Silicon-based gallium nitride SBD device and preparation method thereof

By adopting nested rounded square ring structure and interlaced distribution metal design in silicon-based gallium nitride SBD devices, the current edge collection effect is solved, the uniform increase in current density and VF are achieved, and the breakdown is improved. Voltage.

CN119029014APending Publication Date: 2024-11-26YANGZHOU GUOYU ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411138471.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Conventional silicon-based gallium nitride SBD devices have a current edge collection effect, resulting in high forward current density and low intermediate current density, making it difficult to take into account both low VF and high current density.

Method used

Using a nested rounded square ring structure, by etching the nested rounded square ring window on the N-gallium nitride drift region, an interlaced cathode and anode metal is formed, and the number of rounded square rings is increased to expand the active Area area, reduce the VF of the device, and avoid electric field congestion through arc-shaped corner design.

Benefits of technology

A uniform increase in overall current density and reduction in VF are achieved, while increasing the breakdown voltage of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029014A_ABST
    Figure CN119029014A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon-based gallium nitride SBD device and a preparation method thereof in the technical field of power semiconductor devices. The device comprises a silicon substrate from bottom to top; an AlN / AlGaN buffer layer; an N + gallium nitride transmission layer; the N-gallium nitride drift region is provided with a window etched to the nested rounded square rings of the transmission layer, and the nested rounded square rings are a plurality of rounded square rings which are sequentially enlarged in inner diameter and are arranged at intervals in a sleeving manner; the cathode metal is arranged on the transmission layer; the ion implantation region is arranged on the upper edge and the side wall of the drift region; the anode metal is arranged on the drift region to form Schottky contact; and the dielectric layer is arranged on the upper surface of the exposed transmission layer and the upper surface and the side wall of the exposed drift region. Current distribution below each ring of anode metal of the nested rounded square ring structure of the device is uniform, a larger active region area can be obtained by increasing the number of rounded square rings, and the effects of uniformly improving the overall current density and reducing the VF of the device are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of power semiconductor devices, and in particular to a silicon-based gallium nitride SBD device and a preparation method thereof. Background Art

[0002] The core of power electronics is energy conversion devices based on semiconductor materials. With the continuous maturity and development of the first generation of semiconductor silicon, the performance of the devices has gradually approached the theoretical limit. In order to achieve higher power density, the third generation semiconductor GaN has attracted attention due to its higher BFOM value and lower on-resistance at the same breakdown voltage. The full vertical structure of gallium nitride is expensive and not conducive to commercialization. Silicon-based gallium nitride devices compatible with silicon processes have emerged. Among them, the lateral structure HEMT has achieved a high-frequency switching ratio at 650V, but there is a current collapse effect and serious heat generation in the 2DEG channel. Quasi-vertical silicon-based gallium nitride has the advantages of both. While being low-cost, the longitudinal structure can withstand voltage, and the distribution of current in the material body and the influence of surface states are greatly reduced.

[0003] Conventional quasi-vertical silicon-based gallium nitride SBD devices use a circular anode metal design. When a forward voltage is applied, the current is mainly concentrated at the edge of the anode metal, and the current density in the middle area is low; this makes it not an economically feasible solution to reduce VF by increasing the cell area; and although reducing the cell area can effectively increase the overall current density, it will make the device unable to work in a high current mode. Therefore, based on the current design method, it is difficult to take both low VF and high current density into account, which seriously restricts the application of silicon-based gallium nitride SBD devices in the field of power semiconductors. Summary of the invention

[0004] The present application provides a silicon-based gallium nitride SBD device and a preparation method thereof, thereby solving the problem in the prior art that the conventional silicon-based gallium nitride SBD device has a serious current edge effect, resulting in a high forward current density at the anode metal edge of the device and a low current density in the middle, thereby achieving the effect of uniformly improving the overall current density and reducing the VF of the device.

[0005] The embodiment of the present application provides a silicon-based gallium nitride SBD device, including:

[0006] Silicon substrate;

[0007] An AlN / AlGaN buffer layer is disposed on the silicon substrate;

[0008] An N+ gallium nitride transmission layer is disposed on the AlN / AlGaN buffer layer and serves as a current transmission carrier;

[0009] An N-GaN drift region is disposed on the N+GaN transport layer, and a nested rounded square ring window etched to the N+GaN transport layer is opened on the N-GaN drift region, and the nested rounded square ring is a plurality of rounded square rings with successively increasing inner diameters and spaced apart;

[0010] A cathode metal is disposed on the N+ gallium nitride transmission layer exposed in the nested rounded square ring window to form an ohmic contact;

[0011] An ion implantation region, arranged at the upper edge and sidewall of the N-gallium nitride drift region;

[0012] An anode metal is disposed on the N-gallium nitride drift region, and the anode metal forms a Schottky contact with the N-gallium nitride drift region into which ions are not implanted;

[0013] The dielectric layer is disposed on the exposed upper surface of the N+ gallium nitride transmission layer and the exposed upper surface and sidewall of the N- gallium nitride drift region.

[0014] The beneficial effects of the above-mentioned embodiments are as follows: compared with the general circular structure, the nested rounded square ring structure solves the problem of the difficulty in balancing the device size and the forward current density. The staggered distribution of the cathode and anode makes the current distribution under each ring of the anode metal uniform, and a larger active area can be obtained by increasing the number of rounded square rings, thereby reducing the VF, achieving the effect of uniformly improving the overall current density and reducing the VF of the device; at the same time, since the above-mentioned square rings are all rounded, the connection corners of the cathode and anode metals are all arc-shaped designs rather than simple straight-line connections, thereby avoiding electric field crowding, and the space charge region at the corner is converted from a spherical junction to a cylindrical junction, and the maximum electric field strength at the edge is reduced, thereby increasing the device breakdown voltage.

[0015] Based on the above embodiments, the present application can be further improved as follows:

[0016] In one of the embodiments of the present application, the N+ gallium nitride transmission layer is a heavily doped region with a resistivity of 0.001 to 0.005 Ω·cm and a thickness of 2 to 4 μm.

[0017] In one of the embodiments of the present application, the N-gallium nitride drift region is a lightly doped region doped with Si atoms, has a resistivity of 1 to 20 Ω·cm, and a thickness of 1 to 5 μm.

[0018] In one embodiment of the present application, the nested rounded square ring window separates the N-GaN drift region into a plurality of rounded square ring regions, the unetched N-GaN drift regions are interconnected, the width of the central rounded square N-GaN drift region is 80-120 μm, and the width of the surrounding rounded square ring N-GaN drift region is 40-80 μm; the multiple rounded square rings arranged at intervals in the nested rounded square rings are interconnected, and each rounded square ring (each ring of exposed N+GaN transport layer) is 30-60 μm wide. The anode metal arranged in the drift region is an interconnected structure, and the cathode metal arranged on the transport layer is an interconnected structure, and arc-shaped corners are designed at each connection point.

[0019] In one embodiment of the present application, the cathode metal is sputtered on the surface of the N+ gallium nitride transport layer to form an ohmic contact with a width of 24 to 50 μm and a horizontal distance of 3 to 5 μm from the adjacent N-gallium nitride drift region. The cathode metal is located in the middle area of ​​the nested rounded square ring window and has a gap with the side wall of the adjacent N-gallium nitride drift region.

[0020] In one of the embodiments of the present application, the ions injected into the ion implantation area are Ar ions (or N ions), the injection width is 4 to 6 μm, and the depth is 300 to 1500 nm, so as to form lattice damage and capture surrounding free carriers.

[0021] In one embodiment of the present application, the anode metal is evaporated on the surface of the N-GaN drift region, and the edge of the anode metal is located above the ion implantation region, thereby reducing the maximum electric field strength under reverse bias.

[0022] In one of the embodiments of the present application, the dielectric layer also covers the edge regions of the cathode metal and the anode metal.

[0023] The present application provides a method for preparing a silicon-based gallium nitride SBD device, comprising the following steps:

[0024] Growing the AlN / AlGaN buffer layer on the silicon substrate alleviates the film stress problem caused by the lattice mismatch and large difference in thermal expansion coefficient between silicon and gallium nitride, and prevents cracking;

[0025] Growing the N+ gallium nitride transmission layer on the AlN / AlGaN buffer layer, with a high Si doping concentration, as a current transmission carrier;

[0026] Growing the N-gallium nitride drift region on the N+gallium nitride transport layer as a lightly doped region;

[0027] PECVD deposits silicon oxide on the N-gallium nitride drift region and performs uniform coating, opening the nested rounded square ring window, and ICP dry etching to the N+gallium nitride transport layer, using TMAH solution to repair the sidewall damage caused by plasma bombardment, and decomposing the nitrogen-deficient layer above the transport layer in an NH3 / N2 atmosphere;

[0028] Depositing the cathode metal on the N+ gallium nitride transport layer exposed in the nested rounded square ring window to form an ohmic contact, and etching away the metal above the N- gallium nitride drift region and the metal at the upper edge of the N+ gallium nitride transport layer;

[0029] Implanting Ar ions at the edge of the N-gallium nitride drift region to cause lattice damage and form the ion implantation region;

[0030] Evaporating the anode metal on the surface of the N-gallium nitride drift region so that its edge is above the ion implantation region and forms a Schottky contact with the N-gallium nitride drift region into which Ar ions are not implanted;

[0031] The SOG silicide is spin-coated and cured at high temperature to form a high-quality dielectric layer, thereby improving the reliability of the device and reducing edge leakage.

[0032] One or more technical solutions provided in the embodiments of the present application have at least the following technical effects or advantages:

[0033] 1. Compared with the general circular structure, the nested rounded square ring structure of the silicon-based gallium nitride SBD device solves the problem of the difficulty in balancing the device size and the forward current density. The staggered cathode and anode make the current distribution under each ring of anode metal uniform, and a larger active area can be obtained by increasing the number of rounded square rings, thereby reducing VF, achieving the effect of uniformly increasing the overall current density and reducing the VF of the device;

[0034] 2. In this silicon-based gallium nitride SBD device, since the square rings in the nested rounded square ring structure are all rounded, the connection corners between the cathode and anode metals are all arc-shaped rather than simple straight-line connections, thus avoiding electric field crowding; the space charge region at the corner is transformed from a spherical junction to a cylindrical junction, and the maximum electric field strength at the edge is reduced, thereby increasing the device breakdown voltage. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0036] Figure 1This is a schematic cross-sectional structure diagram of a silicon-based gallium nitride SBD device in an embodiment of the present application;

[0037] Figure 2 This is a schematic diagram of a top view of a silicon-based gallium nitride SBD device in an embodiment of the present application;

[0038] Figure 3 A process diagram of a method for preparing a silicon-based gallium nitride SBD device in an embodiment of the present application Figure 1 ;

[0039] Figure 4 A process diagram of a method for preparing a silicon-based gallium nitride SBD device in an embodiment of the present application Figure 2 ;

[0040] Figure 5 A process diagram of a method for preparing a silicon-based gallium nitride SBD device in an embodiment of the present application Figure 3 ;

[0041] Figure 6 A process diagram of a method for preparing a silicon-based gallium nitride SBD device in an embodiment of the present application Figure 4 ;

[0042] Figure 7 A process diagram of a method for preparing a silicon-based gallium nitride SBD device in an embodiment of the present application Figure 5 .

[0043] Among them, 1. Silicon substrate, 2. AlN / AlGaN buffer layer, 3. N+ gallium nitride transport layer, 4. N- gallium nitride drift region, 5. cathode metal, 6. ion implantation region, 7. anode metal, 8. dielectric layer. DETAILED DESCRIPTION

[0044] The present invention is further explained below in conjunction with specific implementation methods. It should be understood that these implementation methods are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0045] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0046] In the description of the present invention, it should be noted that the orientation or position relationship indicated by the terms "vertical", "peripheral surface", etc. is based on the orientation or position relationship shown in the accompanying drawings, or is the orientation or position relationship in which the product of the invention is usually placed when used. It is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0047] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0048] In the description of the present invention, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in the present invention and the features of different embodiments or examples without contradiction.

[0049] The embodiment of the present application provides a silicon-based gallium nitride SBD device and a preparation method thereof, thereby solving the problem of severe current edge gathering effect in conventional silicon-based gallium nitride SBD devices in the prior art, which leads to high forward current density at the anode metal edge of the device and low current density in the middle, thereby achieving the effect of uniformly improving the overall current density and reducing the VF of the device.

[0050] The technical solution in the embodiment of the present application is to solve the above problems, and the overall idea is as follows:

[0051] Embodiment 1:

[0052] like Figure 1 As shown, a silicon-based gallium nitride SBD device comprises:

[0053] Silicon substrate 1;

[0054] An AlN / AlGaN buffer layer 2 is grown on a silicon substrate 1;

[0055] The N+ gallium nitride transmission layer 3 is grown on the AlN / AlGaN buffer layer 2 and serves as a current transmission carrier; the N+ gallium nitride transmission layer 3 is a heavily doped region, has a resistivity of 0.001 to 0.005 Ω·cm, and a thickness of 2 to 4 μm.

[0056] The N-GaN drift region 4 is grown on the N+GaN transport layer 3; the N-GaN drift region 4 is a lightly doped region doped with Si atoms, has a resistivity of 1 to 20 Ω·cm, and a thickness of 1 to 5 μm.

[0057] The N-GaN drift region 4 is provided with a nested rounded square ring window etched to the N+GaN transport layer 3 . The nested rounded square ring is a plurality of rounded square rings with successively increasing inner diameters and spaced apart.

[0058] The cathode metal 5 is deposited on the exposed N+ gallium nitride transport layer 3 in the nested rounded square ring window to form an ohmic contact; the cathode metal 5 is sputtered on the surface of the N+ gallium nitride transport layer 3 to form an ohmic contact with a width of 24 to 50 μm and a horizontal distance of 3 to 5 μm from the adjacent N-gallium nitride drift region 4. That is, the cathode metal 5 is located in the middle area of ​​the nested rounded square ring window, and there is a gap with the side wall of the adjacent N-gallium nitride drift region 4.

[0059] The ion implantation region 6 is arranged at the upper edge and side wall of the N-gallium nitride drift region 4; the ions implanted in the ion implantation region 6 are Ar ions (or N ions), with an implantation width of 4 to 6 μm and a depth of 300 to 1500 nm, so as to form lattice damage and capture surrounding free carriers.

[0060] The anode metal 7 is arranged to be evaporated on the N-gallium nitride drift region 4, the edge of the anode metal 7 is located above the ion implantation region 6, and the anode metal 7 forms a Schottky contact with the N-gallium nitride drift region 4 where no ions are implanted; the anode metal 7 is evaporated on the surface of the N-gallium nitride drift region 4, and the edge of the anode metal 7 is located above the ion implantation region 6, thereby reducing the maximum electric field strength under reverse bias.

[0061] The dielectric layer 8 is formed by spin coating SOG silicide and curing it at high temperature on the exposed upper surface of the N+ gallium nitride transmission layer 3 and the exposed upper surface and sidewall of the N- gallium nitride drift region 4; and covers the edge areas of the cathode metal 5 and the anode metal 7.

[0062] Among them, the nested rounded square ring window separates the N-gallium nitride drift region 4 into several rounded square ring areas, and the unetched N-gallium nitride drift regions 4 are interconnected. The width of the most central rounded square N-gallium nitride drift region 4 is 80-120μm, and the width of the surrounding rounded square ring N-gallium nitride drift region 4 is 40-80μm; the multiple rounded square rings arranged at intervals in the nested rounded square ring are interconnected, and the width of each rounded square ring (each ring of exposed N+gallium nitride transmission layer 3) is 30-60μm. The above arrangement makes the anode metal 7 arranged in the drift region 4 an interconnected structure, and the cathode metal 5 arranged on the transmission layer 3 an interconnected structure; and arc-shaped corners are used at each connection point.

[0063] Optionally, the nested rounded square ring window can be replaced by a nested circular ring window to form a nested structure of multiple concentric circular rings. After the nested circular ring window is used, there is no need to consider the arc-shaped corner design at the connection point on the anode and cathode metal interconnects, but the cell area will be reduced; however, both structures can effectively improve the current edge collection effect. However, a rectangular square ring window cannot be used because the electric field at the edge corner will increase and the device breakdown voltage will decrease.

[0064] Embodiment 2:

[0065] A method for preparing a silicon-based gallium nitride SBD device as shown in Example 1 comprises the following steps:

[0066] Select substrate and buffer layer: grow AlN / AlGaN buffer layer 2 on silicon substrate 1. Use Si as substrate and AlN / AlGaN as buffer layer to solve the problem of lattice mismatch and large difference in thermal expansion coefficient between GaN and Si substrate, and avoid chip breakage caused by excessive stress.

[0067] Preparation of epitaxy: grow GaN doped with high concentration of Si as the current transmission layer, i.e. N+ gallium nitride transmission layer 3, and continue to grow epitaxial GaN drift layer with wurtzite structure, i.e. N- gallium nitride drift region 4, as the withstand voltage depletion region, such as Figure 3 As shown;

[0068] Deep trench etching: A nested rounded square ring window is opened on the N-GaN drift region 4, and then etched to the N+GaN transport layer 3, such as Figure 4 Specifically, silicon oxide is deposited on the N-gallium nitride drift region 4 by PECVD and then coated, a nested rounded square ring window is opened, and ICP dry etching is performed until the N+gallium nitride transport layer 3 is etched, and TMAH solution is used to repair the side wall damage caused by plasma bombardment, and the nitrogen-deficient layer above the transport layer is decomposed in an NH3 / N2 atmosphere.

[0069] Cathode metal sputtering: Cathode metal 5 is deposited on the N+ GaN transport layer 3 exposed in the nested rounded square ring window. The cathode metal 5 is generally an interconnected structure and forms an ohmic contact with the N+ GaN transport layer 3. The metal above the N- GaN drift region 4 and the metal on the upper edge of the N+ GaN transport layer 3 are corroded, such as Figure 5 As shown;

[0070] Terminal formation: Ar ions are injected into the edge of the N-GaN drift region 4 to cause lattice damage and form an ion implantation region 6. A high resistance region is formed at the edge of the N-GaN drift region 4 to divide the edge electric field force equally, such as Figure 6 As shown;

[0071] Anode metal evaporation: Anode metal 7 is evaporated on the surface of N-GaN drift region 4, so that its edge is above ion implantation region 6 and forms Schottky contact with N-GaN drift region 4 where Ar ions are not implanted, thereby reducing the maximum electric field strength at the edge, such as Figure 7 As shown;

[0072] Dielectric layer deposition: spin-coating SOG silicide, high-temperature curing, forming a high-quality dielectric layer 8, so that the remaining exposed GaN (N+ GaN transport layer 3 surface, N- GaN drift region 4 surface and sidewall) are covered with SOG silicide, improving the overall reliability of the device and reducing edge leakage, such as Figure 1-2 shown.

[0073] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:

[0074] Compared with the general circular structure, the nested rounded square ring structure of the silicon-based gallium nitride SBD device solves the problem of the difficulty in balancing the device size and the forward current density. The staggered cathode and anode make the current distribution under each ring of anode metal uniform, and a larger active area can be obtained by increasing the number of rounded square rings, thereby reducing VF, achieving the effect of uniformly improving the overall current density and reducing the VF of the device; at the same time, since the above-mentioned square rings are all rounded, the connection corners of the cathode and anode metals are all arc-shaped designs instead of simple straight-line connections, avoiding electric field crowding, and the space charge region at the corner is transformed from a spherical junction to a cylindrical junction, and the maximum electric field strength at the edge is reduced, thereby increasing the device breakdown voltage.

[0075] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A silicon-based gallium nitride SBD device, It is characterized in that include: Silicon substrate; An AlN / AlGaN buffer layer is disposed on the silicon substrate; An N+ gallium nitride transmission layer is disposed on the AlN / AlGaN buffer layer; An N-GaN drift region is disposed on the N+GaN transport layer, and a nested rounded square ring window etched to the N+GaN transport layer is opened on the N-GaN drift region, and the nested rounded square ring is a plurality of rounded square rings with successively increasing inner diameters and spaced apart; A cathode metal is disposed on the N+ gallium nitride transport layer exposed in the nested rounded square ring window; An ion implantation region, arranged at the upper edge and sidewall of the N-gallium nitride drift region; Anode metal, disposed on the N-gallium nitride drift region; The dielectric layer is disposed on the exposed upper surface of the N+ gallium nitride transmission layer and the exposed upper surface and sidewall of the N- gallium nitride drift region.

2. The silicon-based gallium nitride SBD device according to claim 1, Features: The N+ gallium nitride transmission layer is a heavily doped region, has a resistivity of 0.001 to 0.005 Ω·cm, and a thickness of 2 to 4 μm.

3. The silicon-based gallium nitride SBD device according to claim 2, Features: The N-gallium nitride drift region is a lightly doped region doped with Si atoms, has a resistivity of 1 to 20 Ω·cm, and a thickness of 1 to 5 μm.

4. The silicon-based gallium nitride SBD device according to claim 1, Features: The nested rounded square ring window separates the N-gallium nitride drift region into a plurality of rounded square ring regions, the unetched N-gallium nitride drift regions are connected to each other, the width of the central N-gallium nitride drift region in the form of a rounded square is 80 to 120 μm, and the width of the surrounding N-gallium nitride drift region in the form of a rounded square ring is 40 to 80 μm; the plurality of spaced-apart rounded square rings in the nested rounded square rings are connected to each other, and each rounded square ring has a width of 30 to 60 μm.

5. The silicon-based gallium nitride SBD device according to claim 1, Features: The cathode metal is sputtered on the surface of the N+ gallium nitride transmission layer to form an ohmic contact with a width of 24 to 50 μm and a horizontal distance of 3 to 5 μm from the adjacent N- gallium nitride drift region.

6. The silicon-based gallium nitride SBD device according to claim 1, Features: The ions implanted in the ion implantation area are Ar ions, the implantation width is 4 to 6 μm, and the depth is 300 to 1500 nm.

7. The silicon-based gallium nitride SBD device according to claim 5, Features: The anode metal is evaporated on the surface of the N-gallium nitride drift region, the edge of the anode metal is located above the ion implantation region, and the anode metal forms a Schottky contact with the N-gallium nitride drift region into which ions are not implanted.

8. The silicon-based gallium nitride SBD device according to claim 1, Features: The dielectric layer also covers the edge regions of the cathode metal and the anode metal.

9. A method for preparing a silicon-based gallium nitride SBD device according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Growing the AlN / AlGaN buffer layer on the silicon substrate; Growing the N+ gallium nitride transport layer on the AlN / AlGaN buffer layer; Growing the N-gallium nitride drift region on the N+gallium nitride transport layer; PECVD deposits silicon oxide on the N-gallium nitride drift region and performs photoresist coating, opens the nested rounded square ring window, and ICP dry etches to the N+gallium nitride transport layer; Depositing the cathode metal on the N+ gallium nitride transport layer exposed in the nested rounded square ring window to form an ohmic contact, and etching away the metal above the N- gallium nitride drift region and the metal at the upper edge of the N+ gallium nitride transport layer; Implanting Ar ions at the edge of the N-gallium nitride drift region to cause lattice damage and form the ion implantation region; Evaporating the anode metal on the surface of the N-gallium nitride drift region so that its edge is above the ion implantation region and forms a Schottky contact with the N-gallium nitride drift region into which Ar ions are not implanted; The SOG silicide is spin-coated and cured at high temperature to form the dielectric layer.

10. The preparation method according to claim 9, Features: After the ICP dry etching reaches the N+gallium nitride transport layer, the method further includes: repairing the side wall damage caused by plasma bombardment with a TMAH solution, and decomposing the nitrogen-deficient layer above the transport layer under an NH3 / N2 atmosphere.