Power VDMOS manufacturing method capable of reducing EMI

By optimizing the parameters and structure of the power VDMOS device, the EMI problem generated during the switching process is solved, the electromagnetic compatibility is improved, and the EMI noise is reduced.

CN119028822AActive Publication Date: 2024-11-2658TH RES INST OF CETC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411152653.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The electromagnetic interference (EMI) problems generated by power VDMOS devices during switching, resulting in complexity of the electromagnetic environment and affecting the power grid and surrounding environment.

Method used

By optimizing device parameters Cgs and Rg, new structures and processes are adopted to design new devices, including the formation of multi-layer conductivity type well regions, heavily doped regions and contact regions, and the use of high dielectric constant silicon nitride material to adjust gate oxygen thickness and impurity concentration, reduce di/dt and dv/dt, form MOM capacitance, and optimize EMI noise.

Benefits of technology

It effectively reduces the EMI noise of power VDMOS devices, optimizes its electromagnetic compatibility, and reduces the oscillation amplitude and oscillation gentleness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028822A_ABST
    Figure CN119028822A_ABST
Patent Text Reader

Abstract

The invention discloses a power VDMOS manufacturing method capable of reducing EMI, and belongs to the field of semiconductor devices. Providing a silicon wafer material, and forming a first conductive type well region, a fourth dielectric oxide layer field oxide, a second conductive type source end heavily doped region and a first conductive type heavily doped body contact region on the silicon wafer; forming a first dielectric oxide layer gate oxide through furnace tube thermal oxidation; carrying out LPCVD (Low Pressure Chemical Vapor Deposition) twice to deposit polycrystals, and carrying out high-temperature annealing to activate impurities to form a gate polycrystalline silicon electrode; wherein the thickness of the polycrystal deposited for the second time is larger than that of the polycrystal deposited for the first time; siO2 is deposited, and a second dielectric oxide layer is formed; depositing SiN by plasma enhanced chemical vapor deposition to form a third dielectric high-K material; and finally, sequentially forming an ohmic contact hole, a source electrode and a drain electrode. By designing a new device structure and a new process, device parameters Cgs and Rg are optimized, di / dt and dv / dt of the power VDMOS are reduced, and EMI noise optimization is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a method for manufacturing a power VDMOS capable of reducing EMI. Background Art

[0002] The continuous improvement of power capacity and power density of modern electronic equipment has led to an increasingly complex internal electromagnetic environment, and the electromagnetic interference (EMI) generated by itself has an increasingly serious impact on the power grid and its surrounding electromagnetic environment. As the power switch tube of the switching power supply, the power VDMOS works in a fast on-off cycle conversion state. The voltage and current on the power switch tube are changing rapidly, which is the main interference source of electric field coupling and magnetic field coupling, and is one of the main sources of EMI of the switching power supply.

[0003] The di / dt and dv / dt generated by the power VDMOS device during the switching process generate EMI transient noise through the parasitic capacitance and parasitic inductance in the circuit. In the gate drive loop of the VDMOS, the internal parasitic gate resistance R g , Gate lead inductance L g And the gate-source parasitic capacitance C gs An RLC series resonant circuit is formed between them. For a series resonant circuit, its quality factor Q = ωL g / R g =(ωR g C gs ) -1 The smaller the Q, the worse the frequency selection characteristics, the smaller the oscillation amplitude, and the smoother the subsequent oscillation. Therefore, the smaller the parasitic gate inductance in the RLC resonant circuit, the larger the gate resistance, and the larger the gate-source capacitance, the smoother the gate drive signal (gate voltage) oscillation. g It is related to the parasitic inductance of the gate bonding wire itself, R g It is related to the doping concentration of the polysilicon gate and the gate routing. gs It is mainly determined by the capacitance between the polysilicon gate and the N+ source, P-type base region, and source metal. Summary of the invention

[0004] The object of the present invention is to provide a method for manufacturing a power VDMOS with reduced EMI, so as to solve the problem of EMI generated by the power VDMOS during the switching process.

[0005] In order to solve the above technical problems, the present invention provides a method for manufacturing a power VDMOS with reduced EMI, comprising:

[0006] Step 1: Provide silicon wafer materials. The silicon wafer materials are n from bottom to top. + Silicon substrate, n buffer layer and n -Epitaxial layer;

[0007] Step 2: forming a first conductivity type well region on a silicon wafer;

[0008] Step 3: deposit SiO2, apply photoresist and expose the pattern window, wet etch SiO2, remove the photoresist, and form the fourth dielectric oxide layer field oxygen;

[0009] Step 4: forming a second conductivity type source end heavily doped region on the first conductivity type well region;

[0010] Step 5: forming a first conductivity type heavily doped body contact region on the first conductivity type well region;

[0011] Step 6: thermal oxidation of the furnace tube to form a first dielectric oxide layer gate oxide;

[0012] Step 7: performing LPCVD deposition of polycrystalline twice, performing high temperature annealing to activate impurities, coating photoresist and exposing a pattern window, etching the polycrystalline, removing the photoresist, and forming a gate polysilicon electrode; wherein the thickness of the polycrystalline deposited the second time is greater than that of the first time;

[0013] Step 8: Plasma enhanced chemical vapor deposition deposits SiO2 to form a second dielectric oxide layer; plasma enhanced chemical vapor deposition deposits SiN to form a third dielectric high-K material;

[0014] Step nine: coating photoresist and exposing a graphic window, dry etching SiN and SiO2, removing the photoresist, and forming an ohmic contact hole; depositing metal, coating photoresist and exposing a graphic window, performing metal corrosion, removing the photoresist, and forming a source electrode;

[0015] Step 10: Thin the silicon wafer and sputter metal TiNiAg on the back to form a drain.

[0016] In one embodiment, the n + The resistivity of the silicon substrate is 0.002-0.004Ω·cm; the resistivity of the n buffer layer is 0.5Ω·cm and the thickness is 10μm; the n - The resistivity of the epitaxial layer is 9Ω·cm and the thickness is 45μm.

[0017] In one embodiment, the step 2 includes: coating a photoresist and exposing a pattern window, implanting boron ions with an implantation energy of 100 keV and an implantation dose of 5×10 13 cm -2 , remove the photoresist; and perform push-in junction at a temperature of 1150° C. for 200 minutes to form a first conductive type well region.

[0018] In one embodiment, the step 4 includes: coating a photoresist and exposing a pattern window, implanting phosphorus ions with an implantation energy of 100 keV and an implantation dose of 5×10 15 cm -2 , remove the photoresist, and perform push-in at a temperature of 900° C. for 30 minutes to form a heavily doped region of the second conductive type source end.

[0019] In one embodiment, the step five includes: coating a photoresist and exposing a pattern window, implanting boron ions with an implantation energy of 45 keV and an implantation dose of 5×10 15 cm -2 , remove the photoresist, and perform push-conduction at a temperature of 900° C. for 30 minutes to form a first conductivity type heavily doped body contact region.

[0020] In one embodiment, in step 7, the first LPCVD polycrystalline is deposited to a thickness of 150 nm, and phosphorus ions are implanted at an implantation energy of 45 keV and an implantation dose of 5×10 15 cm -2 The second LPCVD deposition of polycrystalline with a thickness of 650nm was performed, and phosphorus ions were implanted with an injection energy of 45keV and an injection dose of 5×10 15 cm -2 .

[0021] The present invention provides a method for manufacturing a power VDMOS with reduced EMI, which optimizes the device parameters C by designing a new device structure and a new process. gs , Rg, reduce the di / dt and dv / dt of the power VDMOS and achieve EMI noise optimization. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a cross-sectional view of a cell in a specific implementation mode;

[0023] Figure 2 is a top view and a cross-sectional view of a field region polycrystalline gate connection line in a specific implementation manner;

[0024] Figure 3 Schematic diagram of secondary polycrystalline deposition doping in a specific implementation manner.

[0025] 11 is the first conductivity type well region of the cell region, 12 is the first conductivity type heavily doped body contact region; 21 is the second conductivity type substrate, 22 is the second conductivity type buffer layer, 23 is the second conductivity type drift region, 24 is the second conductivity type source end heavily doped region; 31 is the first dielectric oxide layer gate oxide, 32 is the second dielectric oxide layer, 33 is the third dielectric high-K material, 34 is the fourth dielectric oxide layer field oxide; 41 is the gate polysilicon electrode, which is divided into two layers, 41-1 is the first layer of polycrystalline, 41-2 is the second layer of polycrystalline; 51 is the source metal, and 52 is the drain metal. DETAILED DESCRIPTION

[0026] The following is a further detailed description of a power VDMOS manufacturing method for reducing EMI proposed by the present invention in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become clearer according to the following description. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0027] In the composition C gs Among the several parts, the capacitance between the polysilicon gate and the N+ source and P-type base is mainly determined by the gate oxide thickness and impurity concentration, and the gate oxide thickness and impurity concentration have an impact on the normal characteristics of VDMOS, so adjusting the gate oxide thickness and impurity concentration will destroy the original characteristics of the device; the capacitance between the polysilicon gate and the source metal is mainly determined by the dielectric material and dielectric thickness, and the dielectric between the gate polycrystalline and the source metal has no effect on the normal characteristics of VDMOS and can be used to adjust the gate-source capacitance.

[0028] Similarly, the adjustment of Rg cannot deteriorate other device parameters, which requires that while adjusting Rg, the polycrystalline gate work function and polycrystalline-metal contact resistance must be kept unchanged.

[0029] The low EMI power VDMOS manufacturing method provided by the present invention optimizes the device parameters C by designing a new device structure and a new process flow. gs , Rg, reduce the di / dt and dv / dt of the power VDMOS and achieve EMI noise optimization.

[0030] The present invention is used to control C gs And the methods of Rg are:

[0031] 1) Improve the dielectric constant of the dielectric layer between the polysilicon gate and the source metal, use a composite dielectric layer, and replace silicon oxide with silicon nitride with a higher dielectric constant;

[0032] 2) The polysilicon gate is deposited and doped twice, so that the upper and lower surfaces of the polycrystalline layer are highly doped and the middle layer is low doped;

[0033] 3) A groove is made on the polycrystalline gate connection GateBus in the field area to form a MOM capacitor between the polycrystalline sidewall and the source metal sidewall.

[0034] The present invention provides a method for manufacturing a power VDMOS with reduced EMI. Figure 1 to Figure 3 ,in Figure 1 is a cross-section of a cell. Figure 2 It is the top view and cross-sectional view of the field area polycrystalline gate connection. Figure 3 Schematic diagram of secondary polycrystalline deposition doping, the manufacturing method includes the following steps:

[0035] Step 1: Provide silicon wafer materials. The silicon wafer materials are n from bottom to top. + Silicon substrate 21, n buffer layer 22 and n-epitaxial layer 23; wherein n + The resistivity of the silicon substrate 21 is 0.002-0.004Ω·cm; the resistivity of the n buffer layer 22 is 0.5Ω·cm and the thickness is 10μm; - The resistivity of the epitaxial layer 23 is 9Ω·cm and the thickness is 45μm;

[0036] Step 2: Coat photoresist on the silicon wafer and expose the pattern window, then implant boron ions with an injection energy of 100 keV and an injection dose of 5×10 13 cm -2 , remove the photoresist. Perform push-in junction at a temperature of 1150° C. for 200 minutes to form a first conductive type well region 11;

[0037] Step 3: LPCVD deposits SiO2 with a thickness of 800nm. Coat photoresist and expose the pattern window, wet etch SiO2, remove the photoresist, and form the fourth dielectric oxide layer field oxygen 34;

[0038] Step 4: Apply photoresist and expose the pattern window, and then implant phosphorus ions with an injection energy of 100 keV and an injection dose of 5×10 15 cm -2 , removing the photoresist, and performing a push-in junction at a temperature of 900° C. for 30 minutes to form a second conductivity type source-end heavily doped region 24;

[0039] Step 5: Apply photoresist and expose the pattern window, and implant boron ions with an injection energy of 45keV and an injection dose of 5×10 15 cm -2 , removing the photoresist, and performing a push-in process at a temperature of 900° C. for 30 minutes to form a first conductivity type heavily doped body contact region 12;

[0040] Step 6: thermal oxidation of the furnace tube, the oxide layer thickness is 100nm, and the first dielectric oxide layer gate oxide 31 is formed;

[0041] Step 7: The first LPCVD polycrystalline is deposited with a thickness of 150nm, and phosphorus ions are implanted with an injection energy of 45keV and an injection dose of 5×10 15 cm -2 The second LPCVD deposition of polycrystalline with a thickness of 650nm was performed, and phosphorus ions were implanted with an injection energy of 45keV and an injection dose of 5×10 15 cm -2 , annealing is performed at 850°C for 30 minutes to activate the impurities. Photoresist is applied and a pattern window is exposed, polycrystalline is etched, photoresist is removed, and gate polysilicon electrode 41 is formed. The schematic diagram of secondary polycrystalline deposition and implantation doping is shown in FIG. Figure 3 As shown;

[0042] In step 7, the increase in polycrystalline thickness will increase the sidewall capacitance and reduce the polycrystalline gate resistance, and the reduction in resistance will increase the quality factor; the increase in doping concentration will reduce the polycrystalline gate resistance, which will also increase the quality factor. Therefore, it is necessary to design the polycrystalline thickness and doping so that it can reduce the quality factor without affecting the polycrystalline work function and the ohmic contact between polycrystalline and metal. The present invention uses two-step polycrystalline deposition and implantation. The first step polycrystalline thickness is relatively small, 100nm to 200nm, and the implantation dose is 3×10 15 cm -2 ~1×10 16 cm -2 After doping, the impurity concentration of the polycrystalline-gate oxide interface is high, which ensures the work function of the gate polycrystalline. In the second step, the polycrystalline thickness is relatively large, ranging from 500nm to 1000nm, and the implantation dose is 3×10 15 cm -2 ~1×10 16 cm -2 After the injection of doping, the surface concentration of the polycrystal is higher, which ensures the ohmic contact between the polycrystal and the metal. The middle part of the second layer of polycrystal is relatively low in doping, which is used to adjust the gate resistance Rg.

[0043] Step 8: PECVD deposits SiO2 with a thickness of 100nm to form a second dielectric oxide layer 32; PECVD deposits SiN with a thickness of 100nm to form a third dielectric high-K material 33. The dielectric isolation diagram of the polycrystalline gate-source metal on the gate connection line is shown in Figure 2 As shown;

[0044] In step 8, the isolation between polycrystalline and metal in the conventional process uses USG (undoped silicon glass) and BPSG (boron-phosphorus doped silicon glass), wherein BPSG has a low breakdown field strength but has certain reflow characteristics, while the dielectric constant and breakdown field strength of silicon nitride are higher than BPSG. The present invention uses a single layer of metal, so the isolation medium uses USG+SiN.

[0045] The size of the groove on the field region polycrystalline gate connection GateBus and the width of the groove are determined by the polycrystalline thickness and the second dielectric oxide layer 32 and the third dielectric high-K material 33, so as to better form the MOM capacitor between the polycrystalline sidewall and the source metal sidewall.

[0046] Step 9: coating photoresist and exposing a graphic window, dry etching SiN and SiO2, removing the photoresist, and forming an ohmic contact hole; depositing metal with a thickness of 5 μm, coating photoresist and exposing a graphic window, performing metal corrosion, removing the photoresist, and forming a source 51;

[0047] Step 10: The silicon wafer is thinned to 250 μm, and metal TiNiAg is sputtered on the back with a thickness of 2 μm to form a drain 52 .

[0048] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A method for manufacturing a power VDMOS for reducing EMI, characterized in that: include: Step 1: Provide silicon wafer materials. The silicon wafer materials are n from bottom to top. + A silicon substrate (21), an n buffer layer (22) and an n - epitaxial layer (23); Step 2: forming a first conductivity type well region (11) on a silicon wafer; Step 3: depositing SiO2, coating photoresist and exposing a pattern window, wet etching SiO2, removing the photoresist, and forming a fourth dielectric oxide layer field oxygen (34); Step 4: forming a second conductivity type source end heavily doped region (24) on the first conductivity type well region (11); Step 5: forming a first conductivity type heavily doped body contact region (12) on the first conductivity type well region (11); Step 6: thermally oxidizing the furnace tube to form a first dielectric oxide layer gate oxide (31); Step 7: performing LPCVD deposition of polycrystalline twice, performing high temperature annealing to activate impurities, coating photoresist and exposing a pattern window, etching the polycrystalline, removing the photoresist, and forming a gate polycrystalline silicon electrode (41); wherein the thickness of the polycrystalline deposited the second time is greater than that of the first time; Step 8: Plasma enhanced chemical vapor deposition deposits SiO2 to form a second dielectric oxide layer (32); plasma enhanced chemical vapor deposition deposits SiN to form a third dielectric high-K material (33); Step nine: coating photoresist and exposing a pattern window, dry etching SiN and SiO2, removing the photoresist, and forming an ohmic contact hole; depositing metal, coating photoresist and exposing a pattern window, performing metal etching, removing the photoresist, and forming a source electrode (51); Step 10: Thin the silicon wafer and sputter metal TiNiAg on the back to form a drain (52).

2. The method for manufacturing a power VDMOS with reduced EMI as claimed in claim 1, characterized in that: The + The resistivity of the silicon substrate (21) is 0.002-0.004Ω·cm; the resistivity of the n buffer layer (22) is 0.5Ω·cm and the thickness is 10μm; - The resistivity of the epitaxial layer (23) is 9Ω·cm and the thickness is 45μm.

3. The method for manufacturing a power VDMOS with reduced EMI as claimed in claim 1, characterized in that: The second step includes: coating photoresist and exposing a pattern window, injecting boron ions with an injection energy of 100 keV and an injection dose of 5×10 13 cm -2 , removing the photoresist; and performing push-in at a temperature of 1150° C. for 200 minutes to form a first conductive type well region (11).

4. The method for manufacturing a power VDMOS with reduced EMI as claimed in claim 1, characterized in that: The fourth step includes: coating photoresist and exposing a pattern window, injecting phosphorus ions with an injection energy of 100 keV and an injection dose of 5×10 15 cm -2 , remove the photoresist, and perform push-in at a temperature of 900° C. for 30 minutes to form a second conductivity type source-end heavily doped region (24).

5. The method for manufacturing a power VDMOS with reduced EMI as claimed in claim 1, wherein: The step five comprises: coating a photoresist and exposing a pattern window, implanting boron ions with an implantation energy of 45 keV and an implantation dose of 5×10 15 cm -2 , remove the photoresist, and perform push-connection at a temperature of 900° C. for 30 minutes to form a first conductivity type heavily doped body contact region (12).

6. The method for manufacturing a power VDMOS with reduced EMI as claimed in claim 1, characterized in that: In step 7, the first LPCVD polycrystalline is deposited to a thickness of 150 nm, and phosphorus ions are implanted at an injection energy of 45 keV and an injection dose of 5×10 15 cm -2 ; The second LPCVD deposition of polycrystalline with a thickness of 650nm was performed, and phosphorus ions were implanted with an injection energy of 45keV and an injection dose of 5×10 15 cm -2 .

Citation Information

Patent Citations

  • Field effect device, anti-fuse, random number generating device

    CN109075203A

  • Power semiconductor MOS device and method for fabricating same

    CN109728097A

  • Low-EMI deep trench isolation trench type power semiconductor device and preparation method thereof

    CN110600454A

  • Anti-radiation VDMOS device manufacturing method capable of reducing surface electric field

    CN116959990A

  • VDMOS field effect transistor with low EMI