Process design method of duplex stainless steel forge piece
Through material thermodynamic calculation and finite element simulation, the forging temperature interval and heat treatment process of duplex stainless steel forgings are determined, which solves the problems of long development cycle and high cost of large duplex stainless steel forgings, and achieves rapid development and efficient production.
Patent Information
- Application Number
- CN202411166265.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
The development cycle of large duplex stainless steel forgings is long and the development cost is high. The existing technology has challenges such as closely related material performance and proportion and narrow deformation temperature interval in the manufacturing of super-large products.
Thermodynamic calculation of materials and finite element simulation software are used to perform three-field coupled simulation of temperature-structure-stress, determine the forging temperature interval, rheological stress curve and recrystallization model, and select water cooling as the cooling method to shorten the heat treatment process and reduce the test pieces. Verification steps.
Through the rapid process design method, the R&D cycle is shortened, the cost is reduced, and the market competitiveness is improved. The laboratory results are closer to the results of large forging products and the number of tests is reduced.
Smart Images

Figure CN119028496A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy design, and in particular to a process design method for duplex stainless steel forgings. Background Art
[0002] Duplex stainless steel has the advantages of both ferritic stainless steel and austenitic stainless steel. It combines the excellent toughness and weldability of austenitic stainless steel with the high strength and chloride stress corrosion resistance of ferritic stainless steel. It is these superior properties that make duplex stainless steel one of the preferred materials for offshore oil and gas development. At the same time, due to the special two-phase structure, duplex stainless steel faces many challenges in the manufacturing process, such as its material properties are closely related to the two-phase ratio, the deformation temperature range is narrow, and the heat treatment deformation law is unknown.
[0003] At present, there have been many studies on duplex stainless steel forgings, including the study of factors affecting the hot working properties of the material and how to avoid forging cracks. These studies are based on laboratory test methods. For super-large products with a diameter of more than 2 meters, such as Figure 2 As shown in the figure, the current development method steps are: first, small steel ingots are refined according to standards and literature, and their performance is verified by physical and chemical tests to see if they meet the requirements. Secondly, process design is carried out based on physical simulation tests, simulations and experience, and then it is verified by pilot specimens. If the performance meets the requirements, production can be started. If the performance does not meet the requirements, the process needs to be redesigned. This process makes the development cycle of large duplex stainless steel forgings long and the development cost high. Summary of the invention
[0004] The problem solved by the invention is how to solve the problem of long development cycle and high development cost of large duplex stainless steel forgings.
[0005] In order to solve the above problems, the present invention provides a process design method for duplex stainless steel forgings.
[0006] The present invention provides a process design method for duplex stainless steel forgings, comprising the following steps:
[0007] S1: Through material thermodynamic calculation, it is found that the equilibrium precipitation temperature range of the brittle phase in the material component of duplex stainless steel is 600-950℃, and it is determined that the final forging temperature of the material component cannot be lower than 950℃;
[0008] S2: The flow stress curve and recrystallization model of the material components are obtained through material calculation, and the forging temperature range is determined to be 950-1300℃;
[0009] S3: The precipitation kinetics of the brittle phase at the slowest cooling rate limited by the working conditions is obtained through material thermodynamic calculation, and water cooling is determined as the cooling method for performance heat treatment;
[0010] S4: The influence of solution temperature on the precipitation of brittle phase and the ratio of two phases is obtained through material thermodynamic calculation, and the target temperature of solution temperature is determined;
[0011] S5: The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is performed by finite element simulation software to obtain the heat treatment temperature curve at the workpiece sampling point;
[0012] S6: The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is carried out through finite element simulation software to obtain the heat treatment deformation trend of the workpiece and determine the margin left on the outer wall of the workpiece during process design.
[0013] Optionally, the method further includes step S0: determining the working conditions, determining the heat treatment and water-cooling quenching methods according to the size of the workpiece, and calculating by finite element simulation software the cooling rate that can be achieved at the slowest cooling point of the workpiece during water-cooling quenching.
[0014] Optionally, according to step S1 and step S2, the initial forging temperature of the forging method is designed to be 1100-1300°C, and the final forging temperature is designed to be 950-1050°C.
[0015] Optionally, according to step S2, step S3 and step S4, the homogenization temperature of the heat treatment method is designed to be 1000-1100°C, the insulation time is designed to be 10-15h, and the cooling method is designed to be water cooling.
[0016] Optionally, the target temperature of the solutionizing temperature in step S4 is 1100°C.
[0017] Optionally, S5: perform temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process through finite element simulation software, specifically including: establishing a geometric model, dividing the grid, setting material parameters, setting boundary conditions and submitting calculations, and obtaining a heat treatment temperature curve at the workpiece sampling position based on the simulation calculation results.
[0018] Optionally, a heat treatment temperature curve of the workpiece at the sampling position is extracted, and the average cooling rate is calculated to be 60° C. / min.
[0019] Optionally, S6: after performing temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process through finite element simulation software, it also includes: based on the simulation calculation results, in the simulation post-processing module, extracting the displacement field cloud map of the workpiece after heat treatment, observing the deformation trend and deformation amount of the workpiece after heat treatment, and determining whether to leave a margin on the outer wall of the workpiece when performing process design.
[0020] Optionally, the method further includes step S7: simulating forging, refining steel ingots, and forging steel ingots.
[0021] Optionally, the method further includes step S8: performance testing, in which the steel ingot obtained in step S7 is subjected to performance testing.
[0022] The beneficial effects of the process design method of duplex stainless steel forgings of the present invention are as follows: a rapid process of large duplex stainless steel forging process design based on material thermodynamic calculation, finite element simulation and a small amount of verification tests, determining the forging temperature range and forging ratio according to the characteristics of the material, including the rheological stress curve, the recrystallization model, and the brittle phase precipitation temperature range, and obtaining the heat treatment temperature curve at the sampling point or the concerned position according to the temperature-structure-stress three-field coupling simulation of the heat treatment process, so as to perform physical simulation in the laboratory according to the temperature curve to replace the heat treatment process experienced by the material at the designated position of the large forging during the heat treatment process, so as to make the laboratory results closer to the results of the large forging products, provide a rapid development path for large duplex stainless steel forgings, reduce the test volume, omit the pilot piece verification step, shorten the product development cycle, and improve the market competitiveness of the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a flow chart of the design method of the duplex stainless steel forging of this embodiment 1;
[0024] Figure 2 The flowchart of the current method for producing duplex stainless steel forgings in the background technology is as follows;
[0025] Figure 3 The displacement field cloud map of the workpiece after heat treatment is extracted based on the simulation calculation results according to step 4 of this embodiment 1. DETAILED DESCRIPTION
[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0027] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0028] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0029] In view of the problems existing in the above-mentioned related technologies, this embodiment provides a process design method for duplex stainless steel forgings.
[0030] A process design method for a duplex stainless steel forging provided in an embodiment of the present invention comprises the following steps:
[0031] S1: Through material thermodynamic calculation, the equilibrium precipitation temperature range of the brittle phase in the material component is obtained to be 600-950℃, and it is determined that the final forging temperature of the material cannot be lower than 950℃;
[0032] S2: The material composition rheological stress curve and recrystallization model are obtained through material calculation, and the forging temperature range is determined to be 950-1300℃;
[0033] S3: The precipitation kinetics of the brittle phase at the slowest cooling rate limited by the working conditions is obtained through material thermodynamic calculation, and water cooling is determined as the cooling method for performance heat treatment;
[0034] S4: The influence of solution temperature on the precipitation of brittle phase and the ratio of two phases is obtained through material thermodynamic calculation, and the target temperature of solution temperature is determined;
[0035] S5: The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is performed by finite element simulation software to obtain the heat treatment temperature curve at the workpiece sampling point;
[0036] S6: The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is carried out through finite element simulation software to obtain the heat treatment deformation trend of the workpiece and determine the margin left on the outer wall of the workpiece during process design.
[0037] Specifically, the dual phase ratio is the ratio of the austenite phase to the ferrite phase.
[0038] In this optional embodiment, a rapid process for designing the process of large duplex stainless steel forgings is based on material thermodynamic calculations, finite element simulations, and a small number of verification tests. The forging temperature range and forging ratio are determined according to the characteristics of the material, including the flow stress curve, the recrystallization model, and the brittle phase precipitation temperature range. According to the temperature-structure-stress three-field coupling simulation of the heat treatment process, the heat treatment temperature curve at the sampling point or the position of interest is obtained, and then a physical simulation is performed in the laboratory based on the temperature curve to replace the heat treatment process experienced by the material at the specified position during the heat treatment of the large forging, so that the laboratory results are closer to the results of the large forging products.
[0039] Optionally, the method further includes step S0: determining the working conditions, determining the heat treatment and water-cooling quenching methods according to the size of the workpiece, and calculating by finite element simulation software the cooling rate that can be achieved at the slowest cooling point of the workpiece during water-cooling quenching.
[0040] In this optional embodiment, a fast process for designing large duplex stainless steel forging materials is provided based on material thermodynamic calculation, finite element simulation and a small amount of verification tests. Wherein, when the workpiece is an annular forging, the slowest cooling point of the workpiece is at 1 / 2 thickness of the workpiece.
[0041] Optionally, according to step S1 and step S2, the initial forging temperature of the forging method is designed to be 1100-1300°C, and the final forging temperature is designed to be 950-1050°C.
[0042] In this optional embodiment, based on material thermodynamic calculations, the forging temperature range is determined according to the characteristics of the material, and then the temperature control of the forging process is determined.
[0043] Optionally, according to step S2, step S3 and step S4, the homogenization temperature of the heat treatment method is designed to be 1000-1100°C, the insulation time is designed to be 10-15h, and the cooling method is designed to be water cooling.
[0044] In this optional embodiment, based on the temperature-structure-stress three-field coupling simulation of the heat treatment process, the heat treatment temperature curve at the sampling point or the position of interest is obtained, and then physical simulation is performed in the laboratory based on the temperature curve to replace the heat treatment process experienced by the material at the specified position during the heat treatment process of the large forging, thereby making the laboratory results closer to the results of the large forging products.
[0045] Optionally, the target temperature of the solutionizing temperature in step S4 is 1100°C.
[0046] Optionally, step S5: perform temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process through finite element simulation software, specifically including: establishing a geometric model, dividing the grid, setting material parameters, setting boundary conditions and submitting calculations, and obtaining a heat treatment temperature curve at the workpiece sampling position based on the simulation calculation results.
[0047] In this optional embodiment, the heat treatment temperature curve at the sampling point or the focus position is obtained based on the temperature-structure-stress three-field coupling simulation of the heat treatment process.
[0048] Optionally, a heat treatment temperature curve of the workpiece at the sampling position is extracted, and the average cooling rate is calculated to be 60° C. / min.
[0049] In this optional embodiment, based on the temperature-structure-stress three-field coupling simulation of the heat treatment process, the heat treatment temperature curve at the sampling point or the focus position is obtained, and the cooling rate is calculated.
[0050] Optionally, step S6: after performing temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process through finite element simulation software, it also includes: based on the simulation calculation results, in the simulation post-processing module, extracting the displacement field cloud map of the workpiece after heat treatment, observing the deformation trend and deformation amount of the workpiece after heat treatment, and determining whether to leave a margin on the outer wall of the workpiece when performing process design.
[0051] In this optional embodiment, the temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is performed by finite element simulation software to obtain the heat treatment deformation trend of the workpiece. The results show that the deformation trend of the workpiece heat treatment process is inward contraction, and the shrinkage of the inner wall is greater than the shrinkage of the outer wall, which is completely different from the outward expansion deformation trend of ordinary steel (steel types that undergo phase change during the thermal process) forgings. Therefore, when conducting process design, consideration should be given to leaving a margin on the outer wall of the annular forging. According to the heat treatment deformation trend and deformation amount, the rough processing size requirements of the forging that can meet the product size requirements before deformation are inferred. According to the rough processing size requirements of the forging, the forging size requirements are determined, and according to the forging size requirements, the ingot size is determined.
[0052] Optionally, the method further includes step S7: simulating forging, refining steel ingots, and forging steel ingots.
[0053] In this optional embodiment, the laboratory results of simulated forging are close to the results of large forging products, which provides a rapid development approach for large duplex stainless steel forgings, reduces the amount of testing, omits the pilot piece verification step, shortens the product development cycle, and improves the company's market competitiveness.
[0054] Optionally, the method further includes step S8: performance testing, in which the steel ingot obtained in step S7 is subjected to performance testing.
[0055] In this optional embodiment, a large duplex stainless steel forging with qualified performance and quality is obtained.
[0056] In this embodiment, the composition design method of the duplex stainless steel forging includes the following steps:
[0057] Determination of materials: The equilibrium phase, non-equilibrium phase, phase that has an important influence on the performance, and phase that has an important influence on the process are determined through thermodynamic calculations. The factor that has an important influence on the performance in the material is determined to be the duplex ratio of duplex stainless steel. The duplex ratio is the ratio of the equilibrium phase to the non-equilibrium phase. The duplex ratio is selected as 1:1. The factor that has an important influence on the process is determined to be the brittle phase. Through thermodynamic calculations, based on the composition range of the material specified in the standard, the influence of each material on the duplex ratio, brittle phase and material strength is obtained. The materials are determined to be Fe, C, Si, Mn, P, S, Cr, Ni, Mo and N.
[0058] The material composition is determined by comprehensively considering the material properties, the ratio of the two phases and the precipitation control of the brittle phase. The screening targets are a two phase ratio of 1:1 and avoiding the precipitation of the brittle phase. Through thermodynamic calculation, the material composition of the duplex stainless steel forgings is determined to be C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr22.00-23.00%, Ni 4.50-5.50%, Mo 2.50-3.50% and N0.08-0.20% by weight, and the rest is Fe.
[0059] In this embodiment, a rapid process for designing large duplex stainless steel forging materials is provided based on material thermodynamic calculations, finite element simulations, and a small number of verification tests; based on material thermodynamic calculations, a preliminary evaluation of the material is performed to determine the important factors affecting the performance of the forging, including brittle phase structure, phase ratio, etc.; based on the thermodynamics and kinetics of brittle phase precipitation, and the control of phase ratio, the optimal composition range of the material is determined, so that the laboratory results are closer to the results of large forging products, providing a rapid development path for large duplex stainless steel forgings, reducing the amount of testing, omitting the test piece verification step, shortening the product development cycle, and improving the market competitiveness of the enterprise. At the same time, within a wider range of standard material composition, according to actual working conditions, a narrower range of composition that is more suitable for working conditions and processes is obtained, thereby improving the stability of product performance.
[0060] In this embodiment, the optimal composition range of the material is determined, so that the laboratory results are closer to the results of large forging products, providing a rapid development path for large duplex stainless steel forgings, reducing the amount of testing, omitting the test piece verification step, shortening the product development cycle, and improving the market competitiveness of the enterprise. At the same time, within a wider range of material standard composition, according to actual working conditions, a narrower range of composition that is more suitable for working conditions and processes is obtained, thereby improving the stability of product performance.
[0061] The embodiment of the present invention provides a duplex stainless steel forging, which is designed and manufactured by the composition design method of the duplex stainless steel forging as described in any one of the above items. The obtained duplex stainless steel forging includes, by weight, C 0.01-0.03%, Si 0.4-0.5%, Mn 1.0-1.5%, P≤0.025%, S≤0.003%, Cr 22.00-23.00%, Ni 4.50-5.50%, Mo 2.50-3.50% and N 0.08-0.20%, and the rest is Fe.
[0062] The present invention is further described below in conjunction with specific embodiments.
[0063] Embodiment 1, as Figure 1 As shown, for The manufacturing process design of F51 duplex stainless steel liquid ring sliding forgings (ring forgings) requires that the material has a minimum yield strength of 450 MPa and a minimum tensile strength of 620 MPa. The composition design method and the process design method of the present invention are applied, and the steps are as follows:
[0064] Step 1: Calculation of operating condition limits.
[0065] According to user requirements, preliminarily design the rough machining dimensions of the workpiece.
[0066] Since the product requires high strength, the commonly used cooling method for this material (water cooling) is initially considered for the final performance heat treatment.
[0067] Finite element method was used to calculate that under actual water-cooling quenching conditions, the cooling rate that can be achieved at the slowest cooling point of the workpiece (at the T / 2 thickness of the workpiece) is 38°C / min.
[0068] Step 2: Materials evaluation.
[0069] Through thermodynamic calculation and literature evaluation, the equilibrium phase and non-equilibrium phase of the material, the phase that has an important influence on the performance, and the phase that has an important influence on the process are determined. The factor that has an impact on the performance of the material is the dual-phase ratio. When the dual-phase ratio is 1:1, the comprehensive performance of the material is the best. The factor that has an important impact on the process is the brittle phase (σ phase);
[0070] Through thermodynamic calculation software, based on the composition range specified in the standard, the influence of each element content on the dual-phase ratio is calculated as follows: Ni, Mn, and N are austenite stabilizing elements, which play a role in expanding the austenite region, and the solid solution strengthening of N improves the yield, and Mn promotes the solid solution strengthening of N;
[0071] Through thermodynamic calculation software, based on the composition range specified in the standard, the influence of each element content on the precipitation of σ phase is calculated: Mo and Cr elements promote the precipitation of σ phase, especially Mo element has a significant effect on its precipitation, and Mn and C elements have little effect on the precipitation of σ phase within the standard composition range;
[0072] Through thermodynamic calculation software, based on the composition range specified in the standard, the influence of each element content on material strength is calculated as follows: the material strength increases with the increase of ferrite phase proportion, Mn can increase the limit solid solubility of N in steel, and can be used in combination with N to improve the strength of the material, but the S content needs to be controlled to avoid the formation of MnS;
[0073] Step 3: Determine the target component.
[0074] Comprehensively considering the material properties, the ratio of two phases and the precipitation control of the σ phase, the composition optimization target is determined as follows: the Cr element takes the middle upper limit, the Mo element takes the middle lower limit, the Ni element takes the middle lower limit, the N element takes the middle upper limit, the Mn element takes the middle limit, the C element takes the middle upper limit, and the S element takes the currently achievable process lower limit, thereby determining the internal control composition range;
[0075] The screening targets were to set the dual-phase ratio at 1:1 and to avoid precipitation of σ phase as much as possible, and the composition design was performed using material thermodynamic calculation software, as shown in Table 1, where the internal control was the optional range of the material composition obtained in this embodiment.
[0076] Table 1 Material composition design table
[0077]
[0078] Step 4: Process analysis.
[0079] The equilibrium precipitation temperature range of the σ phase in the material is calculated by the material thermodynamic calculation software to be 600-950°C, so it is determined that the final forging temperature of the material cannot be lower than 950°C;
[0080] The material rheological stress curve and recrystallization model were obtained through material calculation, and the forging temperature range was determined to be 950-1300℃;
[0081] The precipitation kinetics of the σ phase at the slowest cooling rate limited by the working conditions was calculated by the material thermodynamic calculation software. The results showed that the σ phase precipitated faster in the range of 930-800℃, and the precipitation amount was about 0.3% at 100s. The residence time of the product workpiece at T / 2 thickness in the range of 930-800℃ was about 100s during the cooling process. Therefore, the σ phase content produced during the heat treatment quenching cooling process may also be around 0.3%, which will not have a significant impact on the performance. Therefore, water cooling can be used as the cooling method for performance heat treatment;
[0082] The influence of solution temperature on the precipitation of σ phase and the ratio of the two phases was calculated by material thermodynamic calculation software. The results showed that the solution temperature had no significant effect on the precipitation of σ phase during the cooling process, but with the increase of solution temperature, the ferrite content increased. When the solution temperature was around 1100℃, the contents of the two phases were close. Therefore, 1100℃ was determined as the target temperature of the solution temperature.
[0083] The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process was carried out by finite element simulation software to obtain the heat treatment temperature curve at the workpiece sampling point;
[0084] Establish forging model in finite element simulation software, including: establishing geometric model, dividing mesh, setting material parameters, setting boundary conditions, and submitting calculation;
[0085] Based on the simulation calculation results, in the simulation post-processing module, the curve of the temperature change of the forging at the sampling position over time is extracted, and the average cooling rate is calculated, which is about 60°C / min.
[0086] The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process was carried out using finite element simulation software to obtain the heat treatment deformation trend of the workpiece.
[0087] Establish forging model in finite element simulation software, including: establishing geometric model, dividing mesh, setting material parameters, setting boundary conditions, and submitting calculation;
[0088] Based on the simulation calculation results, the displacement field cloud diagram of the forging after heat treatment is extracted in the simulation post-processing module, such as Figure 3 As shown;
[0089] Observe the deformation trend and deformation amount of forgings after heat treatment, such as Figure 3As shown in the figure, the displacement field of the forging after heat treatment, the negative number in the legend is shrinkage, it can be seen that the workpiece is in a shrinkage state after heat treatment, and the shrinkage of the inner wall is greater than that of the outer wall. The results show that the deformation trend of the workpiece during the heat treatment process is inward contraction, and the shrinkage of the inner wall is greater than that of the outer wall, which is completely different from the deformation trend of ordinary steel (steel types that undergo phase change during the thermal process) forgings that expand outward. Therefore, when designing the process, consideration should be given to leaving a margin on the outer wall of the ring forging. This is completely different from the deformation trend of ordinary steel (steel types that undergo phase change during the thermal process) forgings that expand outward. Therefore, when designing the process, consideration should be given to leaving a margin on the outer wall of the ring forging.
[0090] According to the deformation trend and deformation amount of heat treatment, the rough processing size requirements of forgings that can meet the product size requirements before deformation are reversed;
[0091] Determine the forging size requirements based on the forging rough machining size requirements;
[0092] Determine the size of the steel ingot according to the forging size requirements.
[0093] Step 5: Process design.
[0094] Obtain raw materials according to the alloy ratio shown in step 3, and smelt the raw materials to obtain steel ingots;
[0095] According to the conclusions obtained in step 4, design the forging blanking size and the workpiece size after forging;
[0096] According to the conclusion obtained in step 4, the forging process is determined, the initial forging temperature is 1150-1300℃, and the final forging temperature is 950-1050℃; if cracking occurs, it must be promptly heat-cleaned at above 950℃. The obtained forging blank is forged to obtain a ring-shaped blank forging;
[0097] Specifically, after blanking and drawing, forging is performed by using deformation methods such as roughing, punching, pre-expansion of a horse bar, and expansion;
[0098] According to the conclusion obtained in step 4, the heat treatment process design is carried out: the homogenization temperature is 1000-1100℃, the holding time is 10-15h, and the cooling method is water cooling.
[0099] Step 6: Physical simulation.
[0100] Refining small steel ingots according to the composition range in step 3; retesting the composition of the refined small steel ingots;
[0101] The small steel ingots obtained by refining are forged; the samples obtained by forging are cut and subjected to physical simulation heat treatment in the heat treatment furnace in step 4; the obtained samples are tested for performance to determine whether they meet the product performance requirements. The results show that the material properties meet the product performance requirements.
[0102] Step 7: Product production.
[0103] The process described in step 5 is used to carry out production, and sampling and testing are carried out according to user requirements, and the performance test is qualified.
[0104] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A process design method for duplex stainless steel forgings, characterized in that: The following steps are involved: S1: Through material thermodynamic calculation, it is obtained that the equilibrium precipitation temperature range of the brittle phase in the material component of duplex stainless steel is 600-950°C, and it is determined that the final forging temperature of the material component cannot be lower than 950°C; S2: obtaining the flow stress curve and recrystallization model of the material components through material calculation, and determining the forging temperature range to be 950-1300°C; S3: The precipitation kinetics of the brittle phase at the slowest cooling rate limited by the working conditions is obtained through material thermodynamic calculation, and water cooling is determined to be used as the cooling method for performance heat treatment; S4: Calculate the influence of the solid solution temperature on the precipitation of the brittle phase and the ratio of the two phases through material thermodynamics, and determine the target temperature of the solid solution temperature; S5: The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is performed by finite element simulation software to obtain the heat treatment temperature curve at the workpiece sampling point; S6: The temperature-structure-stress three-field coupling simulation calculation of the forging heat treatment process is carried out through finite element simulation software to obtain the heat treatment deformation trend of the workpiece and determine the margin left on the outer wall of the workpiece during process design.
2. The process design method for duplex stainless steel forgings according to claim 1, characterized in that: The method also includes step S0: determining the working conditions, determining the heat treatment and water-cooling quenching methods according to the size of the workpiece, and calculating by finite element simulation software the cooling rate that can be achieved at the slowest cooling point of the workpiece during the water-cooling quenching.
3. The process design method for duplex stainless steel forgings according to claim 1, characterized in that: According to step S1 and step S2, the initial forging temperature of the forging method is designed to be 1100-1300°C, and the final forging temperature is designed to be 950-1050°C.
4. The process design method for duplex stainless steel forgings according to claim 1, characterized in that: According to step S2, step S3 and step S4, it is determined that the homogenization temperature of the heat treatment method is designed to be 1000-1100°C, the insulation time is designed to be 10-15h, and the cooling method is designed to be water cooling.
5. The process design method for duplex stainless steel forgings according to claim 1, characterized in that: The target temperature of the solution temperature in step S4 is 1100°C.
6. The process design method for duplex stainless steel forgings according to claim 1, characterized in that: S5: performing temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process through finite element simulation software, specifically including: establishing a geometric model, dividing a grid, setting material parameters, setting boundary conditions and submitting calculations, and obtaining a heat treatment temperature curve at a workpiece sampling position based on the simulation calculation results.
7. The process design method for duplex stainless steel forgings according to claim 6, characterized in that: The heat treatment temperature curve of the workpiece at the sampling position was extracted, and the average cooling rate was calculated to be 60° C. / min.
8. The process design method for duplex stainless steel forgings according to claim 1, characterized in that: The S6: after performing temperature-structure-stress three-field coupled simulation calculation on the forging heat treatment process by finite element simulation software, it also includes: based on the simulation calculation results, in the simulation post-processing module, extracting the displacement field cloud map of the workpiece after the heat treatment, observing the deformation trend and deformation amount of the workpiece after the heat treatment, and determining whether to leave a margin on the outer wall of the workpiece when performing process design.
9. The process design method for duplex stainless steel forgings according to claim 1, characterized in that: The method further includes step S7: simulating forging, refining steel ingots, and forging the steel ingots.
10. The process design method for duplex stainless steel forgings according to claim 9, characterized in that: The method further comprises step S8: performance testing, in which the steel ingot obtained in step S7 is subjected to performance testing.
Citation Information
Patent Citations
Heat treatment method for ferrite-austenite duplex stainless steel
CN114107631A
Method for optimizing performance of duplex stainless steel
CN114959223A
Heat treatment deformation control method for thin-wall circular ring type part based on simulation prediction
CN115029544A
Duplex stainless steel forging and its manufacturing method
JP2022152427A
Cited By
Erittlement temperature control processing method and system for duplex stainless steel pipe fitting
CN121137326A