Micron silicon dioxide crystal doped high-heat-dissipation tellurate fluorescent glass as well as preparation method and application thereof

By doping micron silicon dioxide crystals in tellurate fluorescent glass, the problem of heat quenching of fluorescent glass under high-power laser is solved, its heat dissipation performance and anti-laser damage threshold are improved, and the high performance requirements of laser illumination are met , and reduces production costs.

CN119038875AActive Publication Date: 2024-11-29CHINA JILIANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411363827.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-28
Publication Date
2024-11-29
Estimated Expiration
2044-09-28

AI Technical Summary

Technical Problem

Existing fluorescent glasses are easily quenched by heat under high-power laser irradiation, and are difficult to prepare and costly. The high melting temperature of traditional borolate glasses is not good for phosphors, and tellurate glass has a low thermal conductivity, making it difficult to meet laser illumination. High performance requirements in the field.

Method used

Using micron silicon dioxide crystal doped tellurate fluorescent glass, the melting temperature of fluorescent glass is reduced through specific component ratios and preparation processes, and its heat dissipation performance is enhanced, and the high thermal conductivity and low light of micron silicon dioxide crystals are passed. Absorption improves the luminous intensity and anti-laser damage threshold of fluorescent glass.

Benefits of technology

It achieves efficient luminescence performance and thermal stability, meets the high performance requirements of white laser illumination, and has simple preparation technology and low production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038875A_ABST
    Figure CN119038875A_ABST
Patent Text Reader

Abstract

The invention discloses micron silicon dioxide crystal doped high-heat-dissipation tellurate fluorescent glass as well as a preparation method and application thereof, and relates to the technical field of laser illumination. The tellurate fluorescent glass doped with the micron silicon dioxide crystal comprises the following raw materials: yttrium aluminum garnet yellow fluorescent powder, the micron silicon dioxide crystal and precursor glass powder, the precursor glass powder comprises the following raw materials in percentage by mole: 59-70% of TeO2, 10-20% of ZnO, 10-20% of Na2O and 1-10% of Al2O3, the mass of the yttrium aluminum garnet yellow fluorescent powder is 1-15% of the mass of the precursor glass powder, and the mass of the micron silicon dioxide crystal is 10-25% of the mass of the precursor glass powder. The fluorescent glass disclosed by the invention is high in luminescence property, excellent in thermal stability and high in laser irradiation threshold value, and can meet the high-performance requirement of white laser illumination; meanwhile, the method has the remarkable advantages of simple preparation process, environment friendliness and low production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of laser lighting technology, and in particular to a high-heat-dissipating tellurite fluorescent glass doped with micron silicon dioxide crystals, and a preparation method and application thereof. Background Art

[0002] Semiconductor solid-state light sources have gradually replaced traditional light sources due to their significant advantages such as high light efficiency, low power, long life and environmental friendliness. The way in which blue light chips excite yellow phosphors is a common way used in white light lighting. Improving the photothermal performance of yellow phosphors and the fluorescent conversion materials they consist of is of great significance to promoting the development of white light lighting technology.

[0003] Fluorescent conversion materials mainly include fluorescent glass, fluorescent ceramics and single crystals. However, under the excitation of high-power blue laser chips, traditional fluorescent glass, fluorescent ceramics and other fluorescent conversion materials are prone to cracking due to high temperature problems, and problems such as reduced luminous efficiency and thermal quenching of phosphors occur. At the same time, the high difficulty and high cost of preparing single crystals themselves limit their large-scale application. Heat dissipation methods such as external heat sinks or high thermal conductivity substrates will increase the cost and structural complexity of lighting devices, seriously affecting the photothermal performance of white light laser lighting.

[0004] In the prior art, borosilicate glass and phosphors can be combined to produce fluorescent glass. However, due to the high melting temperature of borosilicate glass, the temperature must reach over 1,000 degrees Celsius when producing borosilicate glass. Such a high melting temperature places extremely high demands on the production process, and the high temperature environment will also damage the phosphors. At the same time, the refractive index of borosilicate is low, which leads to a mismatch between the refractive index of borosilicate and that of phosphors, affecting the reflection and scattering effects of light. The effect of improving the performance of white light is not ideal and it is difficult to meet actual requirements.

[0005] Compared with borosilicate glass, tellurite glass has a lower melting temperature and a higher refractive index, which is suitable for commercial phosphors, and thus can become a more ideal fluorescent conversion material. However, the problem is that tellurite glass has a low thermal conductivity and will heat up rapidly under high-power laser irradiation, which will lead to thermal quenching of the phosphor, thus limiting its application in the field of laser lighting.

[0006] Therefore, on the basis of improving the heat dissipation capacity of tellurite fluorescent glass, preparing fluorescent glass materials with high refractive index, low melting point and high thermal conductivity, and then enriching the types of fluorescent glass and ensuring its performance are technical problems that need to be urgently solved in the field of laser lighting. Summary of the invention

[0007] The purpose of the present invention is to provide a high-heat-dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals and a preparation method and application thereof, so as to solve the problems existing in the above-mentioned prior art.

[0008] To achieve the above object, the present invention provides the following solutions:

[0009] The present invention provides a tellurite fluorescent glass doped with micron silicon dioxide crystals, the raw materials of which include the following components:

[0010] Yttrium aluminum garnet yellow phosphor, micronized silica crystals, and precursor glass powder;

[0011] The precursor glass powder is composed of the following components in terms of mole percentage: TeO2 59-70%, ZnO 10-20%, Na2O 10-20% and Al2O3 1-10%;

[0012] The mass of the yttrium aluminum garnet yellow phosphor is 1-15% of the mass of the precursor glass powder; the mass of the micron silicon dioxide crystal is 10-25% of the mass of the precursor glass powder.

[0013] Further, the precursor glass powder is composed of the following components in terms of mole percentage: TeO2 65%, ZnO 15%, Na2O 15% and Al2O3 5%;

[0014] The mass of the yttrium aluminum garnet yellow phosphor is 15% of the mass of the precursor glass powder; the mass of the micron silicon dioxide crystal is 20% of the mass of the precursor glass powder.

[0015] Furthermore, the micron silicon dioxide crystals are tetragonal micron silicon dioxide crystals.

[0016] Furthermore, the particle size of the micron silicon dioxide crystals is 1 to 20 μm.

[0017] Furthermore, the method for preparing the micronized silicon dioxide crystals comprises the following steps:

[0018] Amorphous silicon dioxide powder with a purity of ≥99.9% is heated at 1600° C. for 1 hour, cooled to room temperature, then kept at 1300-1500° C. for 6-10 hours, cooled to room temperature again and ground to obtain the micron silicon dioxide crystals.

[0019] The present invention also provides a method for preparing the above-mentioned micron silicon dioxide crystal-doped tellurite fluorescent glass, comprising the following steps:

[0020] After the TeO2, ZnO, Na2O and Al2O3 are mixed and ground, first melting, casting and grinding are performed to obtain the precursor glass powder;

[0021] Mixing the precursor glass powder with the yttrium aluminum garnet yellow phosphor and micron silicon dioxide crystals, and performing a second melting to obtain a mixed glass liquid;

[0022] The mixed glass liquid is solidified and shaped, and then annealed to obtain the tellurite fluorescent glass doped with the micron silicon dioxide crystals.

[0023] Furthermore, the temperature of the first melting is 850-950° C., and the time is 30-50 min; the temperature of the second melting is 550-650° C., and the time is 10-30 min.

[0024] Furthermore, the solidification temperature is 350-450° C.; the annealing temperature is 250-350° C., and the annealing time is 3 hours.

[0025] More preferably, after the first melting and casting, a heat treatment step is further included. Specifically, the heat treatment temperature is 250-350° C. and the time is 1-5 hours.

[0026] The present invention further provides the use of the above-mentioned micron silicon dioxide crystal doped tellurite fluorescent glass in white light laser lighting.

[0027] The present invention has strict restrictions on the amount of micron silicon dioxide crystals added, and the amount of addition cannot exceed the limited range, otherwise the glass network formation body will not be dense enough, resulting in reduced transparency of the fluorescent glass and poor luminescence.

[0028] The purpose of the second melting in the present invention is to lower the melting temperature of the fluorescent glass, shorten the time that the fluorescent powder is at high temperature during the preparation process, and further reduce the damage of the crystal structure of the fluorescent powder caused by high temperature.

[0029] The micron silicon dioxide crystals in the raw material components of the tellurite fluorescent glass of the present invention have high thermal conductivity, which can enhance the heat dissipation capacity of the fluorescent glass, and have low light absorption coefficient and good reflection effect. While enhancing the heat dissipation performance of the tellurite fluorescent glass, they can also act as scattering centers, so that the luminous intensity and anti-laser damage threshold of the high-heat dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals are significantly enhanced.

[0030] The tellurite glass of the present invention ensures excellent fluidity and suitable density of the glass in a molten state by adjusting the components, so that the micron silicon dioxide crystals have good wettability in the glass. This allows the silicon dioxide crystals to fully contact the glass liquid during the doping process, thereby not causing pores and improving the density of the fluorescent glass; and the silicon dioxide crystals can disperse themselves in the fluorescent glass during the melting process, and will not cluster or agglomerate like other high thermal conductivity powders, thereby improving the uniformity of the fluorescent glass.

[0031] The present invention discloses the following technical effects:

[0032] The high-heat-dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals of the present invention has efficient luminescence performance, excellent thermal stability, and a high laser irradiation threshold, and can meet the high-performance requirements of white light laser lighting; at the same time, it has the significant advantages of simple preparation process, green environmental protection, and low production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 High-definition transmission electron microscope and diffraction images of the tetragonal micron silicon dioxide crystal prepared in Example 1 of the present invention;

[0035] Figure 2 XRD images of the micron silicon dioxide crystals obtained in Example 1 of the present invention and the tellurite fluorescent glass materials obtained in Examples 2, 3 and 6;

[0036] Figure 3 Spectra of the transmittance of the high heat dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals prepared in Examples 4 to 7 of the present invention and the tellurite glass matrix material prepared in Comparative Example 1 in the 300 to 800 nm band (the illustrations are, from left to right, actual images of the materials of Comparative Example 1 and Examples 4 to 7 under white light irradiation);

[0037] Figure 4 The emission spectra of the high heat dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals prepared in Examples 4 to 7 of the present invention and the tellurite fluorescent glass material prepared in Comparative Example 2 in the wavelength range of 480 to 700 nm;

[0038] Figure 5A line graph showing the relationship between the luminous flux and the laser irradiation density of the high heat dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals prepared in Examples 4 to 7 of the present invention and the tellurite fluorescent glass material prepared in Comparative Example 2 under 450nm blue laser excitation;

[0039] Figure 6 The line graphs of the relationship between the temperature of the high heat dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals prepared in Example 6 of the present invention and the tellurite fluorescent glass material prepared in Comparative Example 2 under 450nm blue laser excitation and the laser irradiation density (the insets are the temperature of the two materials at 6W / mm 2 Infrared thermal imaging image under blue light laser irradiation with laser irradiation density). DETAILED DESCRIPTION

[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0041] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0045] Unless otherwise specified, the raw materials used in the examples of the present invention were purchased from commercial sources.

[0046] Unless otherwise specified, the "room temperature" described in the embodiments of the present invention is in the range of 20 to 30°C.

[0047] The technical solution of the present invention is further illustrated by the following embodiments.

[0048] Example 1

[0049] Preparation of tetragonal micronized silicon dioxide crystals:

[0050] Amorphous silicon dioxide powder with a purity of ≥99.9% is heated at 1600°C for 1 hour, cooled to room temperature, then kept at 1400°C for 10 hours, cooled to room temperature again and ground to obtain micron silicon dioxide crystals with a particle size of 1 to 20 μm.

[0051] The micronized silicon dioxide crystals prepared in Example 1 were observed using a high-resolution transmission electron microscope. Figure 1 As shown, the left picture is an image of a micron silicon dioxide crystal with a diameter of 2μm. The illustration in the left picture is a high-resolution electron diffraction pattern, in which the diffraction spots are neatly arranged in a square shape and have a high degree of symmetry, which proves that after high-temperature heat treatment, the amorphous silicon dioxide powder has a clear crystal structure. The right picture shows the morphology of silicon dioxide crystals at a scale of 10nm, with clearly visible lattice fringes and a fringe spacing of 0.316nm, which is consistent with the lattice spacing of tetragonal silicon dioxide.

[0052] Example 2

[0053] Preparation of high heat dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals:

[0054] (1) According to the amounts of the raw materials shown in Table 1, weigh yttrium aluminum garnet yellow phosphor, micron silicon dioxide crystals (prepared in Example 1), TeO2, ZnO, Na2O and Al2O3;

[0055] (2) TeO2, ZnO, Na2O and Al2O3 are mixed and ground evenly, and then put into an alumina crucible, and placed in a silicon carbon rod electric furnace at 900°C for melting (first melting) for 40 minutes to obtain glass liquid, and then the glass liquid is poured into a mold at 400°C for casting, and then quickly transferred to a muffle furnace that has been heated to 300°C, kept warm for 3 hours, and then cooled to room temperature to obtain a precursor glass and grind it to obtain a precursor glass powder with fine particles and uniform size;

[0056] (3) The obtained precursor glass powder, micron silica crystals and yttrium aluminum garnet yellow phosphor are mixed evenly and poured into a crucible together, and then placed in a silicon carbon rod electric furnace at 600°C for melting (second melting) for 20 minutes to obtain a mixed glass liquid (clear, uniform and free of bubbles), and the mixed glass liquid is poured into a mold preheated to 400°C for solidification, and then quickly transferred to a muffle furnace heated to 300°C for annealing, and then cooled to room temperature after being kept warm for 3 hours to obtain a high heat dissipation tellurite fluorescent glass material doped with micron silica crystals.

[0057] Example 3

[0058] Preparation of high heat dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals:

[0059] (1) According to the amounts of the raw materials shown in Table 1, weigh yttrium aluminum garnet yellow phosphor, micron silicon dioxide crystals (prepared in Example 1), TeO2, ZnO, Na2O and Al2O3;

[0060] The preparation process of steps (2)-(3) is the same as that of Example 2.

[0061] Example 4

[0062] Preparation of high heat dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals:

[0063] (1) According to the amounts of the raw materials shown in Table 1, weigh yttrium aluminum garnet yellow phosphor, micron silicon dioxide crystals (prepared in Example 1), TeO2, ZnO, Na2O and Al2O3;

[0064] The preparation process of steps (2)-(3) is the same as that of Example 2.

[0065] Example 5

[0066] Preparation of high heat dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals:

[0067] (1) According to the amounts of the raw materials shown in Table 1, weigh yttrium aluminum garnet yellow phosphor, micron silicon dioxide crystals (prepared in Example 1), TeO2, ZnO, Na2O and Al2O3;

[0068] The preparation process of steps (2)-(3) is the same as that of Example 2.

[0069] Example 6

[0070] Preparation of high heat dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals:

[0071] (1) According to the amounts of the raw materials shown in Table 1, weigh yttrium aluminum garnet yellow phosphor, micron silicon dioxide crystals (prepared in Example 1), TeO2, ZnO, Na2O and Al2O3;

[0072] The preparation process of steps (2)-(3) is the same as that of Example 2.

[0073] Example 7

[0074] Preparation of high heat dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals:

[0075] (1) According to the amounts of the raw materials shown in Table 1, weigh yttrium aluminum garnet yellow phosphor, micron silicon dioxide crystals (prepared in Example 1), TeO2, ZnO, Na2O and Al2O3;

[0076] The preparation process of steps (2)-(3) is the same as that of Example 2.

[0077] Comparative Example 1

[0078] Preparation of tellurite glass matrix materials:

[0079] (1) According to the amounts of the raw materials shown in Table 1, weigh TeO2, ZnO, Na2O and Al2O3;

[0080] (2) TeO2, ZnO, Na2O and Al2O3 are mixed and ground evenly, put into an alumina crucible, and placed in a silicon carbon rod electric furnace at 900°C for melting (first melting) for 40 minutes to obtain molten glass, which is poured into a 400°C mold for casting, and then quickly transferred to a muffle furnace that has been heated to 300°C, kept warm for 3 hours, and then cooled to room temperature to obtain a precursor glass, which is polished to obtain a smooth and transparent tellurite glass matrix material.

[0081] Comparative Example 2

[0082] (1) According to the amounts of the raw materials shown in Table 1, weigh yttrium aluminum garnet yellow phosphor, TeO2, ZnO, Na2O and Al2O3;

[0083] (2) TeO2, ZnO, Na2O and Al2O3 are mixed and ground evenly, and then put into an alumina crucible, and placed in a silicon carbon rod electric furnace at 900°C for melting (first melting) for 40 minutes to obtain glass liquid, and then the glass liquid is poured into a mold at 400°C for casting, and then quickly transferred to a muffle furnace that has been heated to 300°C, kept warm for 3 hours, and then cooled to room temperature to obtain a precursor glass and grind it to obtain a precursor glass powder with fine particles and uniform size;

[0084] (3) The obtained precursor glass powder and yttrium aluminum garnet yellow phosphor are evenly mixed and poured into a crucible, and then placed in a 600°C silicon carbon rod electric furnace for melting (second melting) for 20 minutes, and then poured into a mold that has been preheated to 400°C to solidify and form, and quickly transferred to a muffle furnace that has been heated to 300°C for annealing. After keeping warm for 3 hours, it is cooled to room temperature to obtain a tellurite fluorescent glass material.

[0085] Table 1

[0086]

[0087]

[0088] Comparative Example 3

[0089] The only difference from Example 6 is that the micron silicon dioxide crystals are replaced with an equal mass of amorphous silicon dioxide powder.

[0090] Comparative Example 4

[0091] The only difference from Example 6 is that the micron silicon dioxide crystals are replaced with micron boron nitride powder of equal mass.

[0092] The performance tests were performed on the materials prepared in Examples 2-7 and Comparative Examples 1-4:

[0093] 1. Transmission electron microscope images

[0094] The micronized silica crystal obtained in Example 1 was observed using a transmission electron microscope to obtain a high-definition transmission electron microscope image and an electron diffraction pattern. The left figure shows that the diameter of the silica crystal is about 2 μm, and the micron-scale size is very suitable for light scattering centers and thermal conductive materials. The illustration in the left figure is an electron diffraction pattern of the silica crystal. When the incident electron beam meets a certain angle relationship with the crystal plane inside the crystal, the electron beam will be reflected and strengthened by the crystal plane, thus forming a diffraction spot as shown in the figure. Figure 1 The diffraction spots in the figure are arranged neatly, showing a high degree of symmetry and regularity, which indicates that the crystal structure of the silicon dioxide crystal prepared by the present invention has symmetrical crystal planes and the crystal structure shows periodic repetition. This ordered crystal structure provides a stable channel for the conduction of heat, reduces the scattering and obstruction of thermal phonons during the conduction process, and thus improves thermal conductivity. The lattice spacing in the right figure belongs to the (111) crystal plane of tetragonal silicon dioxide, which also proves that the preparation of tetragonal silicon dioxide crystals is successful.

[0095] 2. XRD pattern

[0096] Using Cu~K αX-ray diffraction test in radiation mode shows XRD patterns of the micron silicon dioxide crystals obtained in Example 1 and the tellurite fluorescent glass materials obtained in Examples 2, 3 and 6. Figure 2 As shown. It can be seen that the characteristic peaks shown in Example 1 are completely consistent with those shown in the micron silicon dioxide crystal standard card, proving that the micron silicon dioxide crystals were successfully synthesized. In other examples, yttrium aluminum garnet yellow phosphor (Y3Al5O 12 ) and micron-silicon dioxide crystal phases, which confirms that the micron-silicon dioxide crystals will not introduce impurities into the tellurite fluorescent glass and the yttrium aluminum garnet yellow phosphor crystals are not destroyed.

[0097] 3. Transmission spectrum

[0098] The tellurite glass matrix material prepared in Comparative Example 1 and the high heat dissipation tellurite fluorescent glass doped with micronized silicon dioxide crystals prepared in Examples 4 to 7 were measured in the 300 to 800 nm band using a spectrophotometer and an ultraviolet-visible-near infrared spectrometer to obtain transmission spectra, such as Figure 3 The illustrations are, from left to right, actual pictures of the samples of Comparative Example 1 and Examples 4 to 7 under white light irradiation.

[0099] from Figure 3 It can be seen that the high-heat-dissipation tellurite fluorescent glass doped with micronized silica crystals prepared by the present invention has good transmittance, and as the content of micronized silica increases, the transmittance of the fluorescent glass in visible light gradually decreases, which proves that the silica crystals play a certain light scattering role in the fluorescent glass. Excessive transparency causes the excitation light source to directly penetrate the glass, and effective scattering and uniform distribution of light cannot be achieved. Therefore, when designing and preparing fluorescent glass, it is necessary to comprehensively consider the balance between scattering and transparency. Micronized silica particles can act as scatterers to disperse the incident light, causing the light to be reflected and refracted multiple times inside the fluorescent glass, enhancing the absorption and conversion of the excitation light source by the phosphor, thereby obtaining a higher luminous efficiency.

[0100] 4. Fluorescence spectrum

[0101] The fluorescence spectra of the high heat dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals prepared in Examples 4 to 7 and the tellurite fluorescent glass material prepared in Comparative Example 2 were tested under 450 nm laser diode pumping. Figure 4 As shown. Under the pumping of a laser diode with a wavelength of 450nm, broadband light emission with a central wavelength of 540nm is obtained. It can be seen that since the micron silicon dioxide crystal plays the role of a scattering center, its introduction has a significant improvement on the emission intensity of the tellurite fluorescent glass material.

[0102] 5. Laser irradiation threshold test

[0103] The high heat dissipation tellurite fluorescent glass doped with micron silicon dioxide crystals prepared in Examples 4 to 7 and the tellurite fluorescent glass materials prepared in Comparative Examples 2 to 3 were tested for luminous flux and laser irradiation density. The results are shown in FIG. Figure 5 .Depend on Figure 5 It can be seen that under 450nm blue laser irradiation, the introduction of micron silicon dioxide crystals enhances the heat dissipation capacity of the glass, making the material more difficult to break under high-power laser irradiation. The sample of Example 6 has the best luminous efficiency and laser irradiation threshold. Compared with Comparative Example 2, the maximum laser power density that this micron silicon dioxide crystal doped high heat dissipation tellurite fluorescent glass can withstand is increased by about 40%, at 7W / mm 2 At a laser power density of , the luminous flux remains at 550lm, while Comparative Example 2 at this time is thermally quenched due to the excessive temperature of the phosphor and no longer emits light. The laser irradiation threshold of the tellurite fluorescent glass material prepared in Comparative Example 3 did not show a significant improvement compared with Comparative Example 2. This is because the heat dissipation capacity of amorphous silica powder is much lower than that of tetragonal silica crystals, and it cannot bring additional heat dissipation effect to the fluorescent glass. The sample obtained in Comparative Example 4 has no obvious glass luster and the luminescence effect is extremely poor. This is because the composite effect of boron nitride and tellurite fluorescent glass is poor, and it cannot be spontaneously and evenly dispersed inside the fluorescent glass during the melting process like micron silica crystals, resulting in the agglomeration of boron nitride clusters, which hinders luminescence.

[0104] 6. Temperature and laser irradiation density test

[0105] The tellurite fluorescent glass material prepared in Comparative Example 2 and the tellurite fluorescent glass of Example 6 with the best luminous performance were irradiated with a 450nm blue laser, and the laser irradiation density was continuously adjusted. The temperature of the fluorescent glass was measured with an infrared temperature measuring gun to obtain a relationship diagram between the working temperature and the laser irradiation density, in which the illustrations are respectively the two samples at 6W / mm 2 Infrared thermal imaging of laser irradiation density under blue laser irradiation, the results are shown in Figure 6 .Depend on Figure 6 It can be seen that under 450nm blue laser irradiation, the introduction of micronized silicon dioxide crystals significantly reduced the temperature of the material under laser irradiation. 2 Under the laser irradiation density of 8W / mm, the tellurite fluorescent glass material prepared in Comparative Example 2 has been thermally quenched due to high temperature. However, the tellurite fluorescent glass obtained in Example 6 is still working, and the working temperature is 54.3℃ lower than that of the former, until 8W / mm 2 Thermal quenching occurs only when the laser irradiation density is above 0.05.

[0106] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A tellurite fluorescent glass doped with micronized silicon dioxide crystals, characterized in that: The raw materials include the following components: Yttrium aluminum garnet yellow phosphor, micronized silica crystals, and precursor glass powder; The precursor glass powder is composed of the following components in terms of mole percentage: TeO2 59-70%, ZnO 10-20%, Na2O 10-20% and Al2O3 1-10%; The mass of the yttrium aluminum garnet yellow phosphor is 1-15% of the mass of the precursor glass powder; the mass of the micron silicon dioxide crystal is 10-25% of the mass of the precursor glass powder.

2. The micron silicon dioxide crystal doped tellurite fluorescent glass according to claim 1, characterized in that: The precursor glass powder is composed of the following components in terms of mole percentage: TeO2 65%, ZnO 15%, Na2O 15% and Al2O3 5%; The mass of the yttrium aluminum garnet yellow phosphor is 15% of the mass of the precursor glass powder; the mass of the micron silicon dioxide crystal is 20% of the mass of the precursor glass powder.

3. The tellurite fluorescent glass doped with micronized silicon dioxide crystals according to claim 1, characterized in that: The micron silicon dioxide crystals are tetragonal micron silicon dioxide crystals.

4. The tellurite fluorescent glass doped with micronized silicon dioxide crystals according to claim 1, characterized in that: The particle size of the micron silicon dioxide crystal is 1 to 20 μm.

5. The micron silicon dioxide crystal doped tellurite fluorescent glass according to claim 1, characterized in that: The method for preparing the micron silicon dioxide crystals comprises the following steps: Amorphous silicon dioxide powder with a purity of ≥99.9% is heated at 1600° C. for 1 hour, cooled to room temperature, then kept at 1300-1500° C. for 6-10 hours, cooled to room temperature again and ground to obtain the micron silicon dioxide crystals.

6. The method for preparing the tellurite fluorescent glass doped with micron silicon dioxide crystals according to any one of claims 1 to 5, characterized in that: The following steps are involved: After the TeO2, ZnO, Na2O and Al2O3 are mixed and ground, first melting, casting and grinding are performed to obtain the precursor glass powder; Mixing the precursor glass powder with the yttrium aluminum garnet yellow phosphor and micron silicon dioxide crystals, and performing a second melting to obtain a mixed glass liquid; The mixed glass liquid is solidified and shaped, and then annealed to obtain the tellurite fluorescent glass doped with the micron silicon dioxide crystals.

7. The preparation method according to claim 6, characterized in that: The temperature of the first melting is 850-950° C., and the time is 30-50 min; the temperature of the second melting is 550-650° C., and the time is 10-30 min.

8. The preparation method according to claim 6, characterized in that: The solidification temperature is 350-450° C.; the annealing temperature is 250-350° C., and the annealing time is 3 hours.

9. Use of the tellurite fluorescent glass doped with micronized silicon dioxide crystals as claimed in any one of claims 1 to 5 in white light laser lighting.

Citation Information

Patent Citations

  • Fluorescent powder-glass composite material and rapid synthesis method thereof

    CN117945652A

  • Micron boron nitride doped tellurate fluorescent glass as well as preparation method and application thereof