important factors affecting the forging performance, including the brittle phase structure, phase ratio, etc.; based on the brittle phase precipitation thermodynamics and kinetics, and the control of the phase ratio, the optimal composition range of the material is determined, so that the laboratory results are closer to the results of large forging products, and a rapid development path is provided for large duplex stainless steel forgings, the test amount is reduced, the pilot piece verification step is omitted, the product development cycle is shortened, and the market competitiveness of the enterprise is improved. At the same time, within a wider range of material standard composition, according to the actual working conditions, a narrower range of composition that is more suitable for the working conditions and processes is obtained, thereby improving the stability of product performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is a flow chart of the design method of the duplex stainless steel forging of this embodiment 1;

[0018] Figure 2 The flowchart of the current method for producing duplex stainless steel forgings in the background technology is as follows;

[0019] Figure 3 The displacement field cloud map of the workpiece after heat treatment is extracted based on the simulation calculation results according to step 4 of this embodiment 1. DETAILED DESCRIPTION

[0020] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0021] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0022] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0023] In view of the problems existing in the above-mentioned related technologies, this embodiment provides a duplex stainless steel forging and a composition design method thereof.

[0024] An embodiment of the present invention provides a composition design method for a duplex stainless steel forging, comprising the following steps:

[0025] S1: Determination of materials. The equilibrium phase, non-equilibrium phase, phase that has an important influence on the performance, and precipitation phase that has an important influence on the process are determined through thermodynamic calculations. The factor that has an important influence on the performance in the material is determined to be the duplex ratio of duplex stainless steel. The duplex ratio is the ratio of austenite phase to ferrite phase. The duplex ratio is selected as 1:1. The factor that has an important influence on the process is determined to be the precipitation brittle phase. Through thermodynamic calculations, calculations are performed based on the composition range of the material specified in the standard to obtain the influence of each component element on the duplex ratio, brittle phase and material strength. The material composition is determined to be Fe, C, Si, Mn, P, S, Cr, Ni, Mo and N.

[0026] S2: Determination of material composition, comprehensive material properties, dual-phase ratio and precipitation control of brittle phase, with dual-phase ratio of 1:1 and avoidance of precipitation of brittle phase as screening targets, through thermodynamic calculation, the material composition of duplex stainless steel forgings is determined by weight as C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr22.00-23.00%, Ni 4.50-5.50%, Mo 2.50-3.50% and N0.08-0.20%, and the rest is Fe.

[0027] Specifically, it is determined that the factor that has an important influence on the strength properties in the material is the duplex ratio of the duplex stainless steel.

[0028] In this embodiment, based on the material thermodynamic calculation, the material is preliminarily evaluated to determine the important factors affecting the forging performance, including brittle phase structure, phase ratio, etc.; based on the brittle phase precipitation thermodynamics and kinetics, as well as the control of phase ratio, the optimal material composition range is determined, so that the laboratory results are closer to the results of large forging products, providing a rapid development path for large duplex stainless steel forgings, reducing the test volume, omitting the test piece verification step, shortening the product development cycle, and improving the market competitiveness of the enterprise. At the same time, within a wider range of material standard composition, according to the actual working conditions, a narrower range of composition that is more suitable for working conditions and processes is obtained, thereby improving the stability of product performance.

[0029] Optionally, the method further includes step S0: determining the working conditions, determining the heat treatment and water-cooling quenching methods according to the size of the workpiece, and calculating by finite element simulation software the cooling rate that can be achieved at the slowest cooling point of the workpiece during water-cooling quenching.

[0030] In this optional embodiment, a rapid process for large duplex stainless steel forging material design is provided based on material thermodynamic calculations, finite element simulations, and a small amount of verification tests.

[0031] Optionally, the workpiece is an annular forging, and the slowest cooling point of the workpiece is at 1 / 2 thickness of the workpiece.

[0032] Optionally, the design method of duplex stainless steel forgings includes process design in addition to composition design, specifically including:

[0033] 1. Through material thermodynamic calculation, the equilibrium precipitation temperature range of the brittle phase in the material component is obtained to be 600-934°C, and it is determined that the final forging temperature of the material cannot be lower than 934°C;

[0034] 2. The material component rheological stress curve and recrystallization model are obtained through material calculation, and the forging temperature range is determined to be 900-1300℃;

[0035] 3. The precipitation dynamics of the brittle phase at the slowest cooling rate limited by the working conditions are obtained through material thermodynamic calculation, and water cooling is determined as the cooling method for performance heat treatment;

[0036] 4. The influence of solution temperature on the precipitation of brittle phase and the ratio of two phases is obtained through material thermodynamic calculation, and 1100℃ is determined as the target temperature of solution temperature;

[0037] 5. The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is carried out through finite element simulation software to obtain the heat treatment temperature curve at the workpiece sampling point;

[0038] 6. The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is carried out through finite element simulation software to obtain the heat treatment deformation trend of the workpiece and determine the margin left on the outer wall of the workpiece during process design.

[0039] In this optional embodiment, a rapid process for designing the process of large duplex stainless steel forgings is based on material thermodynamic calculations, finite element simulations, and a small number of verification tests. The forging temperature range and forging ratio are determined according to the characteristics of the material, including the flow stress curve, the recrystallization model, and the brittle phase precipitation temperature range. According to the temperature-structure-stress three-field coupling simulation of the heat treatment process, the heat treatment temperature curve at the sampling point or the position of interest is obtained, and then a physical simulation is performed in the laboratory based on the temperature curve to replace the heat treatment process experienced by the material at the specified position during the heat treatment of the large forging, so that the laboratory results are closer to the results of the large forging products.

[0040] Optionally, according to step 1 and step 2, the initial forging temperature of the forging method is designed to be 1100-1300°C, and the final forging temperature is designed to be 930-1050°C.

[0041] In this optional embodiment, based on material thermodynamic calculations, the forging temperature range is determined according to the characteristics of the material, and then the temperature control of the forging process is determined.

[0042] Optionally, according to step 2, step 3 and step 4, the homogenization temperature of the heat treatment method is designed to be 1000-1100° C., the holding time is designed to be 10-15 hours, and the cooling method is designed to be water cooling.

[0043] In this optional embodiment, based on the temperature-structure-stress three-field coupling simulation of the heat treatment process, the heat treatment temperature curve at the sampling point or the position of interest is obtained, and then physical simulation is performed in the laboratory based on the temperature curve to replace the heat treatment process experienced by the material at the specified position during the heat treatment process of the large forging, thereby making the laboratory results closer to the results of the large forging products.

[0044] Optionally, step 5: perform temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process through finite element simulation software, specifically including: establishing a geometric model, dividing the grid, setting material parameters, setting boundary conditions and submitting calculations, and obtaining the heat treatment temperature curve at the workpiece sampling position based on the simulation calculation results.

[0045] In this optional embodiment, the heat treatment temperature curve at the sampling point or the focus position is obtained based on the temperature-structure-stress three-field coupling simulation of the heat treatment process.

[0046] Optionally, a heat treatment temperature curve of the workpiece at the sampling position is extracted, and the average cooling rate is calculated to be 55° C. / min.

[0047] In this optional embodiment, based on the temperature-structure-stress three-field coupling simulation of the heat treatment process, the heat treatment temperature curve at the sampling point or the focus position is obtained, and the cooling rate is calculated.

[0048] Optionally, step 6: after performing temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process through finite element simulation software, it also includes: based on the simulation calculation results, in the simulation post-processing module, extracting the displacement field cloud map of the workpiece after heat treatment, observing the deformation trend and deformation amount of the workpiece after heat treatment, and determining whether to leave a margin on the outer wall of the workpiece when performing process design.

[0049] In this optional embodiment, the temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is performed by finite element simulation software to obtain the heat treatment deformation trend of the workpiece. The results show that the deformation trend of the workpiece heat treatment process is inward contraction, and the shrinkage of the inner wall is greater than the shrinkage of the outer wall, which is completely different from the outward expansion deformation trend of ordinary steel (steel types that undergo phase change during the thermal process) forgings. Therefore, when conducting process design, consideration should be given to leaving a margin on the outer wall of the annular forging. According to the heat treatment deformation trend and deformation amount, the rough processing size requirements of the forging that can meet the product size requirements before deformation are inferred. According to the rough processing size requirements of the forging, the forging size requirements are determined, and according to the forging size requirements, the ingot size is determined.

[0050] Optionally, the composition design method for duplex stainless steel forgings further includes step S3: simulating forging, refining steel ingots according to the material composition in S2, forging the steel ingots, and obtaining forgings.

[0051] In this optional embodiment, the laboratory results of simulated forging are close to the results of large forging products, which provides a rapid development approach for large duplex stainless steel forgings, reduces the amount of testing, omits the pilot piece verification step, shortens the product development cycle, and improves the company's market competitiveness.

[0052] Optionally, the method further includes step S4: performing performance testing on the forging obtained in step S3.

[0053] In this optional embodiment, the strength, impact toughness and other performance tests are performed to obtain large duplex stainless steel forgings with qualified performance quality. Specifically, the room temperature yield strength is greater than 480MPa, the tensile strength is greater than 680MPa, the elongation is greater than 40%, the cross-sectional shrinkage is greater than 70%, and the impact energy is greater than 70J, then the large duplex stainless steel forgings have qualified performance quality.

[0054] An embodiment of the present invention provides a duplex stainless steel forging, which is designed and manufactured using the composition design method for a duplex stainless steel forging as described in any one of the above items.

[0055] In this embodiment, the optimal composition range of the material is determined, so that the laboratory results are closer to the results of large forging products, providing a rapid development path for large duplex stainless steel forgings, reducing the amount of testing, omitting the test piece verification step, shortening the product development cycle, and improving the market competitiveness of the enterprise. At the same time, within a wider range of material standard composition, according to actual working conditions, a narrower range of composition that is more suitable for working conditions and processes is obtained, thereby improving the stability of product performance.

[0056] Optionally, based on weight percentage, it includes C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr 22.00-23.00%, Ni 4.50-5.50%, Mo 2.50-3.50% and N0.08-0.20%, and the rest is Fe.

[0057] The present invention is further described below in conjunction with specific embodiments.

[0058] Embodiment 1, as Figure 1 As shown, for The manufacturing process design of F51 duplex stainless steel liquid ring sliding forgings (ring forgings) requires that the material has a minimum yield strength of 450 MPa and a minimum tensile strength of 620 MPa. The composition design method and process design method of the present invention are applied, and the steps are as follows:

[0059] Step 1: Calculation of operating condition limits.

[0060] According to user requirements, preliminarily design the rough machining dimensions of the workpiece.

[0061] Since the product requires high strength, the commonly used cooling method for this material (water cooling) is initially considered for the final performance heat treatment.

[0062] Finite element method was used to calculate that under actual water-cooling quenching conditions, the cooling rate that can be achieved at the slowest cooling point of the workpiece (at the T / 2 thickness of the workpiece) is 38°C / min.

[0063] Step 2: Materials evaluation.

[0064] Through thermodynamic calculation and literature evaluation, the equilibrium phase and non-equilibrium phase of the material, the phase that has an important influence on the performance, and the phase that has an important influence on the process are determined. The factor that has an impact on the performance of the material is the dual-phase ratio. When the dual-phase ratio is 1:1, the comprehensive performance of the material is the best. The factor that has an important impact on the process is the brittle phase (σ phase);

[0065] Through thermodynamic calculation software, based on the composition range specified in the standard, the influence of each element content on the dual-phase ratio is calculated as follows: Ni, Mn, and N are austenite stabilizing elements, which play a role in expanding the austenite region, and the solid solution strengthening of N improves the yield, and Mn promotes the solid solution strengthening of N;

[0066] Through thermodynamic calculation software, based on the composition range specified in the standard, the influence of each element content on the precipitation of σ phase is calculated: Mo and Cr elements promote the precipitation of σ phase, especially Mo element has a significant effect on its precipitation, and Mn and C elements have little effect on the precipitation of σ phase within the standard composition range;

[0067] Through thermodynamic calculation software, based on the composition range specified in the standard, the influence of each element content on material strength is calculated as follows: the material strength increases with the increase of ferrite phase proportion, Mn can increase the limit solid solubility of N in steel, and can be used in combination with N to improve the strength of the material, but the S content needs to be controlled to avoid the formation of MnS;

[0068] Step 3: Determine the target component.

[0069] Comprehensively considering the material properties, the ratio of two phases and the precipitation control of the σ phase, the composition optimization target is determined as follows: the Cr element takes the middle upper limit, the Mo element takes the middle lower limit, the Ni element takes the middle lower limit, the N element takes the middle upper limit, the Mn element takes the middle limit, the C element takes the middle upper limit, and the S element takes the currently achievable process lower limit, thereby determining the internal control composition range;

[0070] The screening targets were to set the dual-phase ratio at 1:1 and to avoid precipitation of σ phase as much as possible, and the composition design was performed using material thermodynamic calculation software, as shown in Table 1, where the internal control was the optional range of the material composition obtained in this embodiment.

[0071] Table 1 Material composition design table

[0072]

[0073] Step 4: Process analysis.

[0074] The equilibrium precipitation temperature range of the σ phase in the material is calculated by the material thermodynamic calculation software to be 600-934°C, so it is determined that the final forging temperature of the material cannot be lower than 934°C;

[0075] The material rheological stress curve and recrystallization model were obtained through material calculation, and the forging temperature range was determined to be 900-1300℃;

[0076] The precipitation kinetics of the σ phase at the slowest cooling rate limited by the working conditions was calculated by the material thermodynamic calculation software. The results showed that the σ phase precipitated faster in the range of 930-800℃, and the precipitation amount was about 0.3% at 100s. The residence time of the product workpiece at T / 2 thickness in the range of 930-800℃ was about 100s during the cooling process. Therefore, the σ phase content produced during the heat treatment quenching cooling process may also be around 0.3%, which will not have a significant impact on the performance. Therefore, water cooling can be used as the cooling method for performance heat treatment;

[0077] The influence of solution temperature on the precipitation of σ phase and the ratio of the two phases was calculated by material thermodynamic calculation software. The results showed that the solution temperature had no significant effect on the precipitation of σ phase during the cooling process, but with the increase of solution temperature, the ferrite content increased. When the solution temperature was around 1100℃, the contents of the two phases were close. Therefore, 1100℃ was determined as the target temperature of the solution temperature.

[0078] The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process was carried out by finite element simulation software to obtain the heat treatment temperature curve at the workpiece sampling point;

[0079] Establish forging model in finite element simulation software, including: establishing geometric model, dividing mesh, setting material parameters, setting boundary conditions, and submitting calculation;

[0080] Based on the simulation calculation results, in the simulation post-processing module, the curve of the temperature change of the forging at the sampling position over time is extracted, and the average cooling rate is calculated, which is about 55°C / min.

[0081] The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process was carried out using finite element simulation software to obtain the heat treatment deformation trend of the workpiece.

[0082] Establish forging model in finite element simulation software, including: establishing geometric model, dividing mesh, setting material parameters, setting boundary conditions, and submitting calculation;

[0083] Based on the simulation calculation results, the displacement field cloud diagram of the forging after heat treatment is extracted in the simulation post-processing module, such as Figure 3 As shown;

[0084] Observe the deformation trend and deformation amount of forgings after heat treatment, such as Figure 3As shown in the figure, the displacement field of the forging after heat treatment, the negative number in the legend is shrinkage, it can be seen that the workpiece is in a shrinkage state after heat treatment, and the shrinkage of the inner wall is greater than that of the outer wall. The results show that the deformation trend of the workpiece during the heat treatment process is inward contraction, and the shrinkage of the inner wall is greater than that of the outer wall, which is completely different from the deformation trend of ordinary steel (steel types that undergo phase change during the thermal process) forgings that expand outward. Therefore, when designing the process, consideration should be given to leaving a margin on the outer wall of the ring forging. This is completely different from the deformation trend of ordinary steel (steel types that undergo phase change during the thermal process) forgings that expand outward. Therefore, when designing the process, consideration should be given to leaving a margin on the outer wall of the ring forging.

[0085] According to the deformation trend and deformation amount of heat treatment, the rough processing size requirements of forgings that can meet the product size requirements before deformation are reversed;

[0086] Determine the forging size requirements based on the forging rough machining size requirements;

[0087] Determine the size of the steel ingot according to the forging size requirements.

[0088] Step 5: Process design.

[0089] Obtain raw materials according to the alloy ratio shown in step 3, and perform secondary smelting on the raw materials to obtain steel ingots;

[0090] According to the conclusions obtained in step 4, design the forging blanking size and the workpiece size after forging;

[0091] According to the conclusion obtained in step 4, the forging process is determined, the initial forging temperature is 1100-1300℃, and the final forging temperature is 930-1050℃; if cracking occurs, it must be promptly heat-cleaned at above 930℃. The obtained forging blank is forged to obtain a ring-shaped blank forging;

[0092] Specifically, after blanking and drawing, forging is performed by using deformation methods such as roughing, punching, pre-expansion of a horse bar, and expansion;

[0093] According to the conclusion obtained in step 4, the heat treatment process design is carried out: the homogenization temperature is 1000-1100℃, the holding time is 10-15h, and the cooling method is water cooling.

[0094] Step 6: Physical simulation.

[0095] Refining small steel ingots according to the composition range in step 3; retesting the composition of the refined small steel ingots;

[0096] The small steel ingots obtained by refining are forged; the samples obtained by forging are cut and subjected to physical simulation heat treatment in the heat treatment furnace in step 4; the obtained samples are tested for performance to determine whether they meet the product performance requirements. The results show that the material properties meet the product performance requirements.

[0097] Step 7: Product production.

[0098] The process described in step 5 is used to carry out production, and sampling and testing are carried out according to user requirements, and the performance test is qualified.

[0099] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A composition design method for duplex stainless steel forgings, characterized in that: The following steps are involved: S1: Determination of the material, through thermodynamic calculation, determine the equilibrium phase, non-equilibrium phase, phase that has an important influence on the performance, and precipitation phase that has an important influence on the process of the material, determine that the factor that has an important influence on the performance in the material is the duplex ratio of duplex stainless steel, the duplex ratio is the ratio of the austenite phase to the ferrite phase, select the duplex ratio parameter, and determine that the factor that has an important influence on the process is the brittle phase; through thermodynamic calculation, based on the composition range of the material specified in the standard, calculate the influence of the material on the duplex ratio, the brittle phase and the material strength, and determine that the material is Fe, C, Si, Mn, P, S, Cr, Ni, Mo and N; S2: Determination of material composition, comprehensive material properties, the dual-phase ratio and the precipitation control of the brittle phase, with the dual-phase ratio of 1:1 and avoiding the precipitation of the brittle phase as the screening target, through thermodynamic calculation, it is determined that the material composition of the duplex stainless steel forging is C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr 22.00-23.00%, Ni4.50-5.50%, Mo 2.50-3.50% and N 0.08-0.20% by weight, and the rest is Fe.

2. The composition design method of duplex stainless steel forgings according to claim 1, characterized in that: The method also includes step S0: determining the working conditions, determining the heat treatment and water-cooling quenching methods according to the size of the workpiece, and calculating by finite element simulation software the cooling rate that can be achieved at the slowest cooling point of the workpiece during the water-cooling quenching.

3. The composition design method of duplex stainless steel forgings according to claim 2, characterized in that: The workpiece is an annular forging, and the slowest cooling point of the workpiece is at 1 / 2 thickness of the workpiece.

4. The composition design method of duplex stainless steel forgings according to claim 1, characterized in that: The method further comprises step S3: simulating forging, refining steel ingots according to the material components in S2, and forging the steel ingots to obtain forgings.

5. The composition design method of duplex stainless steel forgings according to claim 4, characterized in that: The method further comprises step S4: performing performance testing on the forging obtained in step S3.

6. The composition design method of duplex stainless steel forgings according to claim 1, characterized in that: In the step S1, the selected two-phase ratio parameter is 1:

1.

7. A duplex stainless steel forging, characterized in that: The duplex stainless steel forging is designed and manufactured by using the composition design method of any one of claims 1 to 6.

8. The duplex stainless steel forging according to claim 7, characterized in that: Calculated by weight, it includes C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr22.00-23.00%, Ni4.50-5.50%, Mo 2.50-3.50% and N 0.08-0.20%, and the rest is Fe.

Citation Information

Patent Citations

  • Heat treatment method for ferrite-austenite duplex stainless steel

    CN114107631A

  • S32750 austenite ferrite super duplex stainless steel seamless tube for deep sea manifold and preparation process of S32750 austenite ferrite super duplex stainless steel seamless tube

    CN114352808A

  • Duplex stainless steel and large-diameter duplex stainless steel liquid slip ring forge piece and preparation method thereof

    CN117210767A