Preparation method of copper sulfide aminated polyacrylonitrile fiber cloth and application of copper sulfide aminated polyacrylonitrile fiber cloth in photo-thermal antibacterial material
By chelating copper sulfate with aminated polyacrylonitrile fiber and synthesizing copper sulfide, aminated polyacrylonitrile copper sulfide composite fiber with photothermal effect, the problems of low antibacterial efficiency and high cost in the prior art are solved. It has achieved efficient bactericidal and improved stability for a variety of bacteria.
Patent Information
- Application Number
- CN202411153563.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the antibacterial application of copper sulfide for fiber materials has problems such as unforming materials, low antibacterial efficiency, high cost and easy dissolution, and the application scenarios are limited, making it difficult to achieve stable, efficient and fast antibacterial effects.
Using two-step hydration method, copper sulfate is chelated with aminated polyacrylonitrile fibers, and then copper sulfide is synthesized with sulfur-containing solution to form aminated polyacrylonitrile copper sulfide composite fiber with photothermal effect, improving antibacterial efficiency and and load copper sulfide on the fiber surface to enhance adsorption capacity.
It has achieved efficient antibacterial effects on a variety of bacteria, including E. coli, Staphylococcus aureus, etc., achieving a sterilization rate of 99.99%. The material is stable and difficult to dissolve, reducing production costs and expanding application scenarios.
Smart Images

Figure CN119041195A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of fiber materials and relates to the preparation of photothermal antibacterial materials, in particular to a preparation method of copper sulfide aminated polyacrylonitrile fiber cloth and the application of the copper sulfide aminated polyacrylonitrile fiber cloth in photothermal antibacterial materials. Background Art
[0002] Polyacrylonitrile (acrylic fiber) is an active material with abundant amino functional groups. After modification with organic amines, a functional fiber material with more abundant amino, carboxyl and other functional groups can be obtained. It has the adsorption effect on ammonia, hydrogen sulfide and sulfur dioxide gas, and also has more than 80% (18 hours of oscillation) antibacterial performance against Escherichia coli and Staphylococcus aureus under the oscillation method (GB / T 20944.3-2008). Aminated polyacrylonitrile fiber materials can chelate with a variety of metal ions to form uniform metalized fiber materials, which broadens its application field.
[0003] Copper sulfide is a photothermal material with certain antibacterial and excellent biocompatibility. It is used in many industries including semiconductors, photothermal, and antibacterial. In recent years, it has also been used in the composite of various different collective materials. For example, when combined with implantable medical materials such as titanium alloy or silk, it has shown some excellent photothermal antibacterial effects. However, there are common defects such as material non-formability or low antibacterial efficiency. At the same time, existing technologies are mostly used in pure solid materials or nano-liquid materials, and the application scenarios are limited.
[0004] The patent with publication number CN113073464A discloses a method for processing cellulose fiber products with photothermal effect. The method first introduces vinyl into cellulose fiber products, and then uses horseradish peroxidase to catalyze the graft polymerization of acrylic acid and N,N-methylenebisacrylamide on the fiber to form a carboxyl-containing mesh template on the fiber surface; then the cellulose fiber products are immersed in a copper ammonia solution, and sodium sulfide is added to promote the in-situ deposition of nano copper sulfide particles on the fiber surface to obtain cellulose fiber products with photothermal effect; this method is the current mainstream antibacterial fiber material for copper sulfide sterilant modification of fiber material matrix, which generally has poor antibacterial timeliness, requires strong energy, or high raw material cost, or antibacterial raw materials are easy to dissolve. Therefore, it is urgent to find a fiber material with certain mechanical support properties, which is stable, efficient, fast, and has low production cost, is not easy to dissolve, is pollution-free, and can be used with a variety of different bacteria. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a preparation method of copper sulfide aminated polyacrylonitrile fiber cloth and its application in photothermal antibacterial materials.
[0006] The technical solution of the present invention is achieved in this way: Aiming at the existing material aminated polyacrylonitrile fiber, the present invention adopts a two-step hydration method, first chelates copper sulfate with aminated polyacrylonitrile, and then uses a sulfur-containing solution to synthesize copper sulfide on the fiber surface, and finally obtains aminated polyacrylonitrile copper sulfide composite fiber with photothermal effect. The combination with aminated polyacrylonitrile fiber can greatly improve its photothermal antibacterial efficiency and rate, and also make the newly obtained material have a certain adsorption effect of ammonia, hydrogen sulfide and sulfur dioxide, and treat the odor caused by bacterial death in an antibacterial environment.
[0007] Specifically, a method for preparing copper sulfide aminated polyacrylonitrile fiber cloth comprises the following steps: (1) Adding polyacrylonitrile fiber to triethylenetetramine, washing and drying after cross-linking reaction to obtain aminated polyacrylonitrile, i.e. APAN; (2) APAN is added to a copper sulfate solution, and then an EDTA-2Na solution is added. After a chelation reaction, an aminated polyacrylonitrile solution of chelated copper, i.e., APAN@CuSO4 solution, is obtained. This process fully chelates the material with the aminated polyacrylonitrile to achieve the Cu 2+ The effect of evenly distributing ions on the fiber surface; (3) Adding a sulfur source to the APAN@CuSO4 solution of step (2) and adjusting the pH to neutral, the reaction was continued to obtain copper sulfide aminated polyacrylonitrile fiber cloth.
[0008] In the above step (1), 0.8-1.5 g of polyacrylonitrile fiber is added to every 10 mL of triethylenetetramine; the purity of the triethylenetetramine is greater than 90%.
[0009] The temperature of the cross-linking reaction is 120-140° C. and the time is 2-4 hours; the temperature of the drying is 50-60° C. and the time is 18-24 hours.
[0010] In the above step (2), the molar amount of copper sulfate added per g APAN is 1.5-3 mmoL, and the molar amount of EDTA-2Na is 1 mmoL; the concentration of the copper sulfate solution is 0.15-0.3 mol / L; and the concentration of the EDTA-2Na solution is 0.2 mol / L.
[0011] The temperature of the above chelation reaction is 75-85°C and the time is 2-3h; The molar ratio of the Cu source to the S source in the reaction system of the above step (3) is (1-2):1; the S source is one or more of thiourea, sodium sulfide or sodium thiosulfate.
[0012] The reaction temperature in the above step (3) is 60°C and the reaction time is 2h.
[0013] The copper sulfide aminated polyacrylonitrile fiber cloth can generate hydroxyl radicals and superoxide radicals in a certain water environment under the action of copper sulfide loaded on the surface, and synergistically increase the antibacterial efficiency with Cu salt and APAN, reaching an antibacterial efficiency of 99.99% within 30 minutes.
[0014] The copper sulfide aminated polyacrylonitrile fiber cloth is used as an antibacterial material, wherein the bacteria are selected from any one of Escherichia coli, Staphylococcus aureus, Klebsiella pneumoniae, Pseudomonas aeruginosa, Enterococcus faecalis and Candida albicans.
[0015] The above light is 170mw / cm 2 Xenon lamp irradiation light.
[0016] The present invention has the following beneficial effects: 1. The copper sulfide aminated polyacrylonitrile fiber cloth of the present application is based on the polyacrylonitrile fiber, which is modified by amination and then loaded with nano copper sulfide. The amount of copper sulfide loaded in the aminated polyacrylonitrile containing copper sulfide is 0.1-10wt%.
[0017] 2. The material of this application can greatly improve the antibacterial rate. On the basis of the original, it can achieve more than 80% antibacterial performance against 7 kinds of bacteria including Escherichia coli, Staphylococcus aureus, Klebsiella pneumoniae, Pseudomonas aeruginosa, Enterococcus faecalis, Candida albicans, and methicillin-resistant Staphylococcus aureus within 2 hours. At the same time, 170mw / cm 2 Xenon lamp irradiation can obtain CFU 1×10 within 30 minutes. 7 The above-mentioned bacterial liquid has a direct bactericidal effect of 99.99%.
[0018] 3. This application characterizes the synthesis of copper sulfide on the surface of APAN fibers by means of FIT-IR, XRD, XPS, SEM / EDS, etc., and tests the photocatalytic antibacterial and photothermal properties of the fiber materials. The fiber used in this technology itself has abundant amino free radical groups, which saves the step of activating the matrix material compared to other traditional fibers, and the preparation method is simple; at the same time, the material has a strong selective chelating ability for copper ions, and can efficiently and evenly capture more copper ions in the reaction solution system; using copper sulfide antibacterial agent, utilizing its photothermal properties, using a xenon lamp at 170 mw / cm 2 Experiments were conducted and the results showed that the surface raw materials have stable performance, high antibacterial efficiency, fast effectiveness, stability and no dissolution. At the same time, the application area is wide and the manufacturing cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 The XPS total spectrum of the material involved in Example 1 and the APAN / Cu-S100 corresponding S 2p and Cu 2p elemental analysis are shown.
[0021] Figure 2 These are scanning electron microscope images of the APAN fiber, APAN / CuSO4, and APAN / Cu-S100 in Example 1.
[0022] Figure 3 The infrared spectra of APAN fiber, APAN / CuSO4, APAN / Cu-S100 in Example 1 and APAN / Cu-S50 prepared in Example 2 are shown.
[0023] Figure 4 XRD spectra of APAN fiber, APAN / CuSO4, APAN / Cu-S100 in Example 1 and APAN / CuS50 prepared in Example 2.
[0024] Figure 5 This is an antibacterial test of the material in Example 1, wherein EC is Escherichia coli, SA is Staphylococcus aureus, KP is Klebsiella pneumoniae, PA is Pseudomonas aeruginosa, EF is Enterococcus faecalis, CA is Candida albicans, and MRSA is methicillin-resistant Staphylococcus aureus.
[0025] Figure 6 These are thermal images of the APAN fiber, APAN / Cu-S100 in Example 1, and APAN / CuS50 prepared in Example 2.
[0026] Figure 7 This is a photothermal antibacterial test of the APAN fiber, APAN / Cu-S100 in Example 1 and the APAN / CuS50 prepared in Example 2.
[0027] Figure 8 These are the antibacterial performance test results of the corresponding synthetic fiber materials in Examples 5 and 6 under light or without light for 5, 15, 30, 45 and 60 minutes, where A is against Escherichia coli and B is against Staphylococcus aureus.
[0028] Fig. 9These are the experimental results of capturing hydroxyl radicals and superoxide radicals of the APAN / Cu-S100 material of Example 1; wherein a is the experimental result of capturing hydroxyl radicals; and b is the experimental result of capturing superoxide radicals. DETAILED DESCRIPTION
[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Unless otherwise specified, the experimental methods used in the following experimental examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0031] Example 1 The method for preparing a copper sulfide aminated polyacrylonitrile fiber cloth of this embodiment comprises the following steps: (1) First, 3 g of polyacrylonitrile fiber was added to 30 ml of 99% or more triethylenetetramine, stirred and cross-linked at 120°C for 4 hours, then rinsed with deionized water three times, and dried in an oven at 60°C for 20 hours to prepare aminated polyacrylonitrile (APAN); (2) Take 1g of the above-mentioned aminated polyacrylonitrile and add it to 10ml of 0.15mol / L copper sulfate. Then immediately add 5ml of 0.2mol / L EDTA-2Na and react at 80℃ for 2 hours to fully chelate the material with the aminated polyacrylonitrile to achieve the Cu 2+ The ions are evenly distributed on the fiber surface to obtain the reaction solution (APAN / CuSO4 solution); (3) After adding 10 ml of 0.15 mol / L sodium sulfide to the reaction solution, the pH of the solution was controlled at 7 with acetic acid buffer solution, and the reaction was continued at 60°C for 2 hours; the obtained fiber was washed 3 times with deionized water, ultrasonically washed for 10 min, and then dried to obtain copper sulfide aminated polyacrylonitrile fiber cloth (APAN / Cu-S100).
[0032] The materials prepared in this application were characterized, such as Figure 1 and Figure 2 As shown: Depend on Figure 1 From the XPS spectrum, it can be seen that with the addition of CuSO4, compared with the original APAN peak, there are more S and Cu peaks, indicating the presence of Cu and S on the fiber surface. The S 2p spectrum of 161.9 and 163.2 corresponds to the S 2p 3 / 2 and S 2p 1 / 2The peaks indicate the presence of metal sulfides, and 167.7 and 168.8 correspond to another pair of S 2p 3 / 2 and S 2p 1 / 2 The peaks indicate the presence of metal sulfates; 932.05 and 951.79 in the Cu 2p spectrum correspond to Cu 2p 3 / 2 and Cu 2p 1 / 2 The peak indicates the presence of divalent copper ions, further confirming the synthesis of CuS on the fiber surface.
[0033] Depend on Figure 2 Electron micrographs of the intermediate materials and final products. APAN is the fiber before modification, APAN@CuSO4 is APAN that only chelates CuSO4 without adding sulfur source materials, and APAN@Cu-S100 is Cu 2+ Originated from S 2- The electron microscope image with a source addition ratio of 1:1. From the scanning electron microscope results, it can be clearly found that compared with APAN fibers, the APAN fiber material loaded with CuS forms flower-like crystals and powder coatings on the surface, indicating the synthesis of copper sulfide on the fiber surface.
[0034] Example 2 The method for preparing a copper sulfide aminated polyacrylonitrile fiber cloth of this embodiment comprises the following steps: (1) First, 3 g of polyacrylonitrile fiber was added to 30 ml of 99% or more triethylenetetramine, stirred and cross-linked at 120°C for 4 hours, then rinsed with deionized water three times, and dried in an oven at 60°C for 15 hours to prepare aminated polyacrylonitrile (APAN); (2) Take 1g of the above-mentioned aminated polyacrylonitrile and add it to 10ml of 0.3mol / L copper sulfate. Then immediately add 5ml of 0.2mol / L EDTA-2Na and react at 80℃ for 2 hours to fully chelate the material with the aminated polyacrylonitrile to achieve the Cu 2+ The ions are evenly distributed on the fiber surface to obtain the reaction solution (APAN / CuSO4 solution); (3) After adding 10 ml of 0.15 mol / L sodium sulfide to the reaction solution, the pH value of the solution was controlled at 7 with acetic acid buffer solution, and the reaction was continued at 60°C for 2 hours; the obtained fiber was washed 3 times with deionized water, ultrasonically washed for 10 min, and then dried to obtain copper sulfide aminated polyacrylonitrile fiber cloth (APAN / Cu-S50).
[0035] Example 3 The method for preparing a copper sulfide aminated polyacrylonitrile fiber cloth of this embodiment comprises the following steps: (1) First, add 3 g of polyacrylonitrile fiber to 30 ml of 99% or more triethylenetetramine, stir and crosslink at 120°C for 4 hours, then rinse with deionized water 3 times, and dry in an oven at 60°C for 15 hours to prepare amino polyacrylonitrile; (2) Take 1g of the above-mentioned aminated polyacrylonitrile and add it to 10ml of 0.3mol / L copper sulfate. Then immediately add 5ml of 0.2mol / L EDTA-2Na and react at 80℃ for 2 hours to fully chelate the material with the aminated polyacrylonitrile to achieve the Cu 2+ The effect of evenly distributing ions on the fiber surface; (3) After adding 10 ml of 0.1.875 mol / L sodium sulfide to the reaction solution, the pH of the solution was controlled at 7 with acetic acid buffer solution, and the reaction was continued at 60°C for 2 hours; the obtained fiber was washed three times with deionized water, ultrasonically washed for 10 minutes, and then dried.
[0036] Example 4 The method for preparing a copper sulfide aminated polyacrylonitrile fiber cloth of this embodiment comprises the following steps: (1) First, add 3 g of polyacrylonitrile fiber to 30 ml of 99% or more triethylenetetramine, stir and crosslink at 120°C for 4 hours, then rinse with deionized water 3 times, and dry in an oven at 60°C for 15 hours to prepare amino polyacrylonitrile; (2) Take 1g of the above-mentioned aminated polyacrylonitrile and add it to 10ml of 0.2mol / L copper sulfate. Then immediately add 5ml of 0.2mol / L EDTA-2Na and react at 80℃ for 2 hours to fully chelate the material with the aminated polyacrylonitrile to achieve the Cu 2+ The effect of evenly distributing ions on the fiber surface; (3) After adding 10 ml of 0.25 mol / L sodium sulfide to the reaction solution, the pH of the solution was controlled at 7 with acetic acid buffer solution, and the reaction was continued at 60°C for 2 hours; the obtained fiber was washed three times with deionized water, ultrasonically washed for 10 minutes, and then dried.
[0037] Example 5 The method for preparing a copper sulfide aminated polyacrylonitrile fiber cloth of this embodiment comprises the following steps: (1) First, 4.5 g of polyacrylonitrile fiber was added to 30 ml of 99% or more triethylenetetramine, stirred and cross-linked at 140°C for 3 hours, then rinsed with deionized water 3 times, and dried in an oven at 50°C for 18 hours to prepare aminated polyacrylonitrile; (2) Take 1g of the above-mentioned aminated polyacrylonitrile and add it to 10ml of 0.3mol / L copper sulfate. Then immediately add 5ml of 0.2mol / L EDTA-2Na and react at 80℃ for 2 hours to fully chelate the material with the aminated polyacrylonitrile to achieve the Cu 2+ The effect of evenly distributing ions on the fiber surface; (3) After adding 10 ml of 0.3 mol / L sodium sulfide to the reaction solution, the pH of the solution was controlled at 7 with acetic acid buffer solution, and the reaction was continued at 65°C for 1.5 hours; the obtained fiber was washed three times with deionized water, ultrasonically washed for 10 minutes, and then dried.
[0038] Example 6 The method for preparing a copper sulfide aminated polyacrylonitrile fiber cloth of this embodiment comprises the following steps: (1) First, add 2 g of polyacrylonitrile fiber to 30 ml of 99% or more triethylenetetramine, stir and crosslink at 120°C for 4 hours, then rinse with deionized water 3 times, and dry in an oven at 60°C for 24 hours to prepare amino polyacrylonitrile; (2) Take 1g of the above-mentioned aminated polyacrylonitrile and add it to 10ml of 0.3mol / L copper sulfate. Then immediately add 5ml of 0.2mol / L EDTA-2Na and react at 75℃ for 3 hours to fully chelate the material with the aminated polyacrylonitrile to achieve the Cu 2+ The effect of evenly distributing ions on the fiber surface; (3) After adding 10 ml of 0.28 mol / L sodium sulfide to the reaction solution, the pH of the solution was controlled at 7 with acetic acid buffer solution, and the reaction was continued at 65°C for 1.5 hours; the obtained fiber was washed three times with deionized water, ultrasonically washed for 10 minutes, and then dried.
[0039] Implementation effect analysis The infrared spectra of the raw material (APAN), the intermediate product (APAN / CuSO4) and the product APAN / CuS100 involved in Example 1 and the product APAN / CuS50 of Example 2 were analyzed. The results are as follows: Figure 3As shown, from the infrared spectrum, it can be observed that compared with APAN fiber, APAN / CuSO4, APAN / CuS50, and APAN / CuS100 have Cu-S stretching vibration peaks at 603 and 545, indicating the formation of CuS. At the same time, the peak value of the -CO- absorption peak at 1052 is significantly enhanced in APAN / CuSO4, and gradually weakened with the addition of sulfide, indicating that the copper sulfate chelated on the fiber surface is gradually converted into copper sulfide; at the same time, all peak types retain characteristic peaks such as 1447, 1632, 2239, and 2906, representing -NH-, -C=O-, -CN- and other groups, respectively, indicating that the fiber matrix is not damaged and the amino groups on the fiber surface are retained.
[0040] The XRD patterns of the raw material (APAN), the intermediate product (APAN / CuSO4) and the product APAN / CuS100 in Example 1 and the product APAN / CuS50 in Example 2 were analyzed as follows: Figure 4 As shown, the XRD data were taken from the surface of the fiber material. It can be clearly seen that the fiber matrix has not been changed. On this basis, there are a series of characteristic peaks at 29.8°, 32.3°, 33.4°, 48.5°, and 59.7° on the characteristic diffraction peaks, which correspond to the (102), (103), (006), (110), and (116) crystal planes of CuS (PDF#06-0464), respectively, indicating the generation of some CuS, but with irregular crystal morphology.
[0041] Application Examples 1. Antibacterial test The APAN / CuS100 fiber material in Example 6 was prepared for bacterial testing according to the steps in GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", and the test time was changed to 2 hours. The results are as follows: Figure 5 As shown: on the basis of the above, it has an antibacterial property of more than 80% against 7 kinds of bacteria including Escherichia coli (EC), Staphylococcus aureus (SA), Klebsiella pneumoniae (KP), Pseudomonas aeruginosa (PA), Enterococcus faecalis (EF), Candida albicans (CA), methicillin-resistant Staphylococcus aureus (MRSA) within 2 hours.
[0042] 2. Photothermal antibacterial test The APAN / CuS100 fiber of Example 6 was constructed according to GB / T 23763-2009 "Evaluation of antibacterial properties of photocatalytic antibacterial materials and products" to build an experimental device and conduct experimental tests on the photocatalytic antibacterial properties. The results are as follows: Figure 6 , Figure 7 and Figure 8 as shown. Figure 6 For fibers at 170 mw / cm 2 From the photothermal changes shown below, it can be seen that APAN / CuS100 can achieve higher problem improvement compared to the original APAN.
[0043] Figure 7 The thermal images at different time points can visually show the thermal changes of the material.
[0044] Figure 8 To add 170mw / cm2 to the dark environment at normal temperature 2 Xenon lamp irradiation can obtain CFU 1×10 for different bacterial species within 45 minutes. 7 The bacterial solution of Escherichia coli (EC) and Staphylococcus aureus (SA) has a direct bactericidal effect of 99.99%.
[0045] 3. Research on antibacterial principle Comparing the illumination and pressing conditions, under the illumination intensity of 170mW / cm2 of a xenon lamp (wavelength 380-760), the APAN / CuS100 of Example 6 was cut into 2mm*2mm, and 0.04ml PBS was added to the surface to simulate the bacterial liquid drop solution environment.
[0046] Hydroxyl free radicals: take 100 μl of the irradiation solution and add 100 μl of 100 mM DMPO solution. Mix well and seal the tube with a capillary. Then put it into the sample tube and put it into the machine for testing and data collection. Superoxide free radicals: take 50 μl of the irradiation solution and add 50 μl of methanol and 100 μl of 100 mM DMPO methanol solution. Mix well and seal the tube with a capillary. Then put it into the sample tube and put it into the machine for testing and data collection.
[0047] The results of the hydroxyl radical capture experiment are as follows Fig. 9 As shown in the left figure, a is the result of the hydroxyl radical capture experiment, and b is the result of the superoxide radical capture. It can be seen that hydroxyl radicals and superoxide radicals are generated under the catalysis of the xenon lamp, and the free radicals act synergistically with copper sulfide to promote more efficient sterilization results; it can be seen that the copper-aminated polyacrylonitrile fiber cloth prepared in Example 6 can generate hydroxyl radicals and superoxide radicals under the action of surface-loaded copper sulfide, and synergize with Cu salts and APAN to increase the antibacterial efficiency, reaching an antibacterial efficiency of 99.99% within 30 minutes.
[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing copper sulfide aminated polyacrylonitrile fiber cloth, characterized in that: The steps are: (1) Adding polyacrylonitrile fiber to triethylenetetramine, washing and drying after cross-linking reaction to obtain aminated polyacrylonitrile, i.e. APAN; (2) Add APAN to a copper sulfate solution, and then add EDTA-2Na solution. After chelation reaction, an aminated polyacrylonitrile solution of chelated copper, i.e., APAN@CuSO4 solution, is obtained; (3) Adding a sulfur source to the APAN@CuSO4 solution of step (2) and adjusting the pH to neutral, the reaction was continued to obtain copper sulfide aminated polyacrylonitrile fiber cloth.
2. The method for preparing the copper sulfide aminated polyacrylonitrile fiber cloth according to claim 1, characterized in that: In the step (1), 0.8-1.5 g of polyacrylonitrile fiber is added to every 10 mL of triethylenetetramine; the purity of the triethylenetetramine is greater than 90%.
3. The method for preparing the copper sulfide aminated polyacrylonitrile fiber cloth according to claim 2, characterized in that: The temperature of the cross-linking reaction is 120-140° C. and the time is 2-4 hours; the temperature of the drying is 50-60° C. and the time is 18-24 hours.
4. The method for preparing the copper sulfide aminated polyacrylonitrile fiber cloth according to claim 1, characterized in that: In the step (2), the molar amount of copper sulfate added per gram of APAN is 1.5-3 mmoL, and the molar amount of EDTA-2Na is 1 mmol; the concentration of the copper sulfate solution is 0.15-0.3 mol / L; and the concentration of the EDTA-2Na solution is 0.2 mol / L.
5. The method for preparing the copper sulfide aminated polyacrylonitrile fiber cloth according to claim 4, characterized in that: The temperature of the chelating reaction is 75-85° C. and the time is 2-3 hours.
6. The method for preparing the copper sulfide aminated polyacrylonitrile fiber cloth according to claim 1, characterized in that: The molar ratio of the Cu source to the S source in the reaction system of step (3) is (1-2):1; the S source is one or more of thiourea, sodium sulfide or sodium thiosulfate.
7. The method for preparing the copper sulfide aminated polyacrylonitrile fiber cloth according to claim 6, characterized in that: The reaction in step (3) is continued at a temperature of 55-65° C., a time of 1-2 h, and a pH of 6-8.
8. A method for preparing copper sulfide aminated polyacrylonitrile fiber cloth by the method according to any one of claims 1 to 7, characterized in that: The copper sulfide aminated polyacrylonitrile fiber cloth generates hydroxyl radicals and superoxide radicals in a water environment through copper sulfide loaded on the surface, and synergistically improves the antibacterial efficiency with Cu salt and APAN, achieving an antibacterial efficiency of 99.99% within 30 minutes.
9. The use of the copper sulfide aminated polyacrylonitrile fiber cloth as claimed in claim 8 as an antibacterial material, characterized in that: The bacteria is selected from any one of Escherichia coli, Staphylococcus aureus, Klebsiella pneumoniae, Pseudomonas aeruginosa, Enterococcus faecalis and Candida albicans.
10. The use of the copper sulfide aminated polyacrylonitrile fiber cloth as claimed in claim 8 for efficient sterilization under light induction, characterized in that: The light is 170mw / cm 2 Xenon lamp irradiation light.
Citation Information
Patent Citations
Processing method of cellulosic fiber product with photothermal effect
CN113073464A