Method for preventing bleed-out of high-pulling-speed billet continuous casting machine
By adjusting the pulling speed, inverted taper of the crystallizer and protective slag characteristics, combined with the cooling design of the whole process, the steel leakage problem in the high pulling speed production of the billet continuous casting machine is solved, and stable production and high billet yield are achieved.
Patent Information
- Application Number
- CN202411248580.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-06
AI Technical Summary
During the high-pull speed production process of billet continuous casting machines, steel leakage is prone to occur, including steel leakage at the end of the crystallizer, steel leakage at the corner of the second cold zone, and steel leakage in the middle longitudinal cracks in front of the pulling machine, resulting in production risks and casting billets Receiving rate decreased.
By adjusting the pulling speed, inverted crystallizer taper, and the melting point, melting speed and viscosity of the protective slag, the temperature of the tundra steel water is controlled to ensure the cooling system design of the crystallizer and the second cold zone, including the full-process cooling and multi-stage cooling sections, ensuring casting The temperature and shape stability of the blank during continuous casting.
It realizes the high pull-speed stable production of billet continuous casting machines, reduces the steel leakage rate, improves the casting billet yield, solves the production planning difficulties caused by steel leakage, and has wide application prospects.
Abstract
Description
Technical Field
[0001] The invention relates to a continuous casting method, in particular to a method for preventing steel leakage from a high-speed billet continuous casting machine. Background Art
[0002] During the high-speed production of the square billet continuous casting machine, three types of steel leakage often occur: one is steel leakage at the end of the crystallizer, the second is steel leakage at the corner of the secondary cooling zone, and the third is steel leakage in the middle longitudinal crack in front of the straightening machine. Although the high-speed production of the continuous casting machine can meet the demand for high-temperature steel billets, it also brings production risks. For example, the high-throughput molten steel causes great disturbance to the molten steel in the crystallizer, resulting in large fluctuations in the liquid slag layer of the protective slag and a disordered temperature field in the crystallizer. Secondly, the shell of the continuous casting billet in the secondary cooling chamber becomes thinner. If the cooling water is not replenished in time, steel leakage accidents are prone to occur. At the same time, due to the high manganese content in the steel, after reacting with the protective slag, the heat transfer of the crystallizer and the lubrication of the cast billet are deteriorated, and the probability of crack leakage increases. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for preventing steel leakage in a high-speed billet continuous casting machine, so as to improve the yield rate of the billet.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: when the square billet continuous casting machine is continuously casting, the pulling speed is 3.5-5.5 m / min, and the inverted taper of the crystallizer is 1.9-2.2% / m; the melting point of the protective slag used is 1055-1095°C, the melting speed is 25-33 seconds, and the viscosity is 0.09-0.13 Pa·S; when the pulling speed is 3.5-4.0 m / min, the temperature of the molten steel in the tundish shall not exceed 1535°C, and when the pulling speed of the continuous casting machine is 4.0-5.5 m / min, the temperature of the molten steel in the tundish shall not exceed 1530°C.
[0005] Furthermore, when the pulling speed is 3.5-4.5 m / min, the consumption of protective slag is 0.42-0.50 kg / ton of steel; when the pulling speed is 4.5-5.5 m / min, the consumption of protective slag is 0.45-0.55 kg / ton of steel.
[0006] Furthermore, during the continuous casting, the gap between the surface of the crystallizer foot roller and the four surfaces of the ingot should be no greater than 2 mm.
[0007] Furthermore, the secondary cooling water system of the square billet continuous casting machine must be arranged for full-process cooling, with at least 4 cooling sections, and each cooling section is not less than 1.5m in length.
[0008] The beneficial effect of adopting the above technical solution is that the present invention adopts a suitable inverted taper of the copper tube of the crystallizer, and adopts a suitable melting point, melting speed and viscosity of the protective slag to control the leakage of steel in the crystallizer or the full roll section; thereby realizing the high-speed stable production of the square billet continuous casting machine. The present invention stabilizes the high-speed production of the continuous casting machine, makes the production go smoothly, solves the difficulty of the continuous casting machine being difficult to handle after the leakage of steel at high speed and cannot complete the production plan, improves the yield rate of the casting billet, and has a wide prospect of promotion and application. DETAILED DESCRIPTION
[0009] The present invention is further described in detail below in conjunction with specific implementation modes.
[0010] The method for preventing steel leakage in a high-speed billet continuous casting machine is applicable to ordinary carbon steel and low-alloy steel, and is particularly applicable to steel with a Mn content ranging from 1.20 to 1.60%, preferably a steel with the following composition ratio (wt): C 0.17 to 0.27%, Mn 1.20 to 1.60%, Si 0.30 to 0.90%, S 0 to 0.047%, P 0 to 0.045, V 0.013 to 0.050%, Nb 0.0080 to 0.020%, and the remainder is Fe and unavoidable impurities.
[0011] The method for preventing steel leakage from a high-speed billet continuous casting machine adopts the following process:
[0012] (1) The cross-section of the square billet continuous casting machine is 150 mm × 150 mm to 180 mm × 180 mm, the arc radius of the casting billet is 9 to 12 m, and the casting speed of the continuous casting machine during the production process is 3.5 to 5.5 m / min. When the casting speed is 3.5 to 4.0 m / min, the temperature of the molten steel in the tundish shall not exceed 1535°C; when the casting speed of the continuous casting machine is 4.0 to 5.5 m / min, the temperature of the molten steel in the tundish shall not exceed 1530°C.
[0013] (2) During direct rolling of the billet continuous casting machine, the effective height of the crystallizer is 900-1000 mm, and the inverted taper of the crystallizer is 1.9-2.2% / m.
[0014] (3) The melting point of the mold slag used is 1055-1095°C, the melting speed is 25-33 seconds, and the viscosity is 0.09-0.13 Pa·S. When the pulling speed is 3.5-4.5 m / min, the consumption of the mold slag is 0.42-0.50 kg / ton of steel; when the pulling speed is 4.5-5.5 m / min, the consumption of the mold slag is 0.45-0.55 kg / ton of steel.
[0015] (4) During continuous casting, the gap between the surface of the foot roller of the crystallizer and the four surfaces of the billet should not be greater than 2 mm; in this way, it can be ensured that the continuous casting billet enters the foot roller section after leaving the crystallizer. At this time, the four surfaces of the continuous casting billet can be squeezed by the foot roller in four directions to ensure that the shape of the continuous casting billet is not deformed, reduce the occurrence of corner cracks, and prevent the billet from leaking steel in the foot roller section.
[0016] (5) During continuous casting, the gap between the rollers of each section of the second cooling zone of the square billet continuous casting machine and the outer arc of the arc template does not exceed 2 mm; thus, the stress / strain generated in the continuous casting billet during operation is less than the critical stress / strain of the crack, thereby avoiding steel leakage in the second cooling section of the billet, that is, further controlling steel leakage in the second cooling section through high arc alignment accuracy.
[0017] (6) During continuous casting, the end of the water system in the secondary cooling zone of the square billet continuous casting is no more than 3m away from the air cooling zone of the first roller of the straightening machine; thus, by reducing the distance to the air cooling zone before straightening, the temperature return of the billet can be effectively controlled, thereby controlling the steel leakage of the billet during temperature return.
[0018] (7) The secondary cooling water system of the billet continuous casting machine is pure water cooling, and the water pressure is 1.8-2.2MPa. The secondary cooling water system of the billet continuous casting machine must be arranged for full-process cooling, and the secondary cooling zone has at least 4 cooling sections, and the length of each cooling section is not less than 1.5m. The secondary cooling water system of the billet continuous casting machine is fully equipped with water bars from the crystallizer foot roll to the straightening machine, and water spray cooling is carried out during production, and the maximum water volume of each section is not less than 5t / h.
[0019] (8) For each row of water nozzles in the secondary cooling water system of the billet continuous casting machine, the distance error between the inner and outer arc water nozzles and the surface of the billet is no more than 2mm; the distance error between the arc water nozzles on both sides and the surface of the billet is no more than 2mm. For each row of water nozzles in the secondary cooling water system of the billet continuous casting machine, the inner and outer arc water nozzles are of the same model, and the arc water nozzles on both sides are of the same model.
[0020] Embodiment 1: The method for preventing steel leakage in a high-speed billet continuous casting machine is specifically described as follows.
[0021] There are two rows of crystallizer foot rollers, four in each row, arranged on four sides, with a total of eight foot rollers in two rows. The gap between the surface of the crystallizer foot rollers and the four surfaces of the ingot is 0.1mm, the gap between the rollers of each section of the secondary cooling zone and the outer arc of the ingot is 0.1mm, the distance between the last section of the secondary cooling zone water system (4 sections of the secondary cooling zone) and the first roller of the straightening machine is 2.53m, the taper of the crystallizer copper tube is 2.0% / m, and the total length of the secondary cooling zone is 11.8 meters. When pouring steel, the temperature of the molten steel in the tundish is 1534℃, the pulling speed is 3.6m / min, the melting point of the protective slag is 1065℃, the consumption of protective slag is 0.436kg / t, the total water volume of the secondary cooling zone is 80.42 tons per hour, and 45.08 tons of ingots are produced per hour. The specific water volume of the secondary cooling zone is 1.78l / kg, which enables normal production. There is no leakage of steel from longitudinal cracks at corners and leakage before straightening when pouring steel. The steel composition of this embodiment is shown in Table 1 below;
[0022] Table 1: Composition of the steel described in Example 1 (wt%)
[0023] C Mn P S Si V Nb 0.24 1.39 0.029 0.032 0.33 0.035 0.0093 0.25 1.42 0.027 0.036 0.34 0.035 0.0091
[0024] In Table 1, the balance of the components is Fe and inevitable impurities.
[0025] Embodiment 2: The method for preventing steel leakage in a high-speed billet continuous casting machine is specifically described as follows.
[0026] There are two rows of crystallizer foot rollers, four in each row, arranged on four sides, with a total of eight foot rollers in two rows. The gap between the surface of the crystallizer foot rollers and the four surfaces of the ingot is 0.1mm, the gap between the rollers of each section of the secondary cooling zone and the outer arc of the ingot is 0.1mm, the distance between the last section of the secondary cooling zone water system (4 sections of the secondary cooling zone) and the first roller of the straightening machine is 2.53m, the taper of the crystallizer copper tube is 2.0% / m, and the total length of the secondary cooling zone is 11.8 meters. When pouring steel, the temperature of the molten steel in the tundish is 1532℃, the pulling speed is 3.7m / min, the melting point of the protective slag is 1065℃, the consumption of protective slag is 0.447kg / t, the total water volume of the secondary cooling zone is 82.74 tons per hour, and 46.33 tons of ingots are produced per hour. The specific water volume of the secondary cooling zone is 1.79l / kg, which enables normal production. There is no leakage of steel from longitudinal cracks at the corners and leakage before straightening when pouring steel. The steel grade composition of this embodiment is shown in Table 2 below;
[0027] Table 2: Composition of the steel described in Example 2 (wt%)
[0028] C Mn P S Si V Nb 0.24 1.39 0.025 0.031 0.34 0.035 0.012 0.24 1.42 0.022 0.036 0.34 0.034 0.0108
[0029] In Table 2, the balance of the components is Fe and inevitable impurities.
[0030] Embodiment 3: The method for preventing steel leakage in a high-speed billet continuous casting machine is specifically described as follows.
[0031] There are two rows of crystallizer foot rollers, four in each row, arranged on four sides, with a total of eight foot rollers in two rows. The gap between the surface of the crystallizer foot rollers and the four surfaces of the ingot is 0.1mm, the gap between the rollers of each section of the secondary cooling zone and the outer arc of the ingot is 0.1mm, the distance between the last section of the secondary cooling zone water system (secondary cooling zone section 4) and the first roller of the straightening machine is 2.53m, the taper of the crystallizer copper tube is 2.0% / m, and the total length of the secondary cooling zone is 11.8 meters. When pouring steel, the temperature of the molten steel in the tundish is 1528℃, the pulling speed is 4.2m / min, the melting point of the protective slag is 1060℃, the consumption of protective slag is 0.462kg / t, the total water volume of the secondary cooling zone is 94.08 tons per hour, and 52.59 tons of ingots are produced per hour. The specific water volume of the secondary cooling zone is 1.79l / kg, which enables normal production. There is no leakage of steel from longitudinal cracks at corners and leakage before straightening when pouring steel. The steel composition of this embodiment is shown in Table 3 below;
[0032] Table 3: Composition of the steel described in Example 3 (wt%)
[0033] C Mn P S Si V Nb 0.24 1.38 0.024 0.034 0.33 0.034 0.0083 0.24 1.33 0.03 0.03 0.32 0.034 0.0134
[0034] In Table 3, the balance of the components is Fe and inevitable impurities.
[0035] Embodiment 4: The method for preventing steel leakage in a high-speed billet continuous casting machine is specifically described as follows.
[0036] There are two rows of crystallizer foot rollers, four in each row, arranged on four sides, with a total of eight foot rollers in two rows. The gap between the surface of the crystallizer foot rollers and the four surfaces of the ingot is 0.1mm, the gap between the rollers of each section of the secondary cooling zone and the outer arc of the ingot is 0.1mm, the distance between the last section of the secondary cooling zone water system (4 sections of the secondary cooling zone) and the first roller of the straightening machine is 2.53m, the taper of the crystallizer copper tube is 2.0% / m, and the total length of the secondary cooling zone is 11.8 meters. When pouring steel, the temperature of the molten steel in the tundish is 1528℃, the pulling speed is 4.7m / min, the melting point of the protective slag is 1060℃, the consumption of protective slag is 0.482kg / t, the total water volume of the secondary cooling zone per hour is 104.92 tons, and 58.85 tons of ingots are produced per hour. The specific water volume of the secondary cooling zone is 1.78l / kg, which enables normal production. There is no leakage of steel from longitudinal cracks at the corners and leakage before straightening when pouring steel. The steel composition of this embodiment is shown in Table 4 below;
[0037] Table 4: Composition of the steel described in Example 4 (wt%)
[0038] C Mn P S Si V Nb 0.23 1.37 0.025 0.025 0.31 0.033 0 0.25 1.39 0.033 0.026 0.32 0.035 0
[0039] In Table 4, the balance of the components is Fe and inevitable impurities.
[0040] Embodiment 5: The method for preventing steel leakage in a high-speed billet continuous casting machine is specifically described as follows.
[0041] There are two rows of crystallizer foot rollers, four in each row, arranged on four sides, with a total of eight foot rollers in two rows. The gap between the surface of the crystallizer foot rollers and the four surfaces of the ingot is 0.1mm, the gap between the rollers of each section of the secondary cooling zone and the outer arc of the ingot is 0.1mm, the distance between the last section of the secondary cooling zone water system (4 sections of the secondary cooling zone) and the first roller of the straightening machine is 2.53m, the taper of the crystallizer copper tube is 2.0% / m, and the total length of the secondary cooling zone is 11.8 meters. When pouring steel, the temperature of the molten steel in the tundish is 1525℃, the pulling speed is 5.0m / min, the melting point of the protective slag is 1053℃, the consumption of protective slag is 0.522kg / t, the total water volume of the secondary cooling zone per hour is 115.32 tons, and 62.61 tons of ingots are produced per hour. The specific water volume of the secondary cooling zone is 1.85l / kg, which enables normal production. There is no leakage of steel from longitudinal cracks at the corners and leakage before straightening when pouring steel. The steel composition of this embodiment is shown in Table 5 below;
[0042] Table 5: Composition of the steel described in Example 5 (wt%)
[0043] C Mn P S Si V Nb 0.23 1.33 0.028 0.029 0.32 0.033 0 0.24 1.34 0.045 0.036 0.31 0.034 0
[0044] In Table 5, the balance of the components is Fe and inevitable impurities.
[0045] Embodiment 6: The method for preventing steel leakage in a high-speed billet continuous casting machine is specifically described as follows.
[0046] There are two rows of crystallizer foot rollers, four in each row, arranged on four sides, two rows with a total of eight foot rollers, the gap between the surface of the crystallizer foot rollers and the four surfaces of the ingot is 0.1mm, the gap between the rollers of each section of the secondary cooling zone and the outer arc of the ingot is 0.1mm, the distance between the last section of the secondary cooling zone water system (secondary cooling zone 4 sections) and the first roller of the straightening machine is 2.53m, the taper of the crystallizer copper tube is 2.0% / m, and the total length of the secondary cooling zone is 11.8 meters. When pouring steel, the temperature of the molten steel in the tundish is 1518℃, the pulling speed is 5.5m / min, the melting point of the protective slag is 1050℃, the consumption of protective slag is 0.532kg / t, the total water volume of the secondary cooling zone per hour is 129.30 tons, and 68.87 tons of ingots are produced per hour. The specific water volume of the secondary cooling zone is 1.88l / kg, which enables normal production. There is no leakage of steel from longitudinal cracks at the corners and leakage before straightening when pouring steel. The steel composition of this embodiment is shown in Table 6 below;
[0047] Table 6: Composition of the steel described in Example 6 (wt%)
[0048] C Mn P S Si V Nb 0.24 1.37 0.028 0.033 0.33 0.032 0 0.25 1.41 0.023 0.026 0.42 0.035 0
[0049] In Table 6, the balance of the components is Fe and inevitable impurities.
[0050] Implementation effect statistics:
[0051] In steel enterprises, continuous casting production is organized by pouring in the ladle, and the number of steel leaks is calculated based on the steel leak rate. The definition of steel leak rate varies from enterprise to enterprise and cannot be unified. The steel leak rate of this method is defined as: steel leak times / 10,000 tons of billet, that is, the number of steel leaks for every 10,000 tons of billet produced.
[0052] Before using this method, the steel leakage rate was 7.6 times / 10,000 tons, mainly due to longitudinal crack leakage at corners and leakage before straightening. With the implementation of the above-mentioned processes of this method, the steel leakage rate gradually decreased. According to the monthly output statistics, it was 5.5 times / 10,000 tons, 3.4 times / 10,000 tons, and 1.2 times / 10,000 tons, respectively. After all the above-mentioned processes were adopted, the steel leakage rate can be stably controlled at 0 times / 10,000 tons.
Claims
1. A method for preventing steel leakage in a high-speed billet continuous casting machine, characterized in that: When the square billet continuous casting machine is performing continuous casting, the pulling speed is 3.5-5.5 m / min, and the inverted taper of the crystallizer is 1.9-2.2% / m; the melting point of the protective slag used is 1055-1095°C, the melting speed is 25-33 seconds, and the viscosity is 0.09-0.13 Pa·S; when the pulling speed is 3.5-4.0 m / min, the temperature of the molten steel in the tundish shall not exceed 1535°C, and when the pulling speed of the continuous casting machine is 4.0-5.5 m / min, the temperature of the molten steel in the tundish shall not exceed 1530°C.
2. The method for preventing steel leakage in a high-speed billet continuous casting machine according to claim 1, characterized in that: When the pulling speed is 3.5-4.5 m / min, the consumption of protective slag is 0.42-0.50 kg / ton of steel; when the pulling speed is 4.5-5.5 m / min, the consumption of protective slag is 0.45-0.55 kg / ton of steel.
3. The method for preventing steel leakage in a high-speed billet continuous casting machine according to claim 1, characterized in that: During the continuous casting, the gap between the surface of the crystallizer foot roller and the four surfaces of the casting billet should not be greater than 2 mm.
4. A method for preventing steel leakage in a high-speed billet continuous casting machine according to claim 1, 2 or 3, characterized in that: The secondary cooling water system of the billet continuous casting machine must be arranged for full-process cooling, with at least 4 cooling sections, and the length of each cooling section must be no less than 1.5m.
Citation Information
Patent Citations
Method for controlling bleed-out in high-casting-speed thin slab continuous casting
CN110961592A
Preparation method of low-carbon steel continuous casting billet and design method of secondary cooling water
CN111496208A
Process for preventing crack breakout in continuous casting pouring process of Q195 steel square billet
CN113399637A
Crystallizer copper pipe suitable for square billet high-drawing-speed continuous casting
CN212976653U
Cited By
Thin slab continuous casting method
CN119634690A
Method for preventing continuous casting square billet from flowing and bleed-out