Method for detecting calcium carbonate in titanium gypsum

By drying and burning in titanium gypsum, and then measuring carbon content in high-frequency induction combustion furnace, the problem of lack of titanium gypsum calcium carbonate detection method in the prior art is solved, and the accurate determination of calcium carbonate content is achieved and Improved detection accuracy.

CN119043985APending Publication Date: 2024-11-29ANHUI ANNADA TITANIUM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411157297.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing methods for determining calcium carbonate content in titanium gypsum lack special methods, and the existing standards are not applicable, resulting in the inability to accurately detect.

Method used

The carbon content was measured by drying titanium gypsum at 80°C, burning at 350°C and roasting in a high-frequency induction combustion furnace at 1200°C. The carbon content was calculated by combining spiking tests.

Benefits of technology

The accurate detection of calcium carbonate content in titanium gypsum is achieved, the method is simple and feasible, and the water and sulfate are removed through secondary pretreatment, which improves the detection accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119043985A_ABST
    Figure CN119043985A_ABST
Patent Text Reader

Abstract

The invention discloses a method for detecting calcium carbonate in titanium gypsum, which is characterized by comprising the following steps: (1) weighing a certain amount of titanium gypsum, drying at 80 DEG C for 3 hours by using a drying oven, cooling in a dryer, and calculating the dry basis content of the titanium gypsum as a%; (2) weighing the dried titanium gypsum, putting the titanium gypsum into a muffle furnace, firing the titanium gypsum at 350 DEG C for 1 hour, taking out the titanium gypsum, putting the titanium gypsum into a dryer, cooling the titanium gypsum, and calculating firing residues as b%; and (3) weighing 0.2 g of the burnt sample, recording as n, putting into a high-frequency induction combustion furnace, roasting at 1200 DEG C, reading the carbon content data as m%, and calculating to obtain the content of calcium carbonate. The method has the beneficial effects that the titanium gypsum is subjected to secondary pretreatment at a certain temperature, water, sulfate and sulfide in the titanium gypsum are removed, the carbon content is measured by using the high-frequency induction calcining furnace at 1200 DEG C, the calcium carbonate content in the titanium gypsum is further calculated, and the method is simple, convenient and feasible through a calcium carbonate standard addition test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sulfuric acid process titanium dioxide production technology, in particular to a method for detecting calcium carbonate in titanium gypsum. Background Art

[0002] Titanium gypsum is a wastewater treatment product in the production of titanium dioxide by sulfuric acid process. It contains calcium sulfate dihydrate, iron oxide, ferrous sulfate, titanium dioxide, calcium carbonate and other products with complex composition. The content of calcium carbonate is directly related to the energy saving and economic benefits of enterprises.

[0003] At present, the calcium carbonate analysis methods include GB / T19281-2014 "Calcium Carbonate Analysis Method", which calculates calcium carbonate by measuring calcium content. GB / T 218-2016 "Determination of Carbonate Carbonate Content in Coal", which determines carbon dioxide by hydrochloric acid-alkali asbestos absorption method, and the method is not applicable. Summary of the invention

[0004] The technical problem to be solved by the present invention is that there is no special method for determining the content of calcium carbonate in the existing titanium gypsum, and other existing standards are not applicable. Therefore, a method for detecting calcium carbonate in titanium gypsum is provided.

[0005] The technical solution of the present invention is: a method for detecting calcium carbonate in titanium gypsum, which is characterized by comprising the following steps: (1) weighing a certain amount of titanium gypsum, drying it in an oven at 80°C for 3h, placing it in a dryer for cooling, and calculating the dry basis content of the titanium gypsum as a%; (2) weighing the dried titanium gypsum, placing it in a muffle furnace, calcining it at 350°C for 1h, taking it out and placing it in a dryer for cooling, and calculating the calcination residue as b%; (3) weighing 0.2g of the sample after calcination treatment, recorded as n, placing it in a high-frequency induction combustion furnace, calcining it at 1200°C, and then reading the carbon content data as m%; according to the calculation formula Calcium carbonate content.

[0006] The certain amount of titanium gypsum in step (1) described in the above scheme is weighed using an analytical balance with a weighing accuracy of 0.001 grams.

[0007] The titanium gypsum dried in step (2) of the above scheme is weighed using an analytical balance with a weighing accuracy of 0.001 grams.

[0008] The sample after the calcination treatment in step (3) of the above scheme is weighed using an analytical balance with a weighing accuracy of 0.001 g.

[0009] The beneficial effect of the present invention is to perform secondary pretreatment on titanium gypsum at a certain temperature to remove water, sulfate and sulfide therein, and then use a high-frequency induction calcining furnace to determine the carbon content at 1200°C, and further calculate the calcium carbonate content in the titanium gypsum through a calcium carbonate spike test. The method is simple and feasible. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is the trend chart of C content after spiked. DETAILED DESCRIPTION

[0011] The technical solutions in the embodiments of the present invention are described clearly and completely below in conjunction with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0012] Measuring instrument:

[0013] Resistance furnace: rated temperature 1200℃;

[0014] Analytical balance: maximum weighing 220g, minimum weighing 10mg;

[0015] High frequency induction combustion furnace: output power greater than 2.5KVA, grounding resistance 2 ohms; oxygen purity greater than 99.5%; temperature greater than 1200℃;

[0016] Oven: 300℃;

[0017] Calcination dish: 250ml, white;

[0018] Dryer: 240mm;

[0019] Small crucible: 10ml;

[0020] Calcium carbonate: AR, purity 99%.

[0021] Determination steps:

[0022] Weigh a certain amount of titanium gypsum (accuracy 0.001 g) with an analytical balance, dry it in an oven at 80°C for 3 hours, cool it in a desiccator, and calculate the dry basis content of titanium gypsum as a%;

[0023] Weigh a certain amount of dried sample (accuracy 0.001 g), put it into a muffle furnace, burn it at 350℃ for 1h, take it out and put it into a desiccator to cool, and calculate the burning residue as b%;

[0024] Weigh 0.2 g (accuracy 0.001 g) of the sample after burning treatment, record it as n, put it into a high-frequency induction combustion furnace, bake it at 1200°C, and then read the carbon content data as m%;

[0025] Calculation formula:

[0026] Where:

[0027] n-------weight, g;

[0028] 12%-----The percentage of C content in CaCO3;

[0029]

[0030] b%-----350℃ ignition dry basis percentage;

[0031]

[0032] a%-----80℃ titanium gypsum dry basis percentage;

[0033]

[0034] Internal standard verification:

[0035] The accuracy of this analytical method was verified by adding CaCO3 (3.8) as an internal standard to the titanium gypsum sample pretreated at 350°C. The data are shown in the following table:

[0036]

[0037] like Figure 1 As shown, the linear equation after integration is Y = 50.557X + 1.1894, R2 = 0.9986, and the intercept is the initial C content of the sample without addition, which is 1.1894%, which is very close to the actual measured value of 1.1805%. Therefore, it can be considered that this method is accurate and reliable.

Claims

1. A method for detecting calcium carbonate in titanium gypsum, characterized in that: The following steps are involved: (1) Weigh a certain amount of titanium gypsum, dry it in an oven at 80°C for 3 hours, put it in a dryer to cool, and calculate the dry content of titanium gypsum as a%; (2) Weigh the dried titanium gypsum, put it in a muffle furnace, burn it at 350°C for 1 hour, take it out and put it in a dryer to cool, and calculate the burning residue as b%; (3) Weigh 0.2 grams of the sample after burning treatment, record it as n, put it in a high-frequency induction combustion furnace, bake it at 1200°C, and then read the carbon content data as m%; according to the calculation formula Calcium carbonate content.

2. A method for detecting calcium carbonate in titanium gypsum as claimed in claim 1, characterized in that: The certain amount of titanium gypsum in step (1) is weighed using an analytical balance with a weighing accuracy of 0.001 grams.

3. A method for detecting calcium carbonate in titanium gypsum as claimed in claim 1, characterized in that: The titanium gypsum dried in step (2) is weighed using an analytical balance with a weighing accuracy of 0.001 grams.

4. A method for detecting calcium carbonate in titanium gypsum as claimed in claim 1, characterized in that: The sample after the calcination treatment in step (3) is weighed using an analytical balance with a weighing accuracy of 0.001 g.