Lead frame and manufacturing method thereof

By forming a specific range of rough surfaces on the lead portion and chip socket surface of the lead frame and combining it with a metal plating layer, the problem of moisture ingress and seepage in flip-chip semiconductor devices is solved, thereby improving the reliability and manufacturing efficiency of the device.

CN119050084APending Publication Date: 2024-11-29DAI NIPPON PRINTING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411165078.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-09-01
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, flip-chip semiconductor devices are prone to problems such as moisture in the air seeping into the semiconductor element electrodes from the periphery, and epoxy resin components may seep out during the heating and curing of the chip mounting paste, affecting the reliability of the device.

Method used

By forming rough surfaces on the lead portion and chip socket of the lead frame, specifically, the upper surface and sidewalls of the lead portion have an a* value of 12 to 19 and a b* value of 12 to 17 in the CIELab color space, the arithmetic mean curvature Spc of the rough surface peaks is 700 mm-1 or more, and the arithmetic mean height Sa is 0.12 μm or more, combined with the use of a metal plating layer, the tightness of the adhesion with the sealing resin is improved, and moisture ingress is prevented.

Benefits of technology

It effectively prevents moisture in the air from seeping into the electrodes of semiconductor components, improves the reliability of semiconductor devices, reduces the risk of leakage, and enables a low-cost manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050084A_ABST
    Figure CN119050084A_ABST
Patent Text Reader

Abstract

The invention provides a lead frame and a manufacturing method thereof. The lead frame (100) is provided with a plurality of lead parts (110), at least a part of the upper surface of each lead part (110) and the side wall surface of each lead part (110) are roughened rough surfaces, and the a * value of the rough surfaces in the CIELab color space is in the range of 12-19, and the b * value of the rough surfaces in the CIELab color space is in the range of 12-17.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the Chinese invention patent application with an application date of September 1, 2022, an invention name of “Lead frame and its manufacturing method”, and an application number of 202280017475.4 (PCT / JP2022 / 033037). Technical Field

[0002] The present disclosure relates to a lead frame and a method of manufacturing the same. Background Art

[0003] In recent years, semiconductor devices mounted on substrates have been required to be miniaturized and thinned. In order to meet such requirements, various so-called QFN (Quad Flat Non-leaded package) type semiconductor devices have been proposed. The QFN type semiconductor device is configured such that a semiconductor element mounted on the mounting surface of a lead frame is sealed with a sealing resin, and a part of the lead is exposed on the back side.

[0004] Conventionally, there is known a flip-chip type semiconductor device (see Patent Document 1). In a flip-chip type semiconductor device, when a semiconductor element is mounted on a mounting substrate, the semiconductor element and the mounting substrate are connected to each other via bumps.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2002-110849

[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-40994

[0009] Generally, in a flip-chip semiconductor device, the distance from the periphery of the semiconductor device to the electrode of the semiconductor element, that is, the path through which moisture contained in the outside air (air) can penetrate, tends to be short. Therefore, moisture in the air may penetrate from the periphery of the semiconductor device to the electrode of the semiconductor element.

[0010] In addition, in the past, when manufacturing semiconductor packages for automotive applications or requiring high reliability, a semiconductor element was mounted on a die pad using a die attach film. In recent years, in such semiconductor packages, a cheaper die attach paste is also used when mounting the semiconductor element on the die pad.

[0011] However, conventionally, when the die attach paste is applied to a die pad and a semiconductor element is mounted thereon and then cured by heating, a phenomenon (bleeding) occurs in which the epoxy resin component in the die attach paste oozes out due to a capillary phenomenon (see Patent Document 2).

[0012] The present embodiment provides a lead frame capable of manufacturing a semiconductor device capable of suppressing intrusion of moisture in the air into an electrode of a semiconductor element, and a method for manufacturing the lead frame.

[0013] The present embodiment provides a lead frame and a method for manufacturing the lead frame, which can satisfactorily connect a bump to the lead frame and can suppress the intrusion of moisture from the periphery of a semiconductor device toward an electrode of a semiconductor element.

[0014] The present embodiment provides a lead frame and a method for manufacturing the lead frame, which can manufacture a lead frame having a rough surface at low cost.

[0015] The present embodiment provides a lead frame and a method for manufacturing the lead frame capable of suppressing the intrusion of moisture from the outer periphery of a semiconductor device toward an electrode of a semiconductor element.

[0016] The present embodiment provides a lead frame and a method for manufacturing the lead frame that can suppress bleeding and can suppress intrusion of moisture from the periphery of a semiconductor device toward an electrode of a semiconductor element. Summary of the invention

[0017] The embodiments of the present disclosure relate to the following [1] to

[51] .

[0018] [1] A lead frame, wherein the lead frame includes a plurality of lead portions, at least a portion of the upper surface of the lead portion and a side wall surface of the lead portion are roughened surfaces, and the roughened surfaces have a roughness of 0.044 in a CIELab color space. * The value ranges from 12 to 19, b * The value ranges from 12 to 17.

[0019] [2] A lead frame, wherein the lead frame includes a plurality of lead portions, at least a portion of the upper surface of the lead portion and a side wall surface of the lead portion are roughened surfaces, and an arithmetic mean curvature Spc of a peak vertex of the rough surface is 700 mm -1 above.

[0020] [3] The lead frame according to [2], wherein an arithmetic mean height Sa of the rough surface is greater than or equal to 0.12 μm.

[0021] [4] A lead frame according to any one of [1] to [3], wherein a portion of the upper surface of the lead portion and a side wall surface of the lead portion are the rough surface, and a metal plating layer is provided on a surface of the upper surface of the lead portion that is not the rough surface.

[0022] [5] The lead frame according to [4], wherein the metal plating layer includes at least one of an Ag plating layer, a Ni plating layer, a Pd plating layer, and an Au plating layer.

[0023] [6] The lead frame according to any one of [1] to [5], wherein the lead portion includes an inner lead portion whose wall thickness is reduced from the lower surface side of the lead portion, and the lower surface of the inner lead portion is the rough surface.

[0024] [7] A lead frame according to any one of [1] to [5], wherein the lead frame also has a chip seat portion for mounting a semiconductor element, the plurality of lead portions are arranged around the chip seat portion, and the upper surface of the chip seat portion and the side wall surface of the chip seat portion are the rough surface.

[0025] [8] A lead frame according to any one of [1] to [7], wherein the lead frame is used to manufacture a semiconductor device, the semiconductor device having a sealing portion for sealing at least the plurality of lead portions, and the upper surface of the lead portion in contact with the sealing portion and the side wall surface of the lead portion are roughened surfaces.

[0026] [9] A method for manufacturing a lead frame, wherein the method for manufacturing a lead frame comprises: a metal substrate preparation step of preparing a metal substrate having a first surface and a second surface opposite to the first surface; a metal substrate processing step of forming a plurality of lead portions by processing the metal substrate; and a rough surface forming step of roughening at least a portion of the upper surface of the lead portion and a side wall surface of the lead portion to form a rough surface, wherein in the rough surface forming step, the rough surface is subjected to a roughening process in a CIELab color space. * The value is in the range of 12 to 19, b * The roughening is performed so that the value falls within the range of 12 to 17.

[0027]

[10] A method for manufacturing a lead frame, wherein the method for manufacturing a lead frame comprises: a metal substrate preparation step of preparing a metal substrate having a first surface and a second surface opposite to the first surface; a metal substrate processing step of forming a plurality of lead portions by processing the metal substrate; and a rough surface forming step of roughening at least a portion of the upper surface of the lead portion and the side wall surface of the lead portion to form a rough surface, wherein in the rough surface forming step, the arithmetic mean curvature Spc of the peak apex of the rough surface is 700 mm. -1 The above method is used for roughening.

[0028]

[11] The method for manufacturing a lead frame according to

[10] , wherein in the rough surface forming step, the rough surface is roughened so that an arithmetic mean height Sa of the rough surface becomes equal to or greater than 0.12 μm.

[0029]

[12] The method for manufacturing a lead frame according to any one of [9] to

[11] , wherein after the rough surface forming step, the lead portion is subjected to an alkali treatment.

[0030]

[13] A method for manufacturing a lead frame according to any one of [9] to

[12] , wherein a metal plating layer is provided on a portion of the upper surface of the lead portion, and in the rough surface forming step, the upper surface and the side wall surface of the lead portion where the metal plating layer is not provided are roughened.

[0031]

[14] The method for manufacturing a lead frame according to

[13] , wherein the metal plating layer includes at least one of an Ag plating layer, a Ni plating layer, a Pd plating layer, and an Au plating layer.

[0032]

[15] A method for manufacturing a lead frame according to any one of [9] to

[14] , wherein, in the metal substrate processing step, the lead portion is formed including an inner lead portion that is thinned from the lower surface side of the lead portion, and in the rough surface forming step, the rough surface is formed on the lower surface of the inner lead portion.

[0033]

[16] A method for manufacturing a lead frame according to any one of [9] to

[15] , wherein, in the metal substrate processing step, a chip seat portion carrying a semiconductor element is formed by arranging the plurality of lead portions around the chip seat portion, and the rough surface forming step includes the following step: roughening the upper surface of the chip seat portion and the side wall surface of the chip seat portion, and at least a portion of the upper surface of the lead portion and the side wall surface of the lead portion to form the rough surface.

[0034]

[17] A lead frame, wherein the lead frame comprises: a chip seat for mounting a semiconductor element; and a lead portion located around the chip seat, a smooth surface area is formed on the front surface of the chip seat or the front surface of the lead portion, and a rough surface area exists in a manner that surrounds the entire circumference of the smooth surface area.

[0035]

[18] The lead frame according to

[17] , wherein the rough surface area is formed along the entire periphery of the chip pad or the entire periphery of the lead portion in a plan view.

[0036]

[19] A lead frame according to

[17] or

[18] , wherein the lead portion has an inner lead that is thinned from the back side, an inner lead front side is formed on the front side of the inner lead, an inner lead back side is formed on the back side of the inner lead, an inner lead end face is formed on the surface of the inner lead facing the chip seat, an external terminal is formed on a portion of the back side of the lead portion that is not thinned, the inner lead back side and the inner lead end face are rough surfaces, and the external terminal is a smooth surface.

[0037]

[20] The lead frame according to any one of

[17] to

[19] , wherein the back surface of the chip pad is a smooth surface, and the side surface of the chip pad is a rough surface.

[0038]

[21] The lead frame according to any one of

[17] to

[20] , wherein the smooth surface region is circular, elliptical, or oval in a plan view.

[0039]

[22] The lead frame according to any one of

[17] to

[20] , wherein the smooth surface region is square or rectangular in a plan view.

[0040]

[23] The lead frame according to any one of

[17] to

[20] , wherein the smooth surface area is a closed figure including curves and line segments when viewed from above.

[0041]

[24] The lead frame according to any one of

[17] to

[23] , wherein the shortest distance between the smooth surface area and the periphery of the chip pad or the lead portion is greater than or equal to 0.025 mm and less than or equal to 1.0 mm.

[0042]

[25] The lead frame according to any one of

[17] to

[24] , wherein the S-ratio of the rough surface is greater than or equal to 1.30, and the S-ratio of the smooth surface is less than 1.30.

[0043]

[26] A method for manufacturing a lead frame, wherein the method for manufacturing a lead frame comprises: a step of preparing a metal substrate; a step of forming a chip seat and a lead portion located around the chip seat by etching the metal substrate; a step of forming a plating layer on a portion of the metal substrate; a step of forming a rough surface on a portion of the metal substrate that is not covered by the plating layer; and a step of removing the plating layer, thereby forming a smooth surface area on the front side of the chip seat or the front side of the lead portion, and the rough surface area is present in a manner that surrounds the entire circumference of the smooth surface area.

[0044]

[27] A method for manufacturing a lead frame, wherein the method for manufacturing a lead frame comprises: a process of preparing a metal substrate having a chip seat and a lead portion located around the chip seat; a process of forming a plating layer on the periphery of the metal substrate except for at least a portion of the front surface; a process of leaving the plating layer existing on at least the back surface of the metal substrate and removing other plating layers; a process of forming a rough surface on a portion of the metal substrate not covered by the plating layer; and a process of removing the plating layer.

[0045]

[28] The method for manufacturing a lead frame according to

[27] , wherein, in the step of forming the plating layer, the plating layer is not formed on the entire front surface of the metal substrate.

[0046]

[29] A method for manufacturing a lead frame according to

[27] , wherein, in the step of forming the plating layer, the plating layer is formed on a portion of the front surface of the lead portion, and in the step of removing the other plating layers, the plating layer existing on a portion of the front surface of the lead portion remains.

[0047]

[30] The method for manufacturing a lead frame according to

[29] , further comprising a step of forming a metal layer on a portion of the front surface of the metal substrate after the step of removing the plating layer.

[0048]

[31] The method for manufacturing a lead frame according to any one of

[27] to

[30] , wherein the S-ratio of the rough surface is greater than or equal to 1.30.

[0049]

[32] A lead frame, wherein the lead frame comprises: a chip seat for mounting a semiconductor element; and a lead portion located around the chip seat, the lead portion having an inner lead that is thinned from the back side, an inner lead front side formed on the front side of the inner lead, an inner lead back side formed on the back side of the inner lead, an inner lead end face formed on the surface of the inner lead facing the chip seat, an external terminal formed on a portion of the back side of the lead portion that is not thinned, at least a portion of the inner lead front side, the inner lead back side, and the inner lead end face are rough surfaces, and the external terminal is a smooth surface.

[0050]

[33] The lead frame according to

[32] , wherein the entire front surface of the inner lead is a rough surface.

[0051]

[34] The lead frame according to

[32] , wherein a metal layer is formed on the front surface of the inner lead, and a portion of the front surface of the inner lead where the metal layer is formed becomes a smooth surface.

[0052]

[35] A lead frame, wherein the lead frame comprises: a chip seat for mounting a semiconductor element; and a lead portion located around the chip seat, wherein a portion of the lead portion is thinned from the back side, and on the back side of the lead portion, the thinned portion becomes a rough surface, and the non-thinned portion becomes a smooth surface.

[0053]

[36] The lead frame according to

[35] , wherein the metal layer is located on the front side of the lead portion, a first front side portion of the front side of the lead portion adjacent to the outer side of the metal layer becomes a smooth surface, and a second front side portion adjacent to the outer side of the first front side portion becomes a rough surface.

[0054]

[37] A lead frame according to

[35] , wherein the metal layer is located on the front side of the lead portion, a recess is formed on the outside of the metal layer on the front side of the lead portion, a third front side portion adjacent to the outside of the recess becomes a rough surface, and an inner surface of the recess becomes a smooth surface.

[0055]

[38] A lead frame according to

[35] , wherein the metal layer is located on the front side of the lead portion, a recess is formed on the outside of the metal layer on the front side of the lead portion, a third front side portion adjacent to the outside of the recess becomes a rough surface, and an inner surface of the recess becomes a rough surface.

[0056]

[39] The lead frame according to any one of

[35] to

[38] , wherein the front and back surfaces of the chip pad are respectively smooth surfaces, and the side surfaces of the chip pad are rough surfaces.

[0057]

[40] A lead frame according to any one of

[35] to

[39] , wherein the lead portion has an inner lead that is thinned from the back side, an inner lead end surface is formed on the surface of the inner lead facing the chip seat, and the inner lead end surface is a rough surface.

[0058]

[41] The lead frame according to any one of

[35] to

[40] , wherein the S-ratio of the rough surface is greater than 1.30, and the S-ratio of the smooth surface is less than 1.30.

[0059]

[42] A method for manufacturing a lead frame, wherein the method for manufacturing a lead frame comprises: a step of preparing a metal substrate; a step of forming a chip seat and a lead portion located around the chip seat by etching the metal substrate, wherein a portion of the lead portion is thinned from the back side; a step of forming a plating layer around the metal substrate; a step of removing a portion of the plating layer in an area where a rough surface is formed; a step of forming a rough surface in a portion of the metal substrate that is not covered by the plating layer; and a step of removing the plating layer, wherein, on the back side of the lead portion, the thinned portion becomes a rough surface and the non-thinned portion becomes a smooth surface.

[0060]

[43] A lead frame, wherein the lead frame comprises: a chip seat for mounting a semiconductor element; and a lead portion located around the chip seat, a first rough surface being formed on at least a portion of the front surface of the chip seat, and a second rough surface being formed on at least a portion of the front surface of the lead portion, the roughness of the second rough surface of the lead portion being greater than the roughness of the first rough surface of the chip seat.

[0061]

[44] The lead frame according to

[43] , wherein a third rough surface is formed on the side surface of the chip seat, and the roughness of the third rough surface of the chip seat is greater than the roughness of the first rough surface of the chip seat.

[0062]

[45] A lead frame according to

[43] or

[44] , wherein the lead portion has an inner lead that is thinned from the back side, an inner lead back side is formed on the back side of the inner lead, a fourth rough surface is formed on the back side of the inner lead, and the roughness of the fourth rough surface of the lead portion is greater than the roughness of the first rough surface of the chip seat.

[0063]

[46] A lead frame according to any one of

[43] to

[45] , wherein the lead portion has an inner lead that is thinned from the back side, an inner lead end surface is formed on the surface of the inner lead facing the chip seat, a fifth rough surface is formed on the inner lead end surface, and the roughness of the fifth rough surface of the lead portion is greater than the roughness of the first rough surface of the chip seat.

[0064]

[47] The lead frame according to any one of

[43] to

[46] , wherein a smooth surface area is formed on the front surface of the lead portion.

[0065]

[48] ​​The lead frame according to

[47] , wherein a metal layer is formed in the region of the smooth surface.

[0066]

[49] The lead frame according to

[47] , wherein the area of ​​the smooth surface is exposed to the outside.

[0067]

[50] The lead frame according to any one of

[43] to

[49] , wherein the S-ratio of the first rough surface is greater than or equal to 1.10 and less than or equal to 1.30, and the S-ratio of the second rough surface is greater than or equal to 1.30 and less than or equal to 2.30.

[0068]

[51] A method for manufacturing a lead frame, wherein the method for manufacturing a lead frame comprises: a process of preparing a metal substrate; a process of forming a chip seat and a lead portion located around the chip seat by etching the metal substrate; a process of forming a covering layer on the chip seat and the lead portion; a process of removing the covering layer existing on at least a portion of the front surface of the chip seat; a process of forming a first rough surface on a portion of the chip seat that is not covered by the covering layer; a process of removing the covering layer existing on at least a portion of the front surface of the lead portion; and a process of forming a second rough surface on a portion of the lead portion that is not covered by the covering layer, the roughness of the second rough surface of the lead portion being greater than the roughness of the first rough surface of the chip seat.

[0069] According to this embodiment, a semiconductor device can be manufactured in which intrusion of moisture in the air into the electrodes of the semiconductor element can be suppressed.

[0070] According to the present embodiment, the bump and the lead frame can be connected well, and the intrusion of moisture from the outer periphery of the semiconductor device to the electrode of the semiconductor element can be suppressed.

[0071] According to this embodiment, a lead frame having a rough surface can be manufactured at low cost.

[0072] According to this embodiment, it is possible to suppress the intrusion of moisture from the outer periphery of the semiconductor device toward the electrode of the semiconductor element.

[0073] According to the present embodiment, it is possible to suppress the seepage and to suppress the intrusion of moisture from the outer periphery of the semiconductor device toward the electrode of the semiconductor element. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 It is a top view showing the lead frame according to the first embodiment.

[0075] Figure 2 This is a partially cut-away end view of the lead frame according to the first embodiment.

[0076] Figure 3 It is a plan view showing the semiconductor device according to the first embodiment.

[0077] Figure 4 This is a partially cut-away end view of the semiconductor device according to the first embodiment.

[0078] Figure 5 This is a partially cut-away end view of a semiconductor device according to a modified example of the first embodiment.

[0079] Fig. 6A The following are process diagrams for explaining the method for manufacturing the lead frame according to the first embodiment.

[0080] Figure 6B This is a method for manufacturing a lead frame according to the first embodiment. Fig. 6A Process diagram.

[0081] Figure 6C This is a method for manufacturing a lead frame according to the first embodiment. Figure 6B Process diagram.

[0082] Fig.6D This is a method for manufacturing a lead frame according to the first embodiment. Figure 6C Process diagram.

[0083] Fig. 6E This is a method for manufacturing a lead frame according to the first embodiment. Fig.6D Process diagram.

[0084] Fig. 6F This is a method for manufacturing a lead frame according to the first embodiment. Fig. 6E Process diagram.

[0085] Figure 6G This is a method for manufacturing a lead frame according to the first embodiment. Fig. 6F Process diagram.

[0086] Figure 6H This is a method for manufacturing a lead frame according to the first embodiment. Figure 6G Process diagram.

[0087] Fig. 7A The following are process diagrams for explaining the method for manufacturing the semiconductor device according to the first embodiment.

[0088] Figure 7B The following is a method for manufacturing a semiconductor device according to the first embodiment. Fig. 7A Process diagram.

[0089] Figure 7C The following is a method for manufacturing a semiconductor device according to the first embodiment. Figure 7B Process diagram.

[0090] Fig.7D The following is a method for manufacturing a semiconductor device according to the first embodiment. Figure 7C Process diagram.

[0091] Figure 8 It is a top view showing a lead frame according to the second embodiment.

[0092] Fig. 9 is a cross-sectional view showing a lead frame according to a second embodiment (along the line Figure 8 sectional view along line IX-IX in FIG. 1 ).

[0093] Fig.10 (a) and (b) are enlarged plan views showing the surface of the chip pad and the surface of the lead portion, respectively.

[0094] Fig.11 It is a plan view showing a semiconductor device according to a second embodiment.

[0095] Fig.12 is a cross-sectional view showing a semiconductor device according to a second embodiment (along the Fig.11 sectional view along line XII-XII in FIG.

[0096] Fig.13 (a) and (b) are enlarged cross-sectional views showing bumps as connecting portions, respectively.

[0097] Fig.14 (a) to (i) are cross-sectional views showing a method for manufacturing a lead frame according to the second embodiment.

[0098] Fig.15 (a) to (d) are cross-sectional views illustrating a method for manufacturing a semiconductor device according to the second embodiment.

[0099] Fig.16 This is a partially enlarged cross-sectional view showing a semiconductor device according to a second embodiment.

[0100] Fig.17 (a) to (d) are enlarged plan views showing the surface of the die pad and the surface of the lead portion according to a modification of the second embodiment, respectively.

[0101] Fig.18 It is a plan view showing a lead frame according to a third embodiment.

[0102] Fig.19 is a cross-sectional view showing a lead frame according to a third embodiment (along the line Fig.18 sectional view along line XIX-XIX in FIG. 1 ).

[0103] Fig. 20 It is a plan view showing a semiconductor device according to a third embodiment.

[0104] Fig.21 is a cross-sectional view showing a semiconductor device according to a third embodiment (along the Fig. 20sectional view along line XXI-XXI in FIG.

[0105] Fig. 22 It is an enlarged cross-sectional view showing a bump as a connecting portion.

[0106] Fig.23 (a) to (i) are cross-sectional views showing a method for manufacturing a lead frame according to the third embodiment.

[0107] Fig.24 (a) to (d) are cross-sectional views showing a method for manufacturing a semiconductor device according to a third embodiment.

[0108] Fig.25 This is a partially enlarged cross-sectional view showing a semiconductor device according to a third embodiment.

[0109] Fig.26 It is a cross-sectional view showing a lead frame according to a fourth embodiment.

[0110] Fig. 27 It is a cross-sectional view showing a semiconductor device according to a fourth embodiment.

[0111] Fig.28 (a) to (j) are cross-sectional views showing a method for manufacturing a lead frame according to a fourth embodiment.

[0112] Fig.29 This is a partially enlarged cross-sectional view showing a semiconductor device according to a fourth embodiment.

[0113] Fig.30 It is a top view showing a lead frame according to the fifth embodiment.

[0114] Fig.31 is a cross-sectional view showing a lead frame according to a fifth embodiment (along the line Fig.30 sectional view along line XXXI-XXXI in FIG.

[0115] Fig.32 It is a top view showing a semiconductor device according to a fifth embodiment.

[0116] Fig.33 is a cross-sectional view showing a semiconductor device according to a fifth embodiment (along the Fig.32 sectional view along line XXXIII-XXXIII in FIG.

[0117] Fig.34 It is an enlarged cross-sectional view showing a bump as a connecting portion.

[0118] Fig.35 (a) to (j) are cross-sectional views showing a method for manufacturing a lead frame according to the fifth embodiment.

[0119] Fig.36(a) to (d) are cross-sectional views showing a method for manufacturing a semiconductor device according to a fifth embodiment.

[0120] Fig.37 This is a partially enlarged cross-sectional view showing a semiconductor device according to a fifth embodiment.

[0121] Fig.38 It is a cross-sectional view showing a lead frame according to the sixth embodiment.

[0122] Fig.39 It is a cross-sectional view showing a semiconductor device according to a sixth embodiment.

[0123] Fig.40 (a) to (j) are cross-sectional views showing a method for manufacturing a lead frame according to the sixth embodiment.

[0124] Fig.41 This is a partially enlarged cross-sectional view showing a semiconductor device according to a sixth embodiment.

[0125] Fig.42 It is a cross-sectional view showing a lead frame according to the seventh embodiment.

[0126] Fig.43 It is a cross-sectional view showing a semiconductor device according to a seventh embodiment.

[0127] Fig.44 (a) to (j) are cross-sectional views showing a method for manufacturing a lead frame according to the seventh embodiment.

[0128] Fig.45 This is a partially enlarged cross-sectional view showing a semiconductor device according to a seventh embodiment.

[0129] Fig.46 It is a cross-sectional view showing a lead frame according to the eighth embodiment.

[0130] Fig.47 It is a cross-sectional view showing a semiconductor device according to an eighth embodiment.

[0131] Fig.48 (a) to (j) are cross-sectional views showing a method for manufacturing a lead frame according to the eighth embodiment.

[0132] Fig.49 It is a partially enlarged cross-sectional view showing a semiconductor device according to an eighth embodiment.

[0133] Fig.50 It is a top view showing the lead frame of the ninth embodiment.

[0134] Fig.51 is a cross-sectional view showing a lead frame according to a ninth embodiment (along the line Fig.50 sectional view along line LI-LI in FIG.

[0135] Fig.52 It is a top view showing a semiconductor device according to a ninth embodiment.

[0136] Fig.53 is a cross-sectional view showing a semiconductor device according to a ninth embodiment (along the Fig.52 sectional view along line LIII-LIII in FIG.

[0137] Fig.54 (a) to (e) are cross-sectional views showing a method for manufacturing a lead frame according to the ninth embodiment.

[0138] Fig.55 (a) to (h) are cross-sectional views showing a method for manufacturing a lead frame according to the ninth embodiment.

[0139] Fig.56 (a)-(e) are cross-sectional views showing a method for manufacturing a semiconductor device according to a ninth embodiment.

[0140] Fig.57 This is a partially enlarged cross-sectional view showing a semiconductor device according to a ninth embodiment.

[0141] Fig.58 It is a cross-sectional view showing a lead frame according to a modified example of the ninth embodiment. DETAILED DESCRIPTION

[0142] (First embodiment)

[0143] Below, refer to Figures 1 to 7D The first embodiment is described. Hereinafter, the embodiments of the present disclosure will be described with reference to the accompanying drawings. It should be noted that the drawings are schematic or conceptual drawings, and the dimensions of the components, the ratio of the sizes between the components, etc. may not be the same as the actual situation. In addition, even when representing the same components, there are cases where the dimensions or ratios of each other are represented differently according to the drawings. In addition, in the drawings attached to this specification, in order to facilitate understanding, the shape, scale, aspect ratio, etc. of each part are sometimes changed or exaggerated relative to the actual object.

[0144] It should be noted that the numerical range represented by "to" in this specification etc. refers to the range containing the numerical values ​​recorded before and after "to" as the lower limit and the upper limit. In addition, in this specification etc., the terms such as "film", "sheet", "plate" are not distinguished from each other based on the difference in the name. For example, "plate" is a concept that also includes components that can be generally called "sheet", "film", etc.

[0145] [Lead frame]

[0146] The embodiment of the lead frame of the present disclosure is described. The lead frame 100 of the present embodiment is used to manufacture a semiconductor device 200 (see Figure 3 and Figure 4 The lead frame 100 includes a plurality of packaging regions 100A. The plurality of packaging regions 100A are arranged in a plurality of rows and a plurality of stages (in a matrix). Figure 1 , only a portion of the lead frame 100 centered on one packaging region 100A is shown.

[0147] The packaging region 100A is a region corresponding to a semiconductor device 200 described later and is defined by a rectangular imaginary line ( Figure 1 The area enclosed by the dotted line (see Figure 1 ). In addition, in the present embodiment, a lead frame including a plurality of packaging regions 100A is exemplified as the lead frame 100, but the present invention is not limited to this form, and the lead frame 100 may be composed of only one packaging region 100A.

[0148] In this specification, "inside" and "inner side" refer to the side facing the center direction of each package area 100A, and "outside" and "outer side" refer to the side away from the center of each package area 100A (connection bar 130 side). In addition, "upper surface" refers to the surface on the side where the semiconductor element 210 is mounted, "lower surface" refers to the surface on the opposite side of the "upper surface" and refers to the surface connected to the external mounting substrate (not shown), and "side wall surface" refers to the surface between the "upper surface" and the "lower surface" and refers to the surface constituting the thickness of the lead frame 100 (metal substrate 310).

[0149] In this specification, half etching means etching the material to be etched halfway along its thickness direction. The thickness of the material to be etched after half etching is 30% to 70%, preferably 40% to 60% of the thickness of the material to be etched before half etching.

[0150] like Figure 1 and Figure 2As shown, each packaging area 100A of the lead frame 100 includes a plurality of lead portions 110, a chip seat portion 120, and a connecting bar 130 connecting the lead portions 110. The lead portion 110 may also include an inner lead portion 111 and a terminal portion 113. The inner lead portion 111 is a portion thinned from the lower surface side, and is located on the inner side (chip seat portion 120 side) in each packaging area 100A. The terminal portion 113 is located on the outer side (connecting bar 130 side) in each packaging area 100A. The inner lead portion 111 extends from the terminal portion 113 to the chip seat portion 120 side. An internal terminal is formed on the upper surface side of the inner lead portion 111. As described later, the internal terminal is an area electrically connected to the semiconductor element 210 via the connecting component 220. On the internal terminal, a metal plating layer 112 is provided to improve the close fit with the connecting component 220.

[0151] Each lead portion 110 is connected to the semiconductor element 210 via a connection member 220 as described later, and is arranged with a space between the die pad portion 120 (see Figure 4 and Figure 5 The plurality of lead portions 110 are arranged at intervals from each other along the longitudinal direction of the connection bar 130 . Each lead portion 110 extends from the connection bar 130 .

[0152] The lead portion 110 is arranged around the chip holder portion 120. A portion of the lead portion 110 is thinned from the lower surface side. The portion thinned from the lower surface side is the inner lead portion 111. In addition, the portion of the lead portion 110 that is not thinned from the lower surface side is the terminal portion 113, and an external terminal 150 is formed on the lower surface of the terminal portion 113. The external terminal 150 is a portion electrically connected to an external mounting substrate (not shown). The external terminal 150 is a portion exposed outside the semiconductor device 200 described later.

[0153] The inner lead portion 111 is thinned from the lower surface side by, for example, half etching. The inner lead portion 111 has an inner lead portion upper surface 111A, an inner lead portion lower surface 111B opposite to the inner lead portion upper surface 111A, and an inner lead portion side wall surface. The inner lead portion upper surface 111A is a part of the upper surface of the lead portion 110. The inner lead portion side wall surface includes: a chip seat portion opposing surface 111C facing the chip seat portion 120 side; and an opposing surface in the adjacent lead portion 110. The inner lead portion lower surface 111B is located on the lower side of the lead portion 110.

[0154] The terminal portion 113 is located on the connecting bar 130 side. The terminal portion 113 is connected to the connecting bar 130. The lower surface of the terminal portion 113 constitutes the above-mentioned external terminal 150. The terminal portion 113 is not half-etched and has the same thickness as the chip holder portion 120. In addition, the lower surface side of a portion of the terminal portion 113 located on the connecting bar 130 side may be thinned and constitute a connection portion connected to the connecting bar 130.

[0155] At least a portion of the upper surface and the side wall surface of the lead portion 110 are roughened surfaces, and the lower surface of the lead portion 110 (terminal portion 113) is a non-roughened surface. The lower surface 111B of the inner lead portion is a roughened surface. Figure 1 In FIG. 1 , the roughened rough surface is indicated by the thick dashed line.

[0156] In the present embodiment, when simply referred to as a “rough surface”, the rough surface refers to a roughened rough surface, and preferably refers to a roughened rough surface roughened by microetching or the like.

[0157] The thinned portion of the lower surface of the lead portion 110 becomes a rough surface that is roughened. Specifically, the entire area of ​​the lower surface 111B of the inner lead portion is a rough surface. On the other hand, the portion of the lower surface of the lead portion 110 that is not thinned becomes a non-roughened surface. Specifically, the terminal portion 113 is not thinned from the lower surface side, and the entire area of ​​the external terminal 150 located on the lower surface side of the terminal portion 113 becomes a non-roughened surface. The side wall surface of the inner lead portion including the chip seat portion opposing surface 111C becomes a rough surface that is roughened in its entire area.

[0158] As long as a portion of the upper surface of the lead portion 110 (inner lead portion 111) located on the chip seat portion 120 side is a non-roughened surface, a metal plating layer 112 may also be provided on the non-roughened surface. The metal plating layer 112 may also be formed, for example, by electroplating. The thickness of the metal plating layer 112 may be in the range of 1 μm to 10 μm. The metal plating layer 112 may be, for example, Ag plating, Ag alloy plating, Au plating, Au alloy plating, Pt plating, Cu plating, Cu alloy plating, Pd plating, Ni plating, etc., or may include one or more of them. The metal plating layer 112 preferably includes at least one of Ag plating, Ni plating, Pd plating, and Au plating. In addition, depending on the situation of forming the metal plating layer 112, when a base plating layer is required, a known base plating layer may be applied as the base plating layer. For example, a Ni plating layer or a Cu plating layer may be used as the base plating layer.

[0159] The semiconductor element 210 is mounted on the upper surface of the chip holder 120 as described later. In addition, a plurality of lead portions 110 may be arranged around the chip holder 120. The upper surface and sidewall surface of the chip holder 120 are roughened surfaces, and the lower surface of the chip holder 120 may be a non-roughened surface (see Figure 2 ).

[0160] The upper surface of the chip holder 120 is a region (internal terminal) bonded to the semiconductor element 210 via an adhesive 240 such as a die attach paste as described later. The lower surface of the chip holder 120 is not thinned by, for example, half etching, and is a non-roughened surface that is not roughened like the metal substrate 310 before processing described later. The lower surface of the chip holder 120 is exposed to the outside in the semiconductor device 200 described later.

[0161] Each package region 100A is connected to each other by a connecting bar 130, and the connecting bar 130 extends in the X direction and the Y direction. In addition, the X direction and the Y direction refer to two directions parallel to the sides of the package region 100A in the surface of the lead frame 100, and the X direction and the Y direction are orthogonal to each other.

[0162] Each connecting bar 130 is arranged around the packaging area 100A and is arranged at a position outside the packaging area 100A. Each connecting bar 130 has a slender rod shape when viewed from above. The width W of each connecting bar 130 (the distance in the direction orthogonal to the long side direction of the connecting bar 130) is not particularly limited, and can be appropriately set in the range of 95μm to 250μm, for example. A plurality of lead portions 110 are connected to the connecting bar 130 at a predetermined interval along the long side direction of the connecting bar 130, and the chip seat portion 120 is supported on the connecting bar 130 via the suspension lead 140. In addition, the connecting bar 130 in this embodiment is not thin-walled, but is not limited to this method. For example, the connecting bar 130 can also be thin-walled from its lower surface side by half etching. For the thickness of the connecting bar 130 in this case, it can be set in consideration of the structure of the semiconductor device 200, etc. The thickness of the connecting bar 130 can be appropriately set in the range of 80μm to 200μm, for example.

[0163] The lead frame 100 of the present embodiment is used to manufacture a semiconductor device 200 having a sealing portion 230 described later, and the upper surface of the lead portion 110 and the side wall surface of the lead portion 110 in contact with the sealing portion 230 can be a rough surface that has been roughened. In addition, the upper surface of the lead portion 110 and the side wall surface of the lead portion 110 located at a position outside the packaging area 100A, and the connecting bar 130 can be a rough surface that has been roughened, or a non-roughened surface that has not been roughened. In addition, when the semiconductor device 200 is manufactured using the lead frame 100, cutting is performed along the connecting bar 130. At this time, if each packaging area 100A is molded and cut separately, if the upper surface of the connecting bar 130 is a rough surface that has been roughened, foreign matter may be generated when the lead frame 100 is cut. Therefore, by setting the upper surface of the connecting bar 130 to a non-roughened surface that has not been roughened, the generation of foreign matter can be suppressed when the semiconductor device 200 is manufactured.

[0164] In the rough surface of the lead frame 100 of the present embodiment, a in the CIELab color space is * The value ranges from 12 to 19, b * The value is in the range of 12 to 17, preferably, a * The value ranges from 13 to 18, b * The value is in the range of 12 to 16. As can be seen from the examples described below, when the a in the CIELab color space of the rough surface of the lead frame 100 of this embodiment is * Value and b * When the value is within the specified range, the surface area ratio becomes higher. Therefore, in the semiconductor device that can be manufactured using the lead frame 100, the close adhesion strength with the molding resin is improved. As a result, it is possible to suppress the moisture in the air from penetrating into the electrodes of the semiconductor element. That is, by making the a in the CIELab color space of the rough surface of the lead frame 100 of this embodiment * Value and b * The value is within the above range, and a semiconductor device that can suppress the moisture in the air from penetrating into the electrodes of the semiconductor element can be manufactured. In addition, in this embodiment, for a in the CIELab color space, * Value and b * The values ​​were measured using a spectrophotometer density and colorimeter eXact (manufactured by X-rite Corporation).

[0165] Here, the CIELab color space (L*a*b* color space) is described. The L*a*b* color space is a chromaticity diagram called CIELab recommended by CIE. * Indicates brightness, a * Indicates the degree of red / magenta or green, b * Indicates the degree of yellow or blue. *The more negative the value is, the closer it is to green, and the more positive the value is, the closer it is to red. * The more negative the value is, the closer it is to blue, and the more positive the value is, the closer it is to yellow. * When the value of L is 100, it displays white (full reflection). * When the value of L is 0, it displays black (total absorption). And the center of these three values ​​becomes the intermediate color (gray). * The movement in the axis direction indicates the change of brightness, a * b * The movement on the plane indicates the change of the color tone. In addition, the distance in the L*a*b* space corresponds to the proximity of the colors. It can be said that the closer the distance, the closer the colors. In the rough surface of the lead frame 100 of the present embodiment, the a in the CIELab color space is * The values ​​can be comparable to the above specified range between red / magenta and green, b * Values ​​can be between yellow and blue and are comparable to the range specified above.

[0166] In the lead frame 100 of the present embodiment, the arithmetic mean curvature Spc of the peak apex of the rough surface is 700 mm. -1 Above, preferably 1000mm -1 ~5000mm -1 , preferably 2000mm -1 ~4000mm -1 . It can be seen from the embodiments described below that when the arithmetic mean curvature Spc of the peak apex of the rough surface in the lead frame 100 of the present embodiment is within a specified range, it indicates that the point of contact with the contacted body is sharp. In this case, in the semiconductor device manufactured using the lead frame 100, the close adhesion strength with the molding resin is improved, and it is possible to suppress the infiltration of moisture in the air into the electrodes of the semiconductor element. That is, by making the arithmetic mean curvature Spc of the peak apex of the rough surface in the lead frame 100 of the present embodiment within the above-mentioned range, a semiconductor device that can suppress the infiltration of moisture in the air into the electrodes of the semiconductor element can be manufactured. Furthermore, the arithmetic mean height Sa of the rough surface is preferably greater than 0.12μm, and more preferably in the range of 0.12μm to 0.34μm. By making the arithmetic mean curvature Spc of the peak apex of the rough surface 700mm -1In the above, the arithmetic mean height Sa of the rough surface is within a specified range, thereby being able to manufacture a semiconductor device that can effectively inhibit moisture in the air from penetrating into the electrodes of the semiconductor element. In addition, the arithmetic mean curvature Spc of the peak vertex represents the average of the main curvatures of the peak vertex existing on the object. The sharper the peak vertex, the greater the value of the arithmetic mean curvature Spc of the peak vertex. In addition, the arithmetic mean height Sa is a parameter obtained by expanding the arithmetic mean height Ra of the line into three dimensions, that is, a surface, and is a numerical value representing the average absolute value of the difference between the height of each point and the average surface of the surface. It should be noted that in the present embodiment, the arithmetic mean curvature Spc and the arithmetic mean height Sa of the peak vertex are measured using a laser microscope VK-X 260 (manufactured by KEYENCE, measurement department) and a laser microscope VK-X 250 (manufactured by KEYENCE, controller department).

[0167] Generally, regarding the lead frame used in a QFN (Quad Flat Non-leaded package) type semiconductor device, there has been a demand in recent years for miniaturization and thinning of the semiconductor device. In such a semiconductor device, the distance from the periphery to the electrode of the semiconductor element, that is, the path through which moisture contained in the external gas (air) can penetrate, tends to be shortened, and there is a concern that moisture in the air penetrates into the electrode of the semiconductor element, causing the semiconductor device to malfunction.

[0168] Therefore, the inventors have noticed that in a lead frame for a semiconductor device, the state of the roughened rough surface of the lead frame is important. In addition, from the viewpoint of the reliability required for the semiconductor device, it has been noticed that as an index representing the state of the rough surface, the arithmetic mean curvature Spc and the arithmetic mean height Sa of the peak vertex in the CIELab color space should be focused on. Moreover, a in the CIELab color space is * The value ranges from 12 to 19. * When the value is in the range of 12 to 17, or the arithmetic mean curvature Spc at the peak of the rough surface is 700 mm -1 As described above, the inventors have found that a lead frame with high reliability required for a semiconductor device can be obtained when the arithmetic mean height Sa of the rough surface is 0.12 μm or more, thereby completing the present invention.

[0169] The rough surface of the present embodiment can be formed, for example, by roughening the metal substrate 310 described later using a micro-etching liquid. It should be noted that, as the micro-etching liquid that can be used in the present embodiment, there can be listed a micro-etching liquid containing sulfuric acid or hydrochloric acid as a main component, a micro-etching liquid containing hydrogen peroxide and sulfuric acid as a main component, and the like.

[0170] Regarding the rough surface in this embodiment, a in the CIELab color space * The value ranges from 12 to 19, b * The value is in the range of 12 to 17. In addition, the arithmetic mean curvature Spc of the peak top of the rough surface is 700 mm -1 In the above, the arithmetic mean height Sa of the rough surface is 0.12 μm or more. By having a rough surface within such a predetermined range, a semiconductor device capable of suppressing the intrusion of moisture in the air into the electrodes of the semiconductor element can be manufactured.

[0171] The lead frame 100 described above is made of metal such as copper, copper alloy or Ni alloy. The thickness of the lead frame 100 can be set in consideration of the structure of the semiconductor device 200 and can be appropriately set within a range of 80 μm to 300 μm, for example.

[0172] The lead portion 110 in the present embodiment is arranged along all four sides of the packaging region 100A, but the present invention is not limited thereto. For example, the lead portion 110 may be arranged only along two opposing sides of the packaging region 100A.

[0173] for Figure 1 and Figure 2 The lead frame 100 shown in the figure is described in the form of having a chip seat portion 120, but is not limited thereto and may not have the chip seat portion 120. For example, each lead portion 110 may also be connected to the semiconductor element 210 via a bump as a connecting member 220 as described later (see Figure 5 ).

[0174] [Semiconductor devices]

[0175] The following describes an embodiment of the semiconductor device disclosed in the present invention. Figure 3 and Figure 4 As shown, the semiconductor device 200 includes a plurality of lead portions 110 , a die pad portion 120 , a semiconductor element 210 , a connection member 220 , and a sealing portion 230 .

[0176] The semiconductor device 200 in this embodiment is a semiconductor device manufactured using the lead frame 100. Therefore, the lead portion 110 and the chip seat portion 120 in the semiconductor device 200 are provided on the lead frame 100. Therefore, the upper surface of the lead portion 110 that is closer to the outside (the side away from the chip seat portion 120) than the metal plating layer 112 and the side wall surface of the lead portion 110 are roughened surfaces. In addition, the upper surface of the chip seat portion 120 and the side wall surface of the chip seat portion 120 are also roughened surfaces. In addition, as Figure 4As shown, the lead portion 110 includes an inner lead portion 111 thinned from the lower surface side of the lead portion 110, and the lower surface 111B of the inner lead portion is a rough surface. The sealing portion 230 is closely attached to the lower surface 111B of the inner lead portion. The terminal portion 113 of the lead portion 110 is not thinned from the lower surface side. The external terminal 150 located on the lower surface of the terminal portion 113 is a non-roughened surface. The external terminal 150 is exposed from the sealing portion 230.

[0177] The a in CIELab color space of the rough surface above * The value ranges from 12 to 19, b * The value is in the range of 12 to 17. * Value and b * When the value is within the above range, it is possible to suppress the moisture in the air from entering the electrode of the semiconductor element 210 .

[0178] In addition, the arithmetic mean curvature Spc of the peak apex of the rough surface is 700 mm -1 By setting the arithmetic mean curvature Spc of the peak apex to 700 mm -1 The above can prevent moisture in the air from penetrating into the electrode of the semiconductor element 210. Furthermore, the arithmetic mean height Sa of the rough surface is preferably 0.12 μm or more, and more preferably in the range of 0.12 μm to 0.34 μm. The arithmetic mean curvature Spc of the peak of the rough surface is 700 mm -1 As described above, when the arithmetic mean height Sa of the rough surface is within a predetermined range, it is possible to more effectively suppress the intrusion of moisture in the air into the electrode of the semiconductor element 210 .

[0179] The semiconductor element 210 may be any conventionally used semiconductor element without particular limitation, and may be, for example, an integrated circuit, a large-scale integrated circuit, a transistor, a thyristor, a diode, etc. The semiconductor element 210 has a plurality of electrodes 210A to which connection members 220 are attached.

[0180] Each connecting member 220 is made of a metal material with good conductivity, such as copper or gold, and one end of each connecting member 220 is electrically connected to the electrode 210A of the semiconductor element 210, and the other end is electrically connected to the metal plating layer 112 located on each lead portion 110. In addition, as a member used as the connecting member 220, a connecting wire, a conductor such as a bump, etc. can be listed.

[0181] The sealing portion 230 seals at least the lead portion 110, the chip seat portion 120, the semiconductor element 210 and the connecting member 220. The sealing portion 230 can be made of a resin such as a thermosetting resin such as a silicone resin or an epoxy resin, a thermoplastic resin such as a PPS resin, etc. In addition, the thickness of the sealing portion 230 as a whole is not particularly limited, and can be appropriately set within a range of about 300 μm to 1500 μm, for example. In addition, when looking down at the semiconductor device 200, the length of one side of the sealing portion 230 (one side of the semiconductor device 200) is not particularly limited, and can be appropriately set within a range of about 0.2 mm to 20 mm, for example.

[0182] for Figure 3 and Figure 4 The semiconductor device 200 shown in the figure is described in a manner that it includes the chip holder 120, but is not limited thereto and may not include the chip holder 120. For example, each lead portion 110 may also serve as a connecting member 220 and be connected to the electrode 210A of the semiconductor element 210 via a bump (see Figure 5 ).

[0183] [Method for manufacturing lead frame]

[0184] by Figure 1 and Figure 2 The manufacturing method of the lead frame 100 shown is described as an example. Figure 6A to Figure 6H The following are process diagrams for explaining the method for manufacturing the lead frame according to the present embodiment.

[0185] <Metal substrate preparation process>

[0186] like Fig. 6A and Figure 6B As shown in FIG. 1 , a metal substrate 310 having a first surface 310A and a second surface 310B opposite to the first surface 310A is prepared (see FIG. 1 ). Fig. 6A ). In addition, as the metal substrate 310 that can be used in this embodiment, a pure copper substrate, a copper alloy substrate, a 42 alloy (Fe alloy with Ni being 42%) substrate, etc. can be listed, but a pure copper substrate or a copper alloy substrate is preferred. In addition, as for the metal substrate 310, a substrate that has been degreased and cleaned on the first surface 310A and the second surface 310B can also be used.

[0187] <Metal substrate processing step>

[0188] Next, a photosensitive resist 320 is applied to the first surface 310A and the second surface 310B of the metal substrate 310 and dried (see Figure 6B ) In addition, as the photosensitive resist 320 that can be used in this embodiment, a conventionally known photosensitive resist can be used.

[0189] Next, the metal substrate 310 is exposed and developed through a photomask, thereby forming a resist layer 340 having a desired opening 330 (see Figure 6C ).

[0190] Next, the metal substrate 310 is etched with an etching solution using the resist layer 340 as a corrosion-resistant film (see Fig.6D ). In addition, the etching liquid can be appropriately selected according to the material of the metal substrate 310 used. For example, when a pure copper substrate is used as the metal substrate 310, an aqueous solution of ferric chloride can usually be used as the etching liquid to spray-etch the first surface 310A and the second surface 310B of the metal substrate 310. Thus, the outer shapes of the lead portion 110, the chip seat portion 120 and the connecting bar 130 are formed. At this time, the lower surface of a part of the lead portion 110 can also be thinned by half etching to form the inner lead portion 111 and the terminal portion 113.

[0191] Next, the resist layer 340 is stripped and removed, and a cover layer 350 is formed on the surface of the etched metal substrate 310 (see Fig. 6E ). Thus, a covering layer 350 is formed around the entire circumference of the lead portion 110, the chip seat portion 120 and the connecting bar 130. The thickness of the covering layer 350 is not particularly limited, for example, as long as the thickness is greater than 0μm and less than 2μm. In addition, there is no particular limitation on the metal forming the covering layer 350, for example, silver can be used. In the case where the covering layer 350 is composed of a silver plating layer, a silver plating solution containing silver cyanide and potassium cyanide as main components can be used as a plating solution for electroplating. In addition, it is preferred that the covering layer 350 is not formed on the external terminal 150 on the lower surface of the lead portion 110 (terminal portion 113) and the lower surface of the chip seat portion 120. In order to avoid forming the covering layer 350 on the lower surface of the external terminal 150 of the lead portion 110 (terminal portion 113) and the lower surface of the chip holder portion 120, for example, the covering layer 350 may be avoided by forming an anti-etching layer 400 on the lower surface of the external terminal 150 of the lower surface of the lead portion 110 (terminal portion 113) and the lower surface of the chip holder portion 120 (see Fig. 6E ).

[0192] Next, the covering layer 350 existing in the region where the rough surface is formed is removed. Specifically, the covering layer 350 formed on the upper surface of the lead portion 110 except the region where the metal plating layer 112 is provided, the side wall surface of the lead portion 110, the lower surface of the inner lead portion 111, the upper surface of the chip holder portion 120, and the side wall surface of the chip holder portion 120 is removed (see Fig. 6F ). During this period, if Fig. 6FAs shown in the figure, elastic components 410 such as rubber gaskets are respectively arranged on the first surface 310A and the second surface 310B of the metal substrate 310, and the metal substrate 310 is clamped by a clamp 420 via the elastic components 410. Next, the covering layer 350 of the portion not covered by the elastic component 410 is peeled off and removed. As a result, the upper surface of the lead portion 110 except the region where the metal plating layer 112 is provided, the side wall surface of the lead portion 110, the lower surface of the inner lead portion 111, the upper surface of the chip holder 120, and the side wall surface of the chip holder 120 are exposed. On the other hand, the upper surface of the region where the metal plating layer 112 is formed and the covering layer 350 on the connecting bar 130 of the upper surface of the lead portion 110 covered by the elastic component 410 remain.

[0193] <Rough surface forming process>

[0194] Next, a support layer 360 (see FIG. 1 ) for supporting the metal substrate is provided on the lower surface side of the metal substrate 310. Figure 6G ). The support layer 360 may be, for example, a resist layer. After the support layer 360 is provided, a rough surface is formed by roughening the portion of the metal substrate 310 that is not covered by the cover layer 350 (see Figure 6G ). Specifically, a rough surface is formed on the upper surface of the lead portion 110 that is closer to the outside (the side away from the chip seat portion 120) than the area where the metal plating layer 112 is formed, the side wall surface of the lead portion 110, the lower surface of the inner lead portion 111, the upper surface of the chip seat portion 120, and the side wall surface of the chip seat portion 120. In order to form the rough surface, for example, a micro-etching liquid is supplied to the metal substrate 310. Thus, a rough surface can be formed on the entire metal substrate 310 except for the portion covered by the covering layer 350. It should be noted that the micro-etching liquid refers to a surface treatment agent that can slightly dissolve the metal surface to form a fine uneven rough surface. As the micro-etching liquid that can be used in this embodiment, a micro-etching liquid containing sulfuric acid or hydrochloric acid as a main component, a micro-etching liquid containing hydrogen peroxide and sulfuric acid as a main component, etc. can be listed.

[0195] In addition, in the process of forming the rough surface, the rough surface is colored by a in the CIELab color space. * The value is in the range of 12 to 19, b * The roughening was performed so that the value was in the range of 12 to 17. In addition, in the step of forming the rough surface, the arithmetic mean curvature Spc of the peak apex of the rough surface was 700 mm. -1The roughening is performed in the above manner. Furthermore, the arithmetic mean height Sa of the rough surface is preferably 0.12 μm or more, and more preferably the roughening is performed in a manner that is in the range of 0.12 μm to 0.34 μm. By forming the rough surface in such a prescribed range, a lead frame 100 can be obtained: it is possible to manufacture a semiconductor device that can suppress the penetration of moisture in the air into the electrodes of the semiconductor element.

[0196] After that, the support layer 360 and the cover layer 350 are sequentially peeled off, and the metal plating layer 112 is provided at the inner side (chip pad 120 side) end of the inner lead portion upper surface 111A, thereby obtaining Figure 1 and Figure 2 The lead frame 100 shown (see Figure 6H ). Regarding the metal plating layer 112, for example, a plating resist layer having a predetermined pattern can be formed by photolithography, and the metal plating layer 112 can be formed by electroplating in a portion not covered by the plating resist layer. In addition, the lead frame 100 produced by the above-mentioned manufacturing method can also be subjected to an alkali treatment. Specifically, the lead frame 100 is immersed in an alkaline aqueous solution. By performing the alkali treatment, the acid contained in the surface treatment agent used in the rough surface forming step is neutralized, and the corrosion of the lead frame 100 can be suppressed. It should be noted that the alkali used in the alkali treatment is not particularly limited, and for example, sodium hydroxide, potassium hydroxide, etc. can be listed. One of them can be used alone, or two or more of them can be used in combination.

[0197] [Method for manufacturing semiconductor device]

[0198] by Figure 3 and Figure 4 The method for manufacturing the semiconductor device 200 shown is described as an example. FIG. 7A to FIG. 7D The diagram is a process diagram for explaining the method for manufacturing the semiconductor device according to the present embodiment.

[0199] First, prepare to pass Figure 6A to Figure 6H The lead frame 100 (see Fig. 7A ). Next, the semiconductor element 210 is mounted on the die pad 120 of the lead frame 100. In this case, the semiconductor element 210 is mounted and fixed on the die pad 120 using an adhesive 240 such as a die attach paste (see Figure 7B ). In addition, the adhesive 240 may also be an epoxy resin adhesive containing components such as silver paste and epoxy resin. At this time, the semiconductor element 210 is arranged on the rough surface of the upper surface of the die pad 120 via the adhesive 240.

[0200] Next, the electrodes 210A of the semiconductor element 210 and the metal plating layers 112 formed on the lead portions 110 are electrically connected to each other using the connection members 220 (see Figure 7C ).

[0201] Next, the lead frame 100 is injection molded or transfer molded with a thermosetting resin or a thermoplastic resin to form the sealing portion 230 (see Fig.7D ). Thus, the lead portion 110, the die pad portion 120, the semiconductor element 210, and the connection member 220 can be sealed with resin.

[0202] Then, the lead frame 100 is cut for each package region 100A. At this time, since the upper surface of the cut connecting bar 130 is a non-roughened surface, it is possible to suppress the generation of foreign matter during cutting. In this way, each semiconductor device 200 is singulated to obtain Figure 3 and Figure 4 A semiconductor device 200 is shown.

[0203] If the semiconductor device 200 is used for a long time, moisture in the air may enter from the side or bottom surface of the semiconductor device 200. For example, moisture in the air may enter through the interface between the sealing portion 230 and the lead portion 110 or the die pad portion 120.

[0204] To address this problem, in this embodiment, a rough surface is formed on the upper surface of the lead portion 110 where the metal plating layer 112 is not provided, the side wall surface of the lead portion 110, the upper surface of the chip seat portion 120, and the side wall surface of the chip seat portion 120. The rough surface is roughened in the following manner: a in the CIELab color space of the rough surface is * The value ranges from 12 to 19, b * The value is in the range of 12 to 17, or the arithmetic mean curvature Spc of the peak of the rough surface is 700 mm -1 As above, the arithmetic mean height Sa of the rough surface is greater than 0.12 μm. As a result, the distance of the infiltration path of moisture from the interface between the sealing portion 230 and the lead portion 110 or the chip seat portion 120 to the semiconductor element 210 side becomes relatively long. Therefore, it is possible to suppress moisture from infiltrating the electrode 210A of the semiconductor element 210. In addition, by having a rough surface within the above-mentioned specified range, the close adhesion strength of the chip seat portion 120, the lead portion 110 and the sealing portion 230 can be improved, and the chip seat portion 120, the lead portion 110 and the sealing portion 230 can be suppressed from peeling off from each other.

[0205] In addition, the lead portion 110 in the present embodiment includes an inner lead portion 111 thinned from the lower surface side of the lead portion 110. The lower surface of the inner lead portion 111 is a rough surface, and thus, on the lower surface side of the semiconductor device 200, the distance of the moisture infiltration path at the interface between the sealing portion 230 and the lead portion 110 becomes longer. As a result, it is possible to suppress moisture from infiltrating the interface between the sealing portion 230 and the lead portion 110 into the electrode 210A of the semiconductor element 210. Furthermore, by having a rough surface within the above-mentioned specified range on the lower surface of the inner lead portion 111, the close adhesion strength between the lead portion 110 and the sealing portion 230 can be improved, and it is possible to suppress the lead portion 110 and the sealing portion 230 from peeling off from each other.

[0206] The embodiments described above are described to facilitate understanding of the present invention, and are not described to limit the present invention. Therefore, it is intended that each element disclosed in the above embodiments also includes all design changes or equivalents belonging to the technical scope of the present invention.

[0207] [Example]

[0208] Hereinafter, the present disclosure will be described in more detail with reference to Examples and Comparative Examples, but the present disclosure is not limited to the following Examples and the like.

[0209] [Example 1]

[0210] have Figure 1 and Figure 2 The lead frame 100 is prepared. In the lead frame 100, the upper surface and side wall surface of the lead portion 110 and the upper surface and side wall surface of the chip seat portion 120 are determined by a in the CIELab color space. * The value is 17.53, b * The value is 14.80, and the arithmetic mean curvature Spc of the peak vertex is 2431.46 mm -1 , and a rough surface with an arithmetic mean height Sa of 0.14 μm. * Value and b * The values ​​were measured using a spectrophotometer and colorimeter eXact (manufactured by X-rite), and the arithmetic mean curvature Spc and arithmetic mean height Sa of the peak apex were measured using a laser microscope VK-X260 (manufactured by KEYENCE, measurement department) and a laser microscope VK-X250 (manufactured by KEYENCE, controller department).

[0211] [Example 2]

[0212] The lead frame 100 is prepared such that the upper surface and the side wall surface of the lead portion 110 and the upper surface and the side wall surface of the chip holder portion 120 are determined by a in the CIELab color space. * The value is 16.03, b* The value is 13.84, and the arithmetic mean curvature Spc of the peak is 2952.08 mm -1 , and a rough surface having an arithmetic mean height Sa of 0.17 μm, and has the same structure as Example 1.

[0213] [Example 3]

[0214] The lead frame 100 is prepared such that the upper surface and the side wall surface of the lead portion 110 and the upper surface and the side wall surface of the chip holder portion 120 are determined by a in the CIELab color space. * The value is 15.39, b * The value is 13.16, and the arithmetic mean curvature Spc of the peak vertex is 3523.76 mm -1 , and a rough surface having an arithmetic mean height Sa of 0.22 μm, and has the same structure as Example 1.

[0215] [Example 4]

[0216] The lead frame 100 is prepared such that the upper surface and the side wall surface of the lead portion 110 and the upper surface and the side wall surface of the chip holder portion 120 are determined by a in the CIELab color space. * The value is 14.65, b * The value is 12.86, and the arithmetic mean curvature Spc of the peak is 3378.00 mm -1 , and a rough surface having an arithmetic mean height Sa of 0.21 μm, and has the same structure as Example 1.

[0217] [Comparative Example 1]

[0218] A lead frame is prepared in which the upper surface and side wall surface of the lead portion 110 and the upper surface and side wall surface of the chip holder portion 120 are formed by a in the CIELab color space. * The value is 18.59, b * The value is 17.29, and the arithmetic mean curvature Spc of the peak is 629.05 mm -1 , and a rough surface having an arithmetic mean height Sa of 0.11 μm, and has the same structure as Example 1.

[0219] [Comparative Example 2]

[0220] A lead frame is prepared in which the upper surface and side wall surface of the lead portion 110 and the upper surface and side wall surface of the chip holder portion 120 are formed by a in the CIELab color space. * The value is 10.06, b * The value is 7.18, and the arithmetic mean curvature Spc of the peak is 986.96 mm -1, and a non-roughened surface having an arithmetic mean height Sa of 0.09 μm, and other than this, the structure is the same as that of Example 1.

[0221] [Test example] Rough surface condition evaluation test

[0222] The rough surface state of each lead frame of Examples 1 to 4 and Comparative Examples 1 to 2 was observed using SEM and a laser microscope, and the shear strength of each lead frame of Examples 1 to 4 and Comparative Examples 1 to 2 was measured. The results are shown in Table 1. It should be noted that the shear strength was measured in the following manner: as a molding resin close fitting strength test (pudding cup test), a molding resin was molded on the lead frame and a shear direction was given. For the molding resin, EME-631 (manufactured by Sumitomo Bakelite Co., Ltd.) was used, and the molding resin was molded under the conditions of a molding time of 120 seconds, a molding temperature of 175±5°C, and a molding pressure of 10 MPa, and then a curing treatment was performed at 175°C for 6 hours. It should be noted that the dimensions of the molded molding resin are a height of 4 mm, a bottom diameter of 4 mm, and an upper surface diameter of 3 mm, and the bottom side is molded into a lead frame. Then, the lead frame was fixed to a bonding strength tester DAGE 4000 (manufactured by Nordson Corporation), and a shear load of 1 kg and a speed of 0.1 mm / sec were applied in the lateral direction of the mold resin on the lead frame to measure the shear strength.

[0223] [Table 1]

[0224]

[0225] As shown in Table 1, it is confirmed that if the rough surface of the lead frame 100 has a * The value ranges from 12 to 19. * The value is in the range of 12 to 17, then * Value and b * The shear strength increases compared to when the value is outside the above range. * Value and b * When the value is within the above range, in a semiconductor device manufactured using the lead frame 100 , the adhesion strength with the molding resin is improved, and intrusion of moisture in the air into the electrode 210A of the semiconductor element 210 can be suppressed.

[0226] In addition, it was confirmed that if the arithmetic mean curvature Spc of the peak apex of the rough surface of the lead frame 100 is 700 mm -1 Above, the arithmetic mean curvature Spc with the peak vertex is less than 700mm -1The shear strength is increased compared to the case of the lead frame 100 of Examples 1 to 4. Furthermore, the arithmetic mean height Sa of the rough surface of each lead frame 100 is 0.12 μm or more. Based on this result, it is inferred that by setting the arithmetic mean curvature Spc of the peak top of the rough surface to 700 mm -1 The above makes the arithmetic mean height Sa of the rough surface not less than 0.12 μm, thereby improving the close adhesion strength with the molding resin in the semiconductor device manufactured using the lead frame 100, and can inhibit the moisture in the air from penetrating into the electrode 210A of the semiconductor element 210. It should be noted that the arithmetic mean curvature Spc of the peak top of the non-roughened surface of Comparative Example 2 that has not been roughened is 700 mm. -1 This is presumably because when the lead frame of Comparative Example 2 is manufactured by rolling the metal substrate, a sharp peak of the rolling mark exists, and therefore the value of the arithmetic mean curvature Spc at the peak top is 700 mm. -1 Above. In addition, the arithmetic mean curvature Spc of the peak apex of the rough surface of the lead frame of Comparative Example 1 is smaller than the arithmetic mean curvature Spc of the peak apex of the non-roughened surface of Comparative Example 2. It is speculated that this is because, when the rough surface is formed, the peak apex of the sharp peak of the rolling mark is roughened to the extent that the rough surface is formed, and therefore, the value of the arithmetic mean curvature Spc becomes smaller. The rough surface of the lead frame 100 of Examples 1 to 4 is a rough surface that is further roughened than the rough surface of the lead frame of Comparative Example 1. Therefore, it is inferred that: as the etching deepens, the value of the arithmetic mean curvature Spc of the peak apex becomes larger.

[0227] (Second embodiment)

[0228] Next, refer to Figures 8 to 17 In the following drawings, the same parts are denoted by the same reference numerals, and a part of the detailed description may be omitted.

[0229] (Lead frame structure)

[0230] First, through Figures 8 to 10 , the outline of the lead frame of this embodiment is described. Figures 8 to 10 It is a diagram showing a lead frame according to this embodiment.

[0231] Figure 8 and Fig. 9 The lead frame 10 shown is used in manufacturing a semiconductor device 20 ( Fig.11 and Fig.12 ) is used. Such a lead frame 10 has a plurality of packaging areas 10a. The plurality of packaging areas 10a are arranged in a plurality of rows and a plurality of stages (matrix). Figure 8 In FIG. 1 , only a portion of the lead frame 10 centered on one packaging region 10 a is shown.

[0232] In this specification, "inside" and "inner side" refer to the side facing the center direction of each packaging area 10a. "Outside" and "outer side" refer to the side away from the center of each packaging area 10a (the side of the connecting bar 13). In addition, the "front side" refers to the surface on the side where the semiconductor element 21 is mounted. The "back side" refers to the surface on the opposite side of the "front side", and refers to the surface on the side connected to the external mounting substrate not shown in the figure. The "side side" refers to the surface located between the "front side" and the "back side", and is the surface that constitutes the thickness of the lead frame 10 (metal substrate).

[0233] In this specification, half etching means etching the material to be etched halfway along its thickness direction. The thickness of the material to be etched after half etching is, for example, 30% to 70%, preferably 40% to 60%, of the thickness of the material to be etched before half etching.

[0234] like Figure 8 and Fig. 9 As shown, each packaging area 10a of the lead frame 10 includes a chip pad 11 and a lead portion 12 located around the chip pad 11. Among them, a part of the lead portion 12 is thinned from the back side. The thinned portion on the back side of the lead portion 12 becomes a rough surface. The non-thinned portion on the back side of the lead portion 12 becomes a smooth surface.

[0235] The package region 10a is a region corresponding to the semiconductor device 20 (described later). Figure 8 In the present embodiment, the lead frame 10 includes a plurality of packaging regions 10 a. However, the present invention is not limited thereto, and only one packaging region 10 a may be formed on one lead frame 10 .

[0236] The package areas 10a are connected to each other by connecting bars (supporting members) 13. The connecting bars 13 support the chip holder 11 and the lead portion 12. The connecting bars 13 extend in the X direction or the Y direction. Here, the X direction and the Y direction refer to two directions parallel to the sides of the package area 10a in the surface of the lead frame 10. The X direction and the Y direction are orthogonal to each other. In addition, the Z direction is a direction perpendicular to both the X direction and the Y direction.

[0237] Each connecting bar 13 is arranged around the packaging area 10a and outside the packaging area 10a. Each connecting bar 13 has a slender rod shape when viewed from above. The width of each connecting bar 13 (the distance in the direction perpendicular to the long side direction of the connecting bar 13) can be greater than 95μm and less than 250μm. A plurality of lead portions 12 are respectively connected to each connecting bar 13 at intervals along the long side direction of the connecting bar 13. The chip seat 11 is supported by the connecting bar 13 via the suspension lead 14. The connecting bar 13 is not thin-walled, but is not limited to this, and can also be thin-walled from the back side by, for example, half etching. The thickness of the connecting bar 13 also depends on the structure of the semiconductor device 20, but can also be set to be greater than 80μm and less than 200μm.

[0238] like Fig. 9 As shown, the chip pad 11 has a chip pad front side 11a located on the front side and a chip pad back side 11b located on the back side. On the chip pad front side 11a, a semiconductor element 21 is mounted as described later. The chip pad back side 11b is exposed to the outside from the semiconductor device 20 (described later). In addition, a first chip pad side surface 11c and a second chip pad side surface 11d are formed on the side of the chip pad 11 facing the lead portion 12. The first chip pad side surface 11c is located on the chip pad front side 11a. The second chip pad side surface 11d is located on the chip pad back side 11b. In this case, the first chip pad side surface 11c and the second chip pad side surface 11d in the chip pad 11 are respectively rough surfaces. On the other hand, as described later, a smooth surface (chip pad smooth surface area 11e) and a rough surface (chip pad rough surface area 11f) are formed on the chip pad front side 11a. The chip pad back side 11b is a smooth surface.

[0239] In the present embodiment, a "rough surface" refers to a surface with an S-ratio of 1.30 or more. A "smooth surface" refers to a surface with an S-ratio of less than 1.30. A rough surface is a surface that is rougher than a smooth surface. In addition, the S-ratio of the "rough surface" is preferably greater than 1.30 and less than 2.30. The S-ratio of the "smooth surface" is preferably greater than 1.00 and less than 1.20. Here, "S-ratio" refers to the value of the surface area obtained by dividing the surface as the measurement object into multiple pixels and measuring using an optical interferometer measuring instrument by the observation area. Specifically, using VertScan manufactured by Hitachi High-Tech Science, the surface as the measurement object is divided into multiple pixels for measurement, and the obtained surface area is divided by the observation area for calculation.

[0240] The rough surface can also be formed by, for example, roughening the outer surface of the metal substrate 31 described later using a micro-etching solution mainly composed of hydrogen peroxide and sulfuric acid. The smooth surface can also be an unprocessed surface of the metal substrate 31 described later without such roughening. Fig. 9 In FIG. 1 , the roughened portion is indicated by a thick dotted line (the same applies to other cross-sectional views).

[0241] The chip pad front surface 11a of the chip pad 11 is a region (internal terminal) electrically connected to the semiconductor element 21 via the bump 26 as described later. The chip pad front surface 11a may be a region that is not thinned by half etching, etc. The chip pad front surface 11a includes a chip pad smooth surface region 11e as a smooth surface region and a chip pad rough surface region 11f as a rough surface region.

[0242] A plurality of chip pad smooth surface areas 11e may be formed on the chip pad front surface 11a. The chip pad smooth surface areas 11e are connected to the corresponding bumps 26 (see Fig.12 ). The number of chip pad smooth surface areas 11e on the chip pad 11 and the number of bumps 26 connected to the chip pad 11 may be the same. Alternatively, a plurality of bumps 26 may be arranged on one chip pad smooth surface area 11e. In this case, the number of chip pad smooth surface areas 11e on the chip pad 11 may be less than the number of bumps 26 connected to the chip pad 11.

[0243] The chip pad rough surface area 11f is rougher than the chip pad smooth surface area 11e (S-ratio is larger). Fig.10 As shown in (a), the chip pad rough surface area 11f is formed to surround the entire periphery of each chip pad smooth surface area 11e when viewed from above. That is, the chip pad smooth surface area 11e is not directly in contact with the peripheral edge 11g of the chip pad 11. In addition, the chip pad rough surface area 11f is formed along the entire area of ​​the peripheral edge 11g of the chip pad 11 when viewed from above. Figure 8 As shown in the figure, the periphery 11g of the chip pad 11 refers to the area surrounded by the plurality of (four) sides of the chip pad 11. In addition, the area of ​​the chip pad front surface 11a other than the chip pad smooth surface area 11e may be the chip pad rough surface area 11f. That is, the chip pad front surface 11a may be composed of only the plurality of chip pad smooth surface areas 11e and the chip pad rough surface areas 11f other than the plurality of chip pad smooth surface areas 11e.

[0244] like Fig.10As shown in (a), the chip pad smooth surface area 11e can be circular when viewed from above. The chip pad smooth surface area 11e is preferably larger than the bump 26 (imaginary line) when viewed from above. The width (diameter) D1 of the chip pad smooth surface area 11e can be set to be greater than 0.030 mm, or greater than 0.035 mm. The width (diameter) D1 can be less than 0.070 mm, or less than 0.065 mm. When the bump 26 is arranged at the center of the chip pad smooth surface area 11e, the shortest distance d1 between the periphery of the bump 26 and the periphery of the chip pad smooth surface area 11e can be greater than 0.005 mm, or greater than 0.010 mm. The shortest distance d1 can be less than 0.020 mm, or less than 0.015 mm. The shortest distance L1 between the chip pad smooth surface area 11e and the periphery 11g of the chip pad 11 can be greater than 0.025 mm, or greater than 0.030 mm. The shortest distance L1 can be set to 1.0 mm or less, or 0.50 mm or less. By making the chip pad smooth surface area 11e circular in a plan view, it is easy to position the circular bump 26 relative to the chip pad smooth surface area 11e. Fig.10 In (a) and (b), the smooth surface is represented by white, and the rough surface is represented by shadow ( Fig.17 The same also applies to (a)-(d).

[0245] In addition, Fig.10 In (a), when there are multiple chip seat smooth surface areas 11e on the front side 11a of the chip seat, the shortest distance M1 between adjacent chip seat smooth surface areas 11e can be greater than 0.030mm, or greater than 0.040mm. The shortest distance M1 can be set to less than 1.0mm, or less than 0.50mm. The spacing P1 between the centers of adjacent chip seat smooth surface areas 11e can be greater than 0.045mm, or greater than 0.057mm. The spacing P1 can also be set to less than 1.2mm, or less than 0.60mm. In addition, the above spacing P1 is equivalent to the spacing between the centers of adjacent bumps 26.

[0246] Reference Fig. 9 , an external terminal may be formed on the chip holder back side 11b of the chip holder 11. The external terminal may also be electrically connected to a mounting substrate (not shown). The chip holder back side 11b is not thinned by half etching, for example, but is a smooth surface similar to the metal substrate (metal substrate 31 described later) before processing. The chip holder back side 11b is exposed to the outside of the semiconductor device 20 after the semiconductor device 20 (described later) is manufactured.

[0247] Each lead portion 12 is connected to the semiconductor element 21 via a bump 26 as described below, and is disposed with a space between the die pad 11. The plurality of lead portions 12 are disposed at intervals along the longitudinal direction of the connection bar 13. Each lead portion 12 extends from the connection bar 13.

[0248] The lead portion 12 is arranged along the periphery of the chip pad 11. A portion of the lead portion 12 is thinned from the back side. In this case, the back side of the inner lead 51 described later in the lead portion 12 is thinned. In addition, an external terminal 17 is formed in a portion of the back side of the lead portion 12 that is not thinned. The external terminal 17 is electrically connected to an external mounting substrate (not shown). The external terminal 17 is exposed to the outside from the semiconductor device 20 after the semiconductor device 20 (described later) is manufactured.

[0249] like Fig. 9 As shown in FIG. 1 , the lead portion 12 includes an inner lead 51 and a terminal portion 53. The inner lead 51 is located on the inner side (chip holder 11 side). The terminal portion 53 is located on the outer side (connection bar 13 side). The inner lead 51 extends from the terminal portion 53 toward the chip holder 11 side. An internal terminal is formed on the front side of the inner lead 51. The internal terminal is a region (lead smooth surface region 12e) electrically connected to the semiconductor element 21 via the bump 26 as described later.

[0250] The inner lead 51 is thinned from the back side by, for example, half etching. The inner lead 51 has an inner lead front side 51a and an inner lead back side 51b. The inner lead front side 51a is located on the front side. In addition, an inner lead terminal surface 51c is formed on the surface of the inner lead 51 facing the chip holder 11. The inner lead back side 51b is located on the back side.

[0251] The terminal portion 53 is located on the connecting bar 13 side. The base end of the terminal portion 53 is connected to the connecting bar 13. The terminal portion 53 has a terminal portion front face 53a. The above-mentioned external terminal 17 is formed on the back face of the terminal portion 53. The terminal portion 53 is not half-etched and has the same thickness as the chip holder 11. In addition, the back face of the portion of the lead portion 12 that is closer to the connecting bar 13 than the terminal portion 53 can also be thinned and constitute a connection portion connected to the connecting bar 13.

[0252] In the present embodiment, the thin-walled portion of the back side of the lead portion 12 becomes a rough surface. Specifically, the inner lead 51 of the lead portion 12 is thin-walled from the back side. The entire area of ​​the inner lead back side 51b located on the back side of the inner lead 51 is a rough surface. On the other hand, the non-thin-walled portion of the back side of the lead portion 12 becomes a smooth surface. Specifically, the terminal portion 53 of the lead portion 12 is not thin-walled from the back side. The entire area of ​​the external terminal 17 located on the back side of the terminal portion 53 is a smooth surface.

[0253] Furthermore, the entire region of the inner lead end surface 51c of the lead portion 12 is made into a rough surface. In addition, although not shown, both side surfaces along the long side direction of the lead portion 12 may also be made into a rough surface. On the other hand, the inner lead 51 of the lead portion 12 is not thinned from the surface side. In addition, the terminal portion 53 of the lead portion 12 is not thinned from the surface side.

[0254] The lead front surface 12a is formed by the inner lead front surface 51a of the inner lead 51 and the terminal portion front surface 53a of the terminal portion 53. The lead front surface 12a is a region that is not thinned from the surface side by half etching or the like. A lead smooth surface region 12e as a smooth surface region and a lead rough surface region 12f as a rough surface region are formed on the lead front surface 12a.

[0255] A lead smooth surface region 12e is formed on the lead front surface 12a of each lead portion 12. Alternatively, a plurality of lead smooth surface regions 12e may be formed on the lead front surface 12a of each lead portion 12. The lead smooth surface regions 12e are connected to corresponding bumps 26 (see Fig.12 ). In addition, a plurality of bumps 26 may be arranged in one lead smooth surface region 12e. In this case, the number of lead smooth surface regions 12e on each lead portion 12 may be less than the number of bumps 26 connected to the lead portion 12.

[0256] There is a lead rough surface region 12f around the lead smooth surface region 12e. The lead rough surface region 12f is rougher than the lead smooth surface region 12e (S-ratio is larger). Fig.10 As shown in (b), the lead rough surface region 12f is formed to surround the entire circumference of each lead smooth surface region 12e when viewed from above. That is, the lead smooth surface region 12e is not directly in contact with the peripheral edge 12g of the lead portion 12. In addition, the lead rough surface region 12f is formed along the entire area of ​​the peripheral edge 12g of the lead portion 12 when viewed from above. Figure 8 As shown in the figure, the periphery 12g of the lead portion 12 refers to the area surrounded by the plurality of (three) sides of the lead portion 12 and the connecting bar 13. In addition, the area other than the lead smooth surface area 12e in the lead front surface 12a may be the lead rough surface area 12f. That is, the lead front surface 12a may be composed only of the lead smooth surface area 12e and the lead rough surface area 12f other than the lead smooth surface area 12e.

[0257] like Fig.10As shown in (b), the lead smooth surface area 12e may also be circular when viewed from above. The shape of the lead smooth surface area 12e may be the same as or different from the above-mentioned chip seat smooth surface area 11e. In addition, the lead smooth surface area 12e is preferably larger than the bump 26 (imaginary line) when viewed from above. The width (diameter) D2 of the lead smooth surface area 12e may be greater than 0.030 mm, or greater than 0.035 mm. The width (diameter) D2 may be less than 0.070 mm, or less than 0.065 mm. When the bump 26 is arranged at the center of the lead smooth surface area 12e, the shortest distance d2 between the periphery of the bump 26 and the periphery of the lead smooth surface area 12e may be greater than 0.005 mm, or greater than 0.010 mm. The shortest distance d2 may be less than 0.020 mm, or less than 0.015 mm. The shortest distance L2 between the lead smooth surface region 12e and the periphery 12g of the lead portion 12 may be 0.025 mm or more, or 0.030 mm or more. The shortest distance L2 may be 1.0 mm or less, or 0.50 mm or less. By making the lead smooth surface region 12e circular in a plan view, it is easy to position the circular bump 26 relative to the chip pad smooth surface region 11e.

[0258] The lead frame 10 described above is entirely made of metal such as copper, copper alloy, 42 alloy (Fe alloy containing 42% Ni), etc. The thickness of the non-thinned portion of the lead frame 10 also depends on the structure of the semiconductor device 20 to be manufactured, but may be set to 80 μm to 300 μm.

[0259] In the present embodiment, the lead portions 12 are arranged along all four sides of the packaging region 10 a , but the present invention is not limited thereto, and for example, the lead portions 12 may be arranged only along two opposing sides of the packaging region 10 a .

[0260] (Structure of Semiconductor Device)

[0261] Next, use Figures 11 to 13 A semiconductor device according to this embodiment will be described. Figures 11 to 13 It is a diagram showing a semiconductor device (flip chip type) according to this embodiment.

[0262] like Fig.11 and Fig.12 As shown, the semiconductor device (semiconductor package) 20 includes a die pad 11 , a semiconductor element 21 , a plurality of lead portions 12 , a plurality of bumps 26 , and a sealing resin 23 .

[0263] The semiconductor element 21 is mounted on the chip holder 11 and the lead portion 12. The plurality of bumps 26 electrically connect the semiconductor element 21 to the chip holder 11 or the lead portion 12. In this case, the bumps 26 constitute a connecting portion. In addition, the bumps 26 may also be columns. The sealing resin 23 performs resin sealing on the chip holder 11, the lead portion 12, the semiconductor element 21, and the bumps 26.

[0264] The chip holder 11 and the lead portion 12 are made of the lead frame 10 described above. In this case, the inner lead 51 of the lead portion 12 is thinned from the back side. The inner lead back side 51b of the inner lead 51 is a rough surface. The sealing resin 23 is closely attached to the inner lead back side 51b. The terminal portion 53 of the lead portion 12 is not thinned from the back side. The external terminal 17 located on the back side of the terminal portion 53 is a smooth surface. The external terminal 17 is exposed to the outside from the sealing resin 23.

[0265] Bumps 26 are provided on the chip pad 11 and the lead portion 12, respectively. The bumps 26 on the chip pad 11 are provided in the chip pad smooth surface area 11e. The bumps 26 are provided at a distance d1 from the chip pad rough surface area 11f. The bumps 26 on the lead portion 12 are provided in the lead smooth surface area 12e. The bumps 26 are provided at a distance d2 from the lead rough surface area 12f. The semiconductor element 21 is electrically connected to the chip pad 11 and the lead portion 12 via the bumps 26.

[0266] As the semiconductor element 21 , various conventionally used semiconductor elements can be used without particular limitation, and examples thereof include integrated circuits, large-scale integrated circuits, transistors, thyristors, diodes, etc. The semiconductor element 21 has a plurality of electrodes 21 a each having a bump 26 mounted thereon.

[0267] As the sealing resin 23, a thermosetting resin such as silicone resin, epoxy resin, or a thermoplastic resin such as PPS resin can be used. The overall thickness of the sealing resin 23 can also be set to about 300 μm or more and 1500 μm or less. In addition, one side of the sealing resin 23 (one side of the semiconductor device 20) can be, for example, 0.2 mm or more and 20 mm or less, or 0.2 mm or more and 16 mm or less. In addition, Fig.11 In FIG. 1 , the portion of the sealing resin 23 that is closer to the front side than the lead portion 12 and the semiconductor element 21 is omitted.

[0268] The bump (connecting portion) 26 is made of, for example, a metal material with good conductivity such as copper, and may also have a solid roughly cylindrical shape or a roughly spherical shape. The upper ends of the bumps 26 are respectively connected to the electrodes 21a of the semiconductor element 21, and the lower ends of the bumps 26 are respectively connected to the chip seat smooth surface area 11e or the lead smooth surface area 12e. The width (diameter) of the bump 26 may also be set to be greater than 0.01mm and less than 0.070mm. In addition, it is not necessary to set the bump 26 on the chip seat 11. In this case, the chip seat 11 and the semiconductor element 21 may also be fixed to each other by, for example, an adhesive such as a chip bonding paste.

[0269] Fig.13 (a) and (b) are enlarged cross-sectional views showing the periphery of the bump 26. Fig.13 As shown in (a), the bump 26 may be composed of a single layer. In this case, the bump 26 may include a metal layer such as copper. The bump 26 may also be composed of the same metal as the main metal (such as copper) included in the chip pad 11 and the lead portion 12. The height of the bump 26 may be set to be greater than 30 μm and less than 110 μm.

[0270] Or, if Fig.13 As shown in (b), the bump 26 may include multiple layers. For example, the bump 26 includes: a first layer 26a located on the chip seat 11 side or the lead portion 12 side; and a second layer 26b located on the semiconductor element 21 side. The first layer 26a may include, for example, a metal such as tin. The height of the first layer 26a may be set to be greater than 1 μm and less than 10 μm. The second layer 26b may include, for example, a metal such as copper. The height of the second layer 26b may be greater than 30 μm and less than 100 μm.

[0271] In addition, the structure of the die pad 11 and the lead portion 12 is the same as that of the above-mentioned embodiment except for the region not included in the semiconductor device 20. Figures 8 to 10 The structures shown are the same, so detailed description is omitted here.

[0272] (Lead frame manufacturing method)

[0273] Next, use Fig.14 (a)-(i) Figure 8 and Fig. 9 A method for manufacturing the lead frame 10 shown will be described. Fig.14 (a)-(i) are cross-sectional views showing a method of manufacturing the lead frame 10 (with Fig. 9 corresponding figure).

[0274] First, if Fig.14As shown in (a), a flat metal substrate 31 is prepared. As the metal substrate 31, a substrate made of metal such as copper, copper alloy, 42 alloy (Fe alloy with Ni as 42%) can be used. In addition, for the metal substrate 31, it is preferable to use a substrate whose both sides have been degreased and cleaned.

[0275] Next, photosensitive resists 32a and 33a are applied to the entire front and back surfaces of the metal substrate 31, respectively, and dried ( Fig.14 (b)). In addition, as the photosensitive resists 32a and 33a, conventionally known photosensitive resists can be used.

[0276] Next, the metal substrate 31 is exposed and developed through a photomask to form etching resist layers 32 and 33 ( Fig.14 (c)).

[0277] Next, the metal substrate 31 is etched using the etching resist layer 32 and the etching resist layer 33 as a corrosion-resistant film using an etching solution ( Fig.14 (d)). In addition, the etching liquid can be appropriately selected according to the material of the metal substrate 31 used. For example, when copper is used as the metal substrate 31, an aqueous solution of ferric chloride can usually be used as the etching liquid, and spray etching is performed from both sides of the metal substrate 31. As a result, the outer shapes of the chip seat 11, the lead portion 12 and the connecting bar 13 are formed. At this time, a part of the lead portion 12 is thinned from the back side by half etching. Specifically, the back side of the inner lead 51 of the lead portion 12 is thinned.

[0278] Next, the etching resist layers 32 and 33 are peeled off and removed ( Fig.14 (e)). In this way, a metal substrate 31 including a die pad 11 and lead portions 12 located around the die pad 11 is obtained.

[0279] Next, a plating layer 36 ( Fig.14(f)). At this time, first, an elastic member 46 such as a rubber gasket having an opening of a prescribed pattern is arranged on the front side of the metal substrate 31. In addition, the opening of the elastic member 46 has a shape corresponding to the chip seat smooth surface area 11e and the lead smooth surface area 12e. Next, the front side of the metal substrate 31 is pressed by a tool 47 through the elastic member 46. The tool 47 has an opening of the same pattern as the elastic member 46. Next, a plating layer 36 is formed on the portion of the front side of the metal substrate 31 that is not covered by the elastic member 46 and the tool 47. Thus, a plating layer 36 is formed on the portion of the chip seat 11 corresponding to the chip seat smooth surface area 11e and the portion of the lead portion 12 corresponding to the lead smooth surface area 12e. The thickness of the plating layer 36 may also be greater than 0μm and less than 2μm. As a metal constituting the plating layer 36, for example, silver can be used. When the plating layer 36 is composed of a silver plating layer, a silver plating solution containing silver cyanide and potassium cyanide as main components can be used as a plating solution for electroplating.

[0280] Next, the elastic member 46 and the tool 47 are removed. In addition, a support layer 37 ( Fig.14 (g)). The support layer 37 may be, for example, a resist layer.

[0281] Then, if Fig.14 As shown in (h), by roughening the portion of the metal substrate 31 that is not covered by the plating layer 36 and the supporting layer 37, a rough surface is formed in the portion. Specifically, a chip seat rough surface area 11f and a lead rough surface area 12f are formed on the metal substrate 31. In addition, the first chip seat side surface 11c, the second chip seat side surface 11d, the inner lead end surface 51c and the inner lead back surface 51b are rough surfaces. During this period, a micro-etching liquid is supplied to the metal substrate 31, thereby forming a rough surface on the entire metal substrate 31 except for the portion covered by the plating layer 36 and the supporting layer 37. Here, the micro-etching liquid refers to a surface treatment agent that slightly dissolves the metal surface to form a fine uneven rough surface. For example, when roughening a metal substrate 31 composed of copper or a copper alloy, a micro-etching liquid with hydrogen peroxide and sulfuric acid as main components can be used.

[0282] Then, if Fig.14 As shown in (i), the support layer 37 and the plating layer 36 are peeled off and removed in sequence to obtain Figure 8 and Fig. 9 The lead frame 10 is shown.

[0283] (Method for manufacturing semiconductor device)

[0284] Next, use Fig.15 (a)-(d) Fig.11 and Fig.12A method for manufacturing the semiconductor device 20 shown will be described. Fig.15 (a) to (d) are cross-sectional views showing a method for manufacturing the semiconductor device 20 (with Fig.12 corresponding figure).

[0285] First, for example, by Fig.14 The method shown in (a)-(i) is used to manufacture the lead frame 10 ( Fig.15 (a)).

[0286] Next, the semiconductor element 21 is mounted on the die pad 11 and the lead portion 12 of the lead frame 10. In this case, bumps 26 are formed in advance on the electrodes 21a of the semiconductor element 21. Next, the bumps 26 are connected and fixed to the die pad 11 and the lead portion 12 ( Fig.15 (b)). At this time, each electrode 21a of the semiconductor element 21 is electrically connected to the chip pad 11 and the lead portion 12 via the bump 26. The bump 26 on the chip pad 11 is connected to the chip pad smooth surface area 11e. At this time, the bump 26 is set separately from the chip pad rough surface area 11f. In addition, the bump 26 on the lead portion 12 is connected to the lead smooth surface area 12e. At this time, the bump 26 is set separately from the lead rough surface area 12f.

[0287] Next, the lead frame 10 is injection molded or transfer molded with a thermosetting resin or a thermoplastic resin to form a sealing resin 23 ( Fig.15 (c)). Thus, the die pad 11, the lead portion 12, the semiconductor element 21, and the bump 26 are sealed with resin.

[0288] Then, the lead frame 10 and the sealing resin 23 are cut for each package region 10a. Thus, the lead frame 10 is separated for each semiconductor device 20 to obtain Fig.11 and Fig.12 The semiconductor device 20 ( Fig.15 (d)).

[0289] However, it is conceivable that during long-term use of the semiconductor device 20 manufactured in this way, moisture in the air or the like may intrude from the side surface or back surface of the semiconductor device 20 through the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 .

[0290] In this regard, according to the present embodiment, the chip pad rough surface region 11f exists in a manner surrounding the entire circumference of the chip pad smooth surface region 11e. Similarly, the lead rough surface region 12f exists in a manner surrounding the entire circumference of the lead smooth surface region 12e. Therefore, on the outside of the bump 26, the distance of the moisture intrusion path at the interface between the chip pad front surface 11a or the lead front surface 12a and the sealing resin 23 becomes longer. As a result, it is possible to suppress the moisture from intruding from the interface between the chip pad front surface 11a or the lead front surface 12a and the sealing resin 23 to the semiconductor element 21 side (see Fig.16 Arrow F A ). As a result, the reliability of the semiconductor device 20 after long-term use can be improved.

[0291] According to the present embodiment, the die pad smooth surface region 11e adjacent to the outside of the bump 26 in the die pad front surface 11a is a smooth surface. Also, the lead smooth surface region 12e adjacent to the outside of the bump 26 in the lead front surface 12a is a smooth surface.

[0292] Therefore, when the bump 26 is composed of a single metal layer such as copper (see Fig.13 (a)) can achieve the following effects. That is, when the semiconductor element 21 is mounted on the chip holder 11 and the lead portion 12, the close fit between the bump 26 and the chip holder 11 and the lead portion 12 can be improved. On the other hand, if the surface of the chip holder 11 and the lead portion 12 to which the bump 26 is connected is a rough surface, the contact area between the bump 26 and the rough surface becomes smaller due to the influence of the oxide film (e.g., copper oxide) formed on the rough surface. In this case, the bonding strength between the bump 26 and the chip holder 11 and the lead portion 12 may be weakened.

[0293] In addition, when the bump 26 contains a metal such as tin (see Fig.13 (b)) can obtain the following effect. That is, when the semiconductor element 21 is mounted on the chip pad 11 and the lead portion 12, it is possible to suppress the tin and the like contained in the bump 26 from flowing out along the rough surface. On the other hand, if the portion adjacent to the outer side of the bump 26 is a rough surface, the tin and the like contained in the bump 26 may flow out along the rough surface due to surface tension.

[0294] According to the present embodiment, the die pad rough surface region 11f is formed along the entire area of ​​the peripheral edge 11g of the die pad 11 in a plan view. Also, the lead rough surface region 12f is formed along the entire area of ​​the peripheral edge 12g of the lead portion 12 in a plan view. Thus, it is possible to more effectively suppress the intrusion of moisture from the interface between the die pad front surface 11a or the lead front surface 12a and the sealing resin 23 to the semiconductor element 21 side.

[0295] In addition, according to the present embodiment, the inner lead back surface 51b and the inner lead end surface 51c of the lead portion 12 are roughened. In addition, the first chip pad side surface 11c and the second chip pad side surface 11d of the chip pad 11 are roughened. Therefore, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the chip pad 11 or the lead portion 12 becomes longer. As a result, it is possible to suppress the moisture from intruding from the interface between the sealing resin 23 and the chip pad 11 or the lead portion 12 to the semiconductor element 21 side (see Fig.16 Arrow F B ). As a result, the reliability of the semiconductor device 20 after long-term use can be improved.

[0296] In particular, in the flip-chip type semiconductor device 20, the electrode 21a of the semiconductor element 21 faces the back side. Therefore, in the flip-chip type semiconductor device 20, the distance from the back side of the semiconductor device 20 to the electrode 21a of the semiconductor element 21 is likely to be shortened. In contrast, according to the present embodiment, the thinned portion of the back side of the lead portion 12 becomes a rough surface. As a result, it is possible to more effectively suppress the intrusion of moisture from the interface between the sealing resin 23 and the lead portion 12 to the semiconductor element 21 side.

[0297] In addition, according to the present embodiment, the inner lead back surface 51b and the inner lead end surface 51c of the lead portion 12 are roughened. In addition, the first die pad side surface 11c and the second die pad side surface 11d of the die pad 11 are roughened. Thus, the close adhesion strength between the die pad 11 and the lead portion 12 and the sealing resin 23 can be improved, thereby preventing the die pad 11 and the lead portion 12 from peeling off from the sealing resin 23.

[0298] (Variation Example)

[0299] Next, according to Fig.17 (a) to (d) of FIG. 1 describe variations of the chip pad smooth surface region 11e and the lead smooth surface region 12e. Fig.17 (a)-(d) are enlarged top views of the chip base smooth surface area 11e and the lead smooth surface area 12e (hereinafter, also referred to as the smooth surface areas 11e and 12e), and the chip base rough surface area 11f and the lead rough surface area 12f (hereinafter, also referred to as the rough surface areas 11f and 12f).

[0300] like Fig.17As shown in (a), the smooth surface areas 11e and 12e can be square or rectangular when viewed from above. The width (length of each side) D3 of the smooth surface areas 11e and 12e can be greater than 0.030 mm, or greater than 0.035 mm. The width D3 can be less than 0.070 mm, or less than 0.065 mm. In addition, when the bump 26 is arranged at the center of the smooth surface areas 11e and 12e, the shortest distance d3 between the periphery of the bump 26 and the periphery of the smooth surface areas 11e and 12e can be set to be greater than 0.005 mm, or greater than 0.010 mm. The shortest distance d3 can be set to be less than 0.020 mm, or less than 0.015 mm. In addition, the shortest distance L3 between the smooth surface areas 11e and 12e and the periphery 11g of the chip seat 11 or the periphery 12g of the lead portion 12 can be greater than 0.025 mm, or greater than 0.030 mm. The shortest distance L3 may be 1.0 mm or less, or 0.50 mm or less. By making the smooth surface regions 11e and 12e square or rectangular in plan view, the shortest distance (interval) d3 between the periphery of the bump 26 and the periphery of the smooth surface regions 11e and 12e can be sufficiently ensured.

[0301] like Fig.17As shown in (b), the smooth surface areas 11e and 12e are square or rectangular when viewed from above, and multiple bumps 26 can also be arranged in one smooth surface area 11e and 12e. The length D4a of the long side of the smooth surface area 11e and 12e can be greater than 0.045mm, or greater than 0.065mm. The length D4a can be less than 0.12mm, or less than 0.10mm. The length D4b of the short side of the smooth surface area 11e and 12e can be greater than 0.030mm, or greater than 0.035mm. The length D4b can be less than 0.070mm, or less than 0.065mm. In addition, when each bump 26 is arranged at the center of the short side direction of the smooth surface area 11e and 12e, the shortest distance d4 between the periphery of the bump 26 and the periphery of the smooth surface area 11e and 12e in the short side direction can be greater than 0.005mm, or greater than 0.010mm. The shortest distance d4 can be less than 0.020 mm, or less than 0.015 mm. In addition, the shortest distance L4 between the smooth surface area 11e, 12e and the periphery 11g of the chip seat 11 or the periphery 12g of the lead portion 12 can be set to be greater than 0.025 mm, or greater than 0.030 mm. The shortest distance L4 can be less than 1.0 mm, or less than 0.50 mm. By making the smooth surface areas 11e, 12e square or rectangular when viewed from above, the shortest distance (interval) d4 between the periphery of the bump 26 and the periphery of the smooth surface areas 11e, 12e can be fully ensured. In addition, two or more bumps 26 adjacent to each other can be provided in each smooth surface area 11e, 12e.

[0302] like Fig.17As shown in (c), the smooth surface areas 11e and 12e are ellipses or elongated circles when viewed from above, and multiple bumps 26 may be arranged in one smooth surface area 11e and 12e. The length D5a of the smooth surface areas 11e and 12e in the longitudinal direction may be greater than 0.045 mm, or greater than 0.065 mm. The length D5a may be less than 0.12 mm, or less than 0.10 mm. The length D5b of the smooth surface areas 11e and 12e in the short side direction may be set to greater than 0.030 mm, or greater than 0.035 mm. The length D5b may be set to less than 0.070 mm, or less than 0.065 mm. In addition, when each bump 26 is arranged at the center of the short side direction of the smooth surface areas 11e and 12e, the shortest distance d5 between the periphery of the bump 26 and the periphery of the smooth surface areas 11e and 12e may be set to greater than 0.005 mm, or greater than 0.010 mm. The shortest distance d5 can be set to be less than 0.020 mm, or less than 0.015 mm. In addition, the shortest distance L5 between the smooth surface area 11e, 12e and the peripheral edge 11g of the chip holder 11 or the peripheral edge 12g of the lead portion 12 can be greater than 0.025 mm, or greater than 0.030 mm. The shortest distance L5 can be set to be less than 1.0 mm, or less than 0.50 mm. By making the smooth surface areas 11e, 12e elliptical or oblong when viewed from above, two or more bumps 26 adjacent to each other can be provided in each smooth surface area 11e, 12e.

[0303] like Fig.17As shown in (d), the periphery of the smooth surface regions 11e and 12e may be a closed figure including the curve Cv and the line segment Ls when viewed from above. The smooth surface regions 11e and 12e may also be a figure formed by removing a part of a circle or an ellipse, such as a semicircle or a semi-ellipse. The line segment Ls constituting the periphery of the smooth surface regions 11e and 12e may be parallel to the periphery 11g of the chip holder 11 or the periphery 12g of the lead portion 12. The length D6a of the smooth surface regions 11e and 12e in a direction orthogonal to the line segment Ls may be greater than 0.030 mm, or greater than 0.050 mm. The length D6a may be less than 0.12 mm, or less than 0.10 mm. The length D6b of the smooth surface regions 11e and 12e in a direction parallel to the line segment Ls may be greater than 0.030 mm, or greater than 0.035 mm. The length D6b can be set to be less than 0.070 mm, or less than 0.065 mm. In addition, when each bump 26 is arranged at the center of the smooth surface area 11e, 12e in the direction parallel to the line segment Ls and the direction orthogonal to the line segment Ls, the shortest distance d6 between the periphery of the bump 26 and the periphery of the smooth surface area 11e, 12e can be set to be greater than 0.005 mm, or greater than 0.010 mm. The shortest distance d6 can be set to be less than 0.020 mm, or less than 0.015 mm. In addition, the shortest distance L6 between the smooth surface area 11e, 12e and the periphery 11g of the chip seat 11 or the periphery 12g of the lead portion 12 can be set to be greater than 0.025 mm, or greater than 0.030 mm. The shortest distance L6 can be set to be less than 1.0 mm, or less than 0.50 mm. By making the smooth surface regions 11e and 12e a closed figure including the curve Cv and the line segment Ls in a plan view, the shortest distance L6 between the smooth surface regions 11e and 12e and the periphery 11g of the die pad 11 or the periphery 12g of the lead portion 12 can be ensured to be greater than a certain distance.

[0304] (Third embodiment)

[0305] Next, refer to Figures 18 to 25 A third embodiment will be described. Figures 18 to 25 FIG. 3 is a diagram showing a third embodiment. Figures 18 to 25 In, with Figures 8 to 17 The same parts as shown in the above-mentioned embodiments are denoted by the same reference numerals and detailed description thereof will be omitted.

[0306] (Lead frame structure)

[0307] First, use Fig.18 and Fig.19 The outline of the lead frame according to the present embodiment will be described. Fig.18 and Fig.19It is a diagram showing a lead frame according to this embodiment.

[0308] In this specification, the “outer periphery” refers to a portion of the lead frame 10 (metal substrate) exposed to the outside, and is a region including the “front side”, “side side”, and “back side”.

[0309] like Fig.18 and Fig.19 As shown, each packaging area 10a of the lead frame 10 includes a chip pad 11 and a lead portion 12 located around the chip pad 11. Among them, a part of the lead portion 12 is thinned from the back side. The thinned portion on the back side of the lead portion 12 becomes a rough surface. The non-thinned portion on the back side of the lead portion 12 becomes a smooth surface.

[0310] like Fig.19 As shown, the chip pad 11 has a chip pad front side 11a located on the front side and a chip pad back side 11b located on the back side. In this case, the chip pad front side 11a, the first chip pad side surface 11c and the second chip pad side surface 11d in the chip pad 11 are respectively rough surfaces. On the other hand, the chip pad back side 11b in the chip pad 11 is a smooth surface.

[0311] like Fig.19 As shown in FIG. 1 , the lead portion 12 includes an inner lead 51 and a terminal portion 53. The inner lead 51 is located on the inner side (chip holder 11 side). The terminal portion 53 is located on the outer side (connection bar 13 side). The inner lead 51 extends from the terminal portion 53 toward the chip holder 11 side. An internal terminal is formed at the end portion of the front side of the inner lead 51. As described later, the internal terminal is a region electrically connected to the semiconductor element 21 via the bump 26.

[0312] The inner lead 51 is thinned from the back side by, for example, half etching. The inner lead 51 has an inner lead front side 51a and an inner lead back side 51b. The inner lead front side 51a is located on the front side. An internal terminal is formed on a portion of the inner lead front side 51a. In addition, an inner lead end face 51c is formed on the surface of the inner lead 51 that faces the chip holder 11. The inner lead back side 51b is located on the back side.

[0313] The entire area of ​​the inner lead end surface 51c of the lead portion 12 is a rough surface. In addition, although not shown in the figure, the two side surfaces along the length direction of the lead portion 12 can also be rough surfaces. On the other hand, the inner lead 51 of the lead portion 12 is not thinned from the front side. The entire area of ​​the inner lead front surface 51a of the inner lead 51 located on the front side is a rough surface. In addition, the terminal portion 53 of the lead portion 12 is not thinned from the front side. The entire area of ​​the terminal portion front surface 53a located on the front side of the terminal portion 53 is a rough surface.

[0314] In addition, the structure of the lead frame 10 of this embodiment may be the same as the structure of the lead frame 10 of the second embodiment.

[0315] In the present embodiment, the definition and measurement method of “rough surface” and “smooth surface” are the same as those in the second embodiment.

[0316] (Structure of Semiconductor Device)

[0317] Next, use Figure 20 to Figure 22 A semiconductor device according to this embodiment will be described. Figure 20 to Figure 22 It is a diagram showing a semiconductor device (flip chip type) according to this embodiment.

[0318] like Fig. 20 and Fig.21 As shown, the semiconductor device (semiconductor package) 20 includes a die pad 11 , a semiconductor element 21 , a plurality of lead portions 12 , a plurality of bumps 26 , and a sealing resin 23 .

[0319] The semiconductor element 21 is mounted on the chip holder 11. In addition, a plurality of lead portions 12 are arranged around the chip holder 11. A plurality of bumps 26 electrically connect the semiconductor element 21 to the chip holder 11 or the lead portion 12, respectively. In this case, the bumps 26 constitute a connecting portion. In addition, the bumps 26 may also be columns. The sealing resin 23 performs resin sealing on the chip holder 11, the lead portion 12, the semiconductor element 21, and the bumps 26.

[0320] Bumps 26 are provided on the die pad 11 and the lead portion 12. Through the bumps 26, the semiconductor element 21, the die pad 11, and the lead portion 12 are electrically connected to each other.

[0321] The bump (connection portion) 26 is made of a metal material with good conductivity, such as copper, and may have a solid substantially cylindrical shape or a substantially spherical shape. The upper ends of the bumps 26 are respectively connected to the electrodes 21a of the semiconductor element 21, and the lower ends of the bumps 26 are respectively connected to the chip holder 11 and the lead portion 12. In addition, the bumps 26 may not necessarily be provided on the chip holder 11. In this case, the chip holder 11 and the semiconductor element 21 may also be fixed to each other by, for example, an adhesive such as a die bonding paste.

[0322] Fig. 22 2 is an enlarged cross-sectional view showing the periphery of the bump 26. Fig. 22As shown, the bump 26 may also include a plurality of layers. For example, the bump 26 includes a first layer 26a located on the chip pad 11 or lead portion 12 side, and a second layer 26b located on the semiconductor element 21 side. The first layer 26a may also include, for example, a metal such as tin. The height of the first layer 26a may be set to be greater than 1 μm and less than 10 μm. The second layer 26b may also include, for example, a metal such as copper. The height of the second layer 26b may be greater than 30 μm and less than 100 μm.

[0323] The semiconductor device 20 is not limited to the flip chip type. For example, the connection portion may be formed by a connection wire instead of the bump 26. In this case, the connection wire can electrically connect the semiconductor element 21 and the lead portion 12 to each other.

[0324] In addition, the structure of the semiconductor device 20 of this embodiment may be the same as the structure of the semiconductor device 20 of the second embodiment.

[0325] (Lead frame manufacturing method)

[0326] Next, use Fig.23 (a)-(i) Fig.18 and Fig.19 A method for manufacturing the lead frame 10 shown will be described. Fig.23 (a)-(i) are cross-sectional views showing a method of manufacturing the lead frame 10 (with Fig.19 corresponding figure).

[0327] First, compared with the second embodiment ( Fig.14 In the case of (a) to (e)), a metal substrate 31 having a chip pad 11 and a lead portion 12 located around the chip pad 11 is prepared in the same manner. Fig.23 (a)-(e)).

[0328] Next, a plating layer 36 ( Fig.23 (f)). At this time, the plating layer 36 is formed in the peripheral area of ​​the metal substrate 31 except for the entire front area. That is, the plating layer 36 is not formed on the entire front area of ​​the metal substrate 31, but is formed on the entire back area and the entire side area of ​​the metal substrate 31. More specifically, the plating layer 36 is not formed on the chip seat front 11a of the chip seat 11, the inner lead front 51a of the lead portion 12, and the terminal portion front 53a. On the other hand, the plating layer 36 is formed on the chip seat back 11b of the chip seat 11, the first chip seat side 11c, and the second chip seat side 11d. In addition, the plating layer 36 is formed on the external terminal 17 of the lead portion 12, the inner lead back 51b, and the inner lead end surface 51c. In addition, the plating layer 36 may not be formed on the front of the connecting bar 13. The plating layer 36 may also be formed on the back of the connecting bar 13.

[0329] At this time, if Fig.23 As shown in (f), the entire front area of ​​the metal substrate 31 is covered with the first clamp 45 via an elastic member 44 such as a rubber gasket. By electroplating the metal substrate 31 in this state, a plating layer 36 is formed in an area other than the entire front area of ​​the metal substrate 31. The thickness of the plating layer 36 may also be greater than 0 μm and less than 2 μm. As a metal constituting the plating layer 36, for example, silver may also be used. When the plating layer 36 is composed of a silver plating layer, a silver plating solution containing silver cyanide and potassium cyanide as main components may be used as a plating solution for electroplating. In this way, the plating layer 36 is not formed on the entire front area of ​​the metal substrate 31, thereby reducing the amount of metal such as silver constituting the plating layer 36. As a result, the manufacturing cost of the lead frame 10 can be reduced.

[0330] Next, a portion of the plating layer 36 existing in the region where the rough surface is formed is removed. Specifically, the plating layer 36 existing on at least the back side of the metal substrate 31 is left, and the other plating layers 36 are removed ( Fig.23 (g)). Specifically, the portion of the plating layer 36 that is present on the side surface of the metal substrate 31 is removed. As a result, the plating layer 36 on the first die pad side surface 11c and the second die pad side surface 11d of the die pad 11 is removed. In addition, the plating layer 36 on the inner lead end surface 51c and the inner lead back surface 51b of the lead portion 12 is removed.

[0331] During this period, if Fig.23 As shown in (g), first, an elastic member 46 such as a rubber gasket is arranged on the back side of the metal substrate 31, and a second clamp 47A is arranged on the back side of the metal substrate 31 through the elastic member 46. Next, the plating layer 36 of the portion not covered by the elastic member 46 is peeled off and removed. As a result, the first chip pad side surface 11c, the second chip pad side surface 11d, the inner lead end surface 51c, and the inner lead back surface 51b are exposed. On the other hand, the plating layer 36 on the chip pad back surface 11b and the external terminal 17 covered by the elastic member 46 remains.

[0332] Then, if Fig.23 As shown in (h), a support layer 37 for supporting the metal substrate 31 is provided on the back side of the metal substrate 31. The support layer 37 may be, for example, a resist layer. Fig.23As shown in (h), by roughening the portion of the metal substrate 31 not covered by the plating layer 36, a rough surface is formed in the portion not covered by the plating layer 36. Specifically, the front face 11a of the chip seat, the side face 11c of the first chip seat, the side face 11d of the second chip seat, the front face 51a of the inner lead, the front face 53a of the terminal portion, the end face 51c of the inner lead, and the back face 51b of the inner lead are rough surfaces. During this period, a micro-etching liquid is supplied to the metal substrate 31, thereby forming a rough surface on the entire metal substrate 31 except for the portion covered by the plating layer 36. Here, the micro-etching liquid refers to a surface treatment agent that slightly dissolves the metal surface to form a fine uneven rough surface. For example, when roughening a metal substrate 31 composed of copper or a copper alloy, a micro-etching liquid mainly composed of hydrogen peroxide and sulfuric acid can be used.

[0333] Then, if Fig.23 As shown in (i), the support layer 37 and the plating layer 36 are peeled off in sequence to obtain Fig.18 and Fig.19 The lead frame 10 is shown.

[0334] (Method for manufacturing semiconductor device)

[0335] like Fig.24 As shown in (a) to (d) of FIG. 1 , the manufacturing method of the semiconductor device 20 of this embodiment can be performed in substantially the same manner as the manufacturing method of the semiconductor device 20 of the second embodiment. In this case, each electrode 21a of the semiconductor element 21 is electrically connected to the die pad 11 and the lead portion 12 via the bump 26, respectively.

[0336] Thus, according to the present embodiment, the plating layer 36 ( Fig.24 Next, the plating layer 36 on the back side of the metal substrate 31 is left, and the other plating layers 36 are removed ( Fig.24 Then, a rough surface is formed on the portion of the metal substrate 31 that is not covered by the plating layer 36 ( Fig.24 (h)). In this way, the plating layer 36 for forming the rough surface is not provided on the entire surface of the metal substrate 31, but is provided in the area other than the front surface of the metal substrate 31. As a result, the amount of metal such as silver constituting the plating layer 36 can be reduced. As a result, the manufacturing cost of the lead frame 10 can be reduced.

[0337] However, it is conceivable that during the long-term use of the semiconductor device 20 manufactured in this way, moisture in the air and the like will intrude from the back side of the semiconductor device 20 through the interface between the sealing resin 23 and the chip seat 11 or the lead portion 12. In response to this, according to the present embodiment, the inner lead back side 51b and the inner lead end surface 51c of the lead portion 12 become rough surfaces. In addition, the first chip seat side surface 11c and the second chip seat side surface 11d of the chip seat 11 become rough surfaces, respectively. Therefore, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the chip seat 11 or the lead portion 12 becomes longer. As a result, it is possible to suppress the intrusion of moisture from the interface between the sealing resin 23 and the chip seat 11 or the lead portion 12 to the semiconductor element 21 side (see Fig.25 Arrow F A ). As a result, the reliability of the semiconductor device 20 after long-term use can be improved.

[0338] (Fourth embodiment)

[0339] Next, refer to Figure 26 to Figure 29 A fourth embodiment will be described. Figure 26 to Figure 29 It is a figure which shows the 4th embodiment. Figure 26 to Figure 29 The fourth embodiment shown in the figure is different mainly in that a metal layer 25 is provided on the front surface of the chip base 11 and the lead portion 12, and the other structures are substantially the same as those of the third embodiment described above. Figure 26 to Figure 29 In, with Figures 8 to 17 The second embodiment shown, and Figures 18 to 25 The same parts as those in the third embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted.

[0340] (Structure of lead frame and semiconductor device)

[0341] Fig.26 1 is a cross-sectional view showing a lead frame 10A according to the present embodiment. Fig. 27 2 is a cross-sectional view showing a semiconductor device 20A according to the present embodiment.

[0342] exist Fig.26 The lead frame 10A and Fig. 27 In the semiconductor device 20A shown, the metal layer 25 is located on a portion of the die pad 11 and a portion of the lead portion 12. Specifically, a plurality of metal layers 25 for improving the close contact with the bump 26 are provided on the die pad front surface 11a of the die pad 11. In addition, a metal layer 25 for improving the close contact with the bump 26 is provided on the internal terminal formed on the inner lead 51 of the lead portion 12.

[0343] The metal layer 25 is used to make the connection between the bump 26 and the chip seat 11 and the lead portion 12 good. The metal layer 25 can be, for example, a plated layer formed by an electroplating method. The thickness of the metal layer 25 can be greater than 1 μm and less than 10 μm. As the metal constituting such a plated layer, silver, silver alloy, gold, gold alloy, platinum group, copper, copper alloy, palladium, etc. can be used. Depending on the metal constituting the metal layer 25, when base plating is required, it is sufficient to apply a known material such as nickel or copper.

[0344] like Fig.26 and Fig. 27 As shown, the front surface of the lead portion 12 has a first front surface portion 56a as a smooth surface and a second front surface portion 56b as a rough surface. The first front surface portion 56a is located at the inner side (chip pad 11 side) end of the lead portion 12. A metal layer 25 is formed on the first front surface portion 56a. The entire first front surface portion 56a is a smooth surface. In addition, the first front surface portion 56a is located at a part of the inner lead front surface 51a.

[0345] The second front portion 56b is adjacent to the outer side of the first front portion 56a and the metal layer 25 (the opposite side of the chip seat 11). The second front portion 56b is directly connected to the first front portion 56a and the metal layer 25. The entire second front portion 56b is a rough surface. In addition, in the lead frame 10A, the second front portion 56b preferably extends continuously to the connection portion between the lead portion 12 and the connecting bar 13. The front surface of the connecting bar 13 can be a rough surface. In addition, the second front portion 56b is located at a part of the inner lead front surface 51a and a part of the terminal portion front surface 53a.

[0346] like Fig. 27 As shown, in the semiconductor device 20A, the bumps 26 are provided on the metal layer 25. The upper ends of the bumps 26 are respectively connected to the electrodes 21a of the semiconductor element 21, and the lower ends of the bumps 26 are respectively connected to the die pad 11 and the lead portion 12 via the metal layer 25. In addition, the metal layer 25 and the bumps 26 do not need to be provided on the die pad 11.

[0347] In the present embodiment, the definition and measurement method of “rough surface” and “smooth surface” are the same as those in the second embodiment.

[0348] (Lead frame manufacturing method)

[0349] Next, use Fig.28 (a)-(j) pairs Fig.26 A method for manufacturing the lead frame 10A shown in FIG. Fig.28 In (a)-(j), Fig.23 The same parts of the structures shown in (a)-(i) are marked with the same reference numerals and detailed descriptions are omitted.

[0350] First, compared with the second embodiment ( Fig.14 In the same manner as in the cases (a) to (e)), a metal substrate 31 having a chip pad 11 and lead portions 12 located around the chip pad 11 is prepared. Fig.28 (a)-(e)).

[0351] Next, a plating layer 36 ( Fig.28 (f)). At this time, the plating layer 36 is formed on a part of the front surface, the entire back surface area, and the entire side surface area of ​​the metal substrate 31. In addition, the plating layer 36 is formed on a part of the front surface of the chip holder 11 and a part of the front surface of the lead portion 12. More specifically, the plating layer 36 is formed in the area where the metal layer 25 is formed in the chip holder front surface 11a of the chip holder 11, and is not formed in areas other than the area where the metal layer 25 is formed. In addition, the plating layer 36 is formed on the chip holder back surface 11b, the first chip holder side surface 11c, and the second chip holder side surface 11d of the chip holder 11. In addition, the plating layer 36 is formed on the first front surface portion 56a of the lead portion 12, the external terminal 17, the inner lead back surface 51b, and the inner lead terminal surface 51c. On the other hand, the plating layer 36 is not formed on the second front surface portion 56b of the lead portion 12. It should be noted that the plating layer 36 may not be formed on the front surface of the connecting bar 13, but may be formed on the back surface of the connecting bar 13.

[0352] At this time, if Fig.28 As shown in (f), a portion of the front surface of the metal substrate 31 is covered with the first clamp 45A via an elastic member 44A such as a rubber gasket. By electroplating the metal substrate 31 in this state, a plating layer 36 is formed in a region other than a portion of the front surface of the metal substrate 31. In this way, by not forming the plating layer 36 on a portion of the front surface of the metal substrate 31, the amount of metal such as silver constituting the plating layer 36 can be reduced. As a result, the manufacturing cost of the lead frame 10A can be reduced. In addition, the material and thickness of the plating layer 36 can be the same as those in the third embodiment.

[0353] Next, a portion of the plating layer 36 existing in the region where the rough surface is formed is removed ( Fig.28 At this time, the plating layer 36 existing on a part of the front surface and the back surface of the metal substrate 31 is removed, and the other plating layers 36 are removed. Specifically, the portions of the plating layer 36 corresponding to the first die pad side surface 11c, the second die pad side surface 11d, the inner lead end surface 51c, and the inner lead back surface 51b of the metal substrate 31 are removed.

[0354] During this period, if Fig.28As shown in (g), first, elastic components 46 are arranged on the front and back sides of the metal substrate 31, respectively, and the metal substrate 31 is clamped by the second clamp 47B via the elastic components 46 such as rubber pads. In addition, the elastic components 46 on the front side of the metal substrate 31 cover the entire front side of the metal substrate 31. Next, the plating layer 36 of the portion not covered by the elastic components 46 is peeled off and removed. As a result, the first chip holder side surface 11c, the second chip holder side surface 11d, the inner lead end surface 51c, and the inner lead back surface 51b are exposed. On the other hand, the plating layer 36 on the chip holder front surface 11a, the chip holder back surface 11b, the first front portion 56a, and the external terminal 17 covered by the elastic components 46 remains.

[0355] Then, with the above Fig.23 The support layer 37 is provided on the back side of the metal substrate 31 in substantially the same manner as the step (h) shown in FIG. Next, the portion of the metal substrate 31 not covered by the plating layer 36 is roughened, thereby forming a rough surface ( Fig.28 (h)). As a result, the first die pad side surface 11c, the second die pad side surface 11d, the second front surface portion 56b, the inner lead terminal surface 51c, and the inner lead back surface 51b become rough surfaces.

[0356] Then, with Fig.23 The step (i) shown in FIG. 1 is similar to the step in which the support layer 37 and the plating layer 36 are sequentially peeled off and removed. Fig.28 (i)).

[0357] Then, if Fig.28 As shown in (j), a metal layer 25 is formed on a portion of the front surface of the metal substrate 31. Specifically, the metal layer 25 is formed on a portion of the chip holder 11 and a portion of the lead portion 12. In this case, first, a plating resist layer of a predetermined pattern not shown is formed on the chip holder 11 and the lead portion 12, for example, by photolithography. Next, a metal layer 25 consisting of a plated layer is formed on the portion not covered by the plating resist layer, for example, by electroplating. Then, the plating resist layer is removed, thereby obtaining Fig.26 Lead frame 10A is shown.

[0358] (Method for manufacturing semiconductor device)

[0359] The method for manufacturing the semiconductor device 20A of the present embodiment can be used in conjunction with Fig.24 The method for manufacturing the semiconductor device 20 shown in (a) to (d) of FIG. 2 is performed in substantially the same manner. In this case, each electrode 21 a of the semiconductor element 21 is electrically connected to the die pad 11 and the lead portion 12 via the bump 26 and the metal layer 25 .

[0360] Thus, according to the present embodiment, the plating layer 36 ( Fig.28 Next, the plating layer 36 existing on a part of the front surface and the back surface of the metal substrate 31 is left, and the other plating layers 36 are removed ( Fig.28 Then, a rough surface is formed on the portion of the metal substrate 31 that is not covered by the plating layer 36 ( Fig.28 (h)). In this way, the plating layer 36 for forming the rough surface is not provided on the entire surface of the metal substrate 31, but is provided in the area other than a part of the front surface of the metal substrate 31. As a result, the amount of metal such as silver constituting the plating layer 36 can be reduced. As a result, the manufacturing cost of the lead frame 10 can be reduced.

[0361] In addition, according to the present embodiment, the second front surface portion 56b adjacent to the outer side of the metal layer 25 is formed into a rough surface. Therefore, the distance of the moisture intrusion path at the interface between the surface of the lead portion 12 and the sealing resin 23 becomes longer. As a result, it is possible to suppress the moisture from intruding from the interface between the surface of the lead portion 12 and the sealing resin 23 to the semiconductor element 21 side (see Fig.29 Arrow F B ). As a result, the reliability of the semiconductor device 20A after long-term use can be improved.

[0362] According to the present embodiment, the second front surface portion 56b of the lead portion 12 is roughened, thereby improving the adhesion strength between the second front surface portion 56b and the sealing resin 23 and preventing the surface of the lead portion 12 and the sealing resin 23 from peeling off from each other.

[0363] In addition, according to the present embodiment, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 is lengthened on the back side of the semiconductor device 20A. This can suppress the moisture from intruding from the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 to the semiconductor element 21 side (see Fig.29 Arrow F A ). As a result, the reliability of the semiconductor device 20A after long-term use can be improved.

[0364] (Fifth embodiment)

[0365] Reference Figures 30 to 37 A fifth embodiment will be described. Figures 30 to 37 is a diagram showing a fifth embodiment. Figures 30 to 37 In, with Figures 8 to 29 The same parts in the illustrated embodiments are denoted by the same reference numerals and detailed description thereof will be omitted.

[0366] (Lead frame structure)

[0367] First, use Fig.30 and Fig.31 The outline of the lead frame according to the present embodiment will be described. Fig.30 and Fig.31 It is a diagram showing a lead frame according to this embodiment.

[0368] In this specification, the “outer periphery” refers to a portion of the lead frame 10 (metal substrate) exposed to the outside, and is a region including the “front side”, “side side”, and “back side”.

[0369] like Fig.30 and Fig.31 As shown, each packaging area 10a of the lead frame 10 includes a chip pad 11 and a lead portion 12 located around the chip pad 11. Among them, a part of the lead portion 12 is thinned from the back side. The thinned portion on the back side of the lead portion 12 becomes a rough surface. The non-thinned portion on the back side of the lead portion 12 becomes a smooth surface.

[0370] like Fig.31 As shown, the chip pad 11 has a chip pad front side 11a located on the front side and a chip pad back side 11b located on the back side. On the chip pad front side 11a, a semiconductor element 21 is mounted as described later. The chip pad back side 11b is exposed to the outside from the semiconductor device 20 (described later). In addition, a first chip pad side surface 11c and a second chip pad side surface 11d are formed on the side of the chip pad 11 facing the lead portion 12. The first chip pad side surface 11c is located on the chip pad front side 11a. The second chip pad side surface 11d is located on the chip pad back side 11b. In this case, the first chip pad side surface 11c and the second chip pad side surface 11d in the chip pad 11 are respectively rough surfaces. On the other hand, the chip pad front side 11a and the chip pad back side 11b in the chip pad 11 are respectively smooth surfaces.

[0371] In the present embodiment, the definition and measurement method of “rough surface” and “smooth surface” are the same as those in the second embodiment.

[0372] The rough surface may be formed by roughening the outer surface of the metal substrate 31 described later using a micro-etching solution mainly composed of hydrogen peroxide and sulfuric acid. The smooth surface may also be an unprocessed surface of the metal substrate 31 described later without such roughening. Fig.31 In FIG. 1 , the roughened portion is indicated by a thick dotted line (the same applies to other cross-sectional views).

[0373] like Fig.31As shown, the lead portion 12 has an inner lead 51 and a terminal portion 53. The inner lead 51 is located on the inner side (chip holder 11 side). The terminal portion 53 is located on the outer side (connection bar 13 side). The inner lead 51 extends from the terminal portion 53 to the chip holder 11 side. An internal terminal is formed at the end portion of the front side of the inner lead 51. As described later, the internal terminal is an area electrically connected to the semiconductor element 21 via the bump 26. A metal layer 25 for improving the close contact with the bump 26 is provided on the internal terminal.

[0374] The inner lead 51 is thinned from the back side by, for example, half etching. The inner lead 51 has an inner lead front side 51a and an inner lead back side 51b. The inner lead front side 51a is located on the front side. An internal terminal is formed on a portion of the inner lead front side 51a. In addition, an inner lead end face 51c is formed on the surface of the inner lead 51 that faces the chip holder 11. The inner lead back side 51b is located on the back side.

[0375] Furthermore, the entire area of ​​the inner lead end surface 51c of the lead portion 12 becomes a rough surface. In addition, although not shown in the figure, the two side surfaces along the long side direction of the lead portion 12 can also be rough surfaces. On the other hand, the inner lead 51 of the lead portion 12 is not thinned from the front side. The entire area of ​​the inner lead front surface 51a of the inner lead 51 located on the front side is a smooth surface. In addition, the terminal portion 53 of the lead portion 12 is not thinned from the front side. The entire area of ​​the terminal portion front surface 53a of the terminal portion 53 located on the front side is a smooth surface.

[0376] In addition, if Fig.31 As shown, the metal layer 25 is located on the chip seat 11 and the lead portion 12. The metal layer 25 is formed on a portion of the chip seat 11 and a portion of the lead portion 12. The metal layer 25 is used to ensure good connection between the bump 26 and the chip seat 11 and the lead portion 12. The metal layer 25 can be, for example, a plated layer formed by electroplating. The thickness of the metal layer 25 can be greater than 1 μm and less than 10 μm. As a metal constituting such a plated layer, silver, silver alloy, gold, gold alloy, platinum group, copper, copper alloy, palladium, etc. can be used. As a metal constituting the metal layer 25, when base plating is required, it is sufficient to use a known material such as nickel and copper.

[0377] In addition, the structure of the lead frame 10 of this embodiment may be the same as the structure of the lead frame 10 of the second embodiment.

[0378] (Structure of Semiconductor Device)

[0379] Next, use Figure 32 to Figure 34 A semiconductor device according to this embodiment will be described. Figure 32 to Figure 34 It is a diagram showing a semiconductor device (flip chip type) according to this embodiment.

[0380] like Fig.32 and Fig.33 As shown, the semiconductor device (semiconductor package) 20 includes a die pad 11 , a semiconductor element 21 , a plurality of lead portions 12 , a plurality of bumps 26 , and a sealing resin 23 .

[0381] The semiconductor element 21 is mounted on the die pad 11. In addition, a plurality of lead portions 12 are arranged around the die pad 11. In addition, metal layers 25 are formed on the die pad 11 and the lead portions 12, respectively. Bumps 26 are provided on the metal layer 25. The semiconductor element 21, the die pad 11, and the lead portions 12 are electrically connected to each other via the bumps 26.

[0382] One side of the sealing resin 23 (one side of the semiconductor device 20 ) may be, for example, not less than 0.2 mm and not more than 16 mm.

[0383] The bump (connecting portion) 26 is made of a metal material with good conductivity, such as copper, and may have a solid substantially cylindrical shape or a substantially spherical shape. The upper ends of the bumps 26 are respectively connected to the electrodes 21a of the semiconductor element 21, and the lower ends of the bumps 26 are respectively connected to the chip holder 11 and the lead portion 12 via the metal layer 25. In addition, the metal layer 25 and the bumps 26 may not be provided on the chip holder 11. In this case, the chip holder 11 and the semiconductor element 21 may be fixed to each other by, for example, an adhesive such as a die bonding paste.

[0384] Fig.34 2 is an enlarged cross-sectional view showing the periphery of the bump 26. Fig.34 As shown, the bump 26 may also include a plurality of layers. For example, the bump 26 includes a first layer 26a located on the metal layer 25 side and a second layer 26b located on the semiconductor element 21 side. The first layer 26a may also include a metal such as tin, for example. The height of the first layer 26a may be set to be greater than 1 μm and less than 10 μm. The second layer 26b may also include a metal such as copper, for example. The height of the second layer 26b may be greater than 30 μm and less than 100 μm.

[0385] The structure of the die pad 11 and the lead portion 12 is similar to the above-mentioned structure except for the region not included in the semiconductor device 20. Fig.30 as well as Fig.31 The structures shown are the same, so detailed description is omitted here.

[0386] The semiconductor device 20 is not limited to the flip chip type. For example, the connection portion may be formed by a connection wire instead of the bump 26. In this case, the connection wire may electrically connect the semiconductor element 21 and the lead portion 12 to each other.

[0387] In addition, the structure of the semiconductor device 20 of this embodiment may be the same as the structure of the semiconductor device 20 of the second embodiment.

[0388] (Lead frame manufacturing method)

[0389] Next, use Fig.35 (a)-(j) pairs Fig.30 and Fig.31 A method for manufacturing the lead frame 10 shown will be described. Fig.35 (a) to (j) are cross-sectional views showing a method of manufacturing the lead frame 10 (with Fig.31 corresponding figure).

[0390] First, compared with the second embodiment ( Fig.14 In the case of (a) to (e)), a metal substrate 31 having a chip pad 11 and a lead portion 12 located around the chip pad 11 is prepared in the same manner. Fig.35 (a)-(e)).

[0391] Next, a plating layer 36 ( Fig.35 (f)). At this time, the plating layer 36 is formed on the entire periphery of the chip seat 11, the lead portion 12 and the connecting bar 13. The thickness of the plating layer 36 may be greater than 0 μm and less than 2 μm. As a metal constituting the plating layer 36, for example, silver may also be used. When the plating layer 36 is composed of a silver plating layer, a silver plating solution containing silver cyanide and potassium cyanide as main components may be used as a plating solution for electroplating.

[0392] Next, a portion of the plating layer 36 present in the region where the rough surface is formed is removed. Specifically, the portion of the plating layer 36 other than the front and back surfaces of the metal substrate 31 is removed ( Fig.35 (g)). As a result, the plating layer 36 on the first chip pad side surface 11c of the chip pad 11, the second chip pad side surface 11d of the chip pad 11, the inner lead end surface 51c of the lead portion 12, and the inner lead back surface 51b of the lead portion 12 is removed.

[0393] During this period, if Fig.35 As shown in (g), first, elastic components 46 such as rubber pads are respectively arranged on the front and back sides of the metal substrate 31, and the metal substrate 31 is clamped by a clamp 47C via the elastic components 46. Next, the plating layer 36 of the portion not covered by the elastic components 46 is peeled off and removed. As a result, the first chip holder side surface 11c, the second chip holder side surface 11d, the inner lead end surface 51c, and the inner lead back surface 51b are exposed. On the other hand, the plating layer 36 on the chip holder front surface 11a, the terminal portion front surface 53a, the chip holder back surface 11b, the inner lead front surface 51a, and the external terminal 17 covered by the elastic components 46 remains.

[0394] Then, if Fig.35As shown in (h), a support layer 37 for supporting the metal substrate 31 is provided on the back side of the metal substrate 31. The support layer 37 may be, for example, a resist layer. Fig.35 As shown in (h), by roughening the portion of the metal substrate 31 not covered by the plating layer 36, a rough surface is formed in the portion not covered by the plating layer 36. Specifically, the first chip seat side 11c, the second chip seat side 11d, the inner lead end surface 51c and the inner lead back surface 51b are rough surfaces. During this period, a micro-etching liquid is supplied to the metal substrate 31, thereby forming a rough surface on the entire metal substrate 31 except for the portion covered by the plating layer 36. Here, the micro-etching liquid refers to a surface treatment agent that slightly dissolves the metal surface to form a fine uneven rough surface. For example, in the case of roughening the metal substrate 31 composed of copper or a copper alloy, a micro-etching liquid mainly composed of hydrogen peroxide and sulfuric acid can also be used.

[0395] Then, if Fig.35 As shown in (i), the support layer 37 and the plating layer 36 are sequentially peeled off and removed.

[0396] Afterwards, if Fig.35 As shown in (j), a metal layer 25 is formed on the chip base 11 and the lead portion 12. In this case, first, a plating resist layer of a predetermined pattern (not shown) is formed on the chip base 11 and the lead portion 12, for example, by photolithography. Next, a metal layer 25 composed of a plated layer is formed on the portion not covered by the plating resist layer, for example, by electroplating. Then, the plating resist layer is removed, thereby obtaining Fig.30 and Fig.31 The lead frame 10 is shown.

[0397] (Method for manufacturing semiconductor device)

[0398] like Fig.36 As shown in (a) to (d) of the present embodiment, the manufacturing method of the semiconductor device 20 of the present embodiment can be performed in substantially the same manner as the manufacturing method of the semiconductor device 20 of the second embodiment. In this case, each electrode 21a of the semiconductor element 21 is electrically connected to the chip pad 11 and the lead portion 12 via the bump 26 and the metal layer 25, respectively.

[0399] However, it is conceivable that during the long-term use of the semiconductor device 20 manufactured in this way, moisture in the air and the like will intrude from the back side of the semiconductor device 20 through the interface between the sealing resin 23 and the chip seat 11 or the lead portion 12. In response to this, according to the present embodiment, the inner lead back side 51b and the inner lead end surface 51c of the lead portion 12 become rough surfaces. In addition, the first chip seat side surface 11c and the second chip seat side surface 11d of the chip seat 11 become rough surfaces, respectively. Therefore, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the chip seat 11 or the lead portion 12 becomes longer. As a result, it is possible to suppress the intrusion of moisture from the interface between the sealing resin 23 and the chip seat 11 or the lead portion 12 to the semiconductor element 21 side (see Fig.37 Arrow F A ). As a result, the reliability of the semiconductor device 20 after long-term use can be improved.

[0400] In particular, in a flip-chip semiconductor device 20, the electrode 21a of the semiconductor element 21 faces the back side. Therefore, in a flip-chip semiconductor device 20, the distance from the back side of the semiconductor device 20 to the electrode 21a of the semiconductor element 21 tends to be short. In response to this, according to the present embodiment, the thinned portion of the back side of the lead portion 12 is roughened. As a result, it is possible to more effectively suppress the intrusion of moisture from the interface between the sealing resin 23 and the lead portion 12 to the semiconductor element 21 side.

[0401] In addition, according to the present embodiment, the inner lead back surface 51b and the inner lead end surface 51c of the lead portion 12 are roughened. In addition, the first die pad side surface 11c and the second die pad side surface 11d of the die pad 11 are roughened. Thus, the close adhesion strength between the die pad 11 and the lead portion 12 and the sealing resin 23 can be improved, and the die pad 11 and the lead portion 12 and the sealing resin 23 can be prevented from peeling off from each other.

[0402] (Sixth embodiment)

[0403] Next, refer to Figures 38 to 41 A sixth embodiment will be described. Figures 38 to 41 It is a figure which shows the 6th embodiment. Figures 38 to 41 The main difference of the sixth embodiment shown is that a rough surface is formed on the front surface of the lead portion 12, and the other structures are substantially the same as those of the fifth embodiment described above. Figures 38 to 41 In, with Figures 8 to 37 The same parts in the illustrated embodiments are denoted by the same reference numerals and detailed description thereof will be omitted.

[0404] (Structure of lead frame and semiconductor device)

[0405] Fig.38 1 is a cross-sectional view showing a lead frame 10A according to the present embodiment. Fig.39 2 is a cross-sectional view showing a semiconductor device 20A according to the present embodiment.

[0406] exist Fig.38 The lead frame 10A and Fig.39 In the semiconductor device 20A shown, the front surface of the lead portion 12 has a first front surface portion 54 a which is a smooth surface and a second front surface portion 54 b which is a rough surface.

[0407] The first front portion 54a is adjacent to the outer side of the metal layer 25 (the side opposite to the die pad 11). The first front portion 54a is directly in contact with the metal layer 25. The entire first front portion 54a is a smooth surface. The length L of the first front portion 54a along the long side direction of the lead portion 12 (the length in the X direction) is A The thickness may be 25 μm or more and 200 μm or less, preferably 50 μm or more and 100 μm or less. In addition, the first front portion 54a is located at a portion of the inner lead front 51a, but is not limited thereto. The first front portion 54a may also be located at a portion of the inner lead front 51a and a portion of the terminal portion front 53a, for example.

[0408] The second front portion 54b is adjacent to the outer side of the first front portion 54a. That is, the second front portion 54b is directly connected to the first front portion 54a. The entire second front portion 54b is a rough surface. In addition, in the lead frame 10A, the second front portion 54b preferably extends continuously to the connection portion between the lead portion 12 and the connecting bar 13. The front surface of the connecting bar 13 can be a rough surface. In addition, the second front portion 54b is located at a part of the inner lead front surface 51a and a part of the terminal portion front surface 53a, but is not limited to this. The second front portion 54b can also be located at a part of the terminal portion front surface 53a.

[0409] In this embodiment, the definition and measurement method of "rough surface" and "smooth surface" are the same as those in the second embodiment.

[0410] (Lead frame manufacturing method)

[0411] Next, use Fig.40 (a)-(j) pairs Fig.38 A method for manufacturing the lead frame 10A shown in FIG. Fig.40 In (a)-(j), Fig.35 The same components as shown in (a) to (j) are denoted by the same reference numerals and detailed descriptions thereof are omitted.

[0412] First, compared with the second embodiment ( Fig.14 In the case of (a) to (e)), a metal substrate 31 having a chip pad 11 and a lead portion 12 located around the chip pad 11 is prepared in the same manner. Fig.40 (a)-(e)).

[0413] Then, with the above Fig.35 The plating layer 36 ( Fig.40 (f)).

[0414] Next, the portions of the plating layer 36 corresponding to the first die pad side surface 11c, the second die pad side surface 11d, the second front surface portion 54b, the inner lead end surface 51c, and the inner lead back surface 51b of the metal substrate 31 are removed ( Fig.40 (g)).

[0415] During this period, if Fig.40 As shown in (g), first, elastic members 46 such as rubber pads are arranged on the front and back sides of the metal substrate 31, and the metal substrate 31 is clamped by the clamp 47D via the elastic members 46. In addition, the elastic member 46 on the front side of the metal substrate 31 covers the chip holder front side 11a, the area corresponding to the first front portion 54a, and the area where the metal layer 25 is provided in the lead portion 12. Next, the plating layer 36 of the portion not covered by the elastic member 46 is peeled off and removed. As a result, the first chip holder side surface 11c, the second chip holder side surface 11d, the second front portion 54b, the inner lead end surface 51c, and the inner lead back surface 51b are exposed. On the other hand, the plating layer 36 on the chip holder front side 11a, the chip holder back surface 11b, the first front portion 54a, and the external terminal 17 covered by the elastic member 46 remains.

[0416] Then, with the above Fig.35 The support layer 37 is provided on the back side of the metal substrate 31 in substantially the same manner as the step (h) shown in FIG. Next, the portion of the metal substrate 31 not covered by the plating layer 36 is roughened, thereby forming a rough surface ( Fig.40 (h)). As a result, the first die pad side surface 11c, the second die pad side surface 11d, the second front surface portion 54b, the inner lead terminal surface 51c, and the inner lead back surface 51b become rough surfaces.

[0417] Then, with Fig.35 The step (i) shown in FIG. 1 is similar to the step in which the support layer 37 and the plating layer 36 are sequentially peeled off and removed. Fig.40 (i)).

[0418] Then, with the above Fig.35 The metal layer 25 is formed on the chip pad 11 and the lead portion 12 in a substantially similar manner to the step (j) shown in FIG. Fig.38 The lead frame 10A shown in FIG. Fig.40 (j)).

[0419] (Method for manufacturing semiconductor device)

[0420] The method for manufacturing the semiconductor device 20A of the present embodiment can be used in conjunction with Fig.36 The method for manufacturing the semiconductor device 20 shown in (a) to (d) is performed in substantially the same manner.

[0421] According to the present embodiment, the first front surface portion 54a adjacent to the outer side of the metal layer 25 in the front surface of the lead portion 12 is formed into a smooth surface. Thus, when the semiconductor element 21 is mounted on the die pad 11, it is possible to suppress the tin contained in the bump 26 from flowing out along the first front surface portion 54a (see Fig.41 Arrow F C On the other hand, if the first front surface portion 54a is a rough surface, tin and the like contained in the bump 26 may flow out along the first front surface portion 54a due to surface tension.

[0422] In addition, according to the present embodiment, the second front portion 54b adjacent to the outer side of the first front portion 54a is a rough surface. Therefore, the distance of the moisture intrusion path at the interface between the surface of the lead portion 12 and the sealing resin 23 becomes longer. As a result, it is possible to suppress the moisture from intruding from the interface between the surface of the lead portion 12 and the sealing resin 23 to the semiconductor element 21 side (see Fig.41 Arrow F B ). As a result, the reliability of the semiconductor device 20A after long-term use can be improved.

[0423] According to the present embodiment, the second front surface portion 54b of the lead portion 12 is roughened, thereby improving the adhesion strength between the second front surface portion 54b and the sealing resin 23, and preventing the surface of the lead portion 12 and the sealing resin 23 from peeling off from each other.

[0424] In addition, according to the present embodiment, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 is lengthened on the back side of the semiconductor device 20A. This can suppress the moisture from intruding from the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 to the semiconductor element 21 side (see Fig.41 Arrow F A ). As a result, the reliability of the semiconductor device 20A after long-term use can be improved.

[0425] (Seventh Implementation Method)

[0426] Next, refer to Figure 42 to Figure 45 A seventh embodiment will be described. Figure 42 to Figure 45 It is a figure which shows the 7th embodiment. Figure 42 to Figure 45The main difference of the seventh embodiment shown is that a recess 18 is formed on the front surface of the lead portion 12, and the other structures are substantially the same as those of the fifth embodiment described above. Figure 42 to Figure 45 In, with Figures 8 to 41 The same parts in the illustrated embodiments are denoted by the same reference numerals and detailed description thereof will be omitted.

[0427] (Structure of lead frame and semiconductor device)

[0428] Fig.42 1 is a cross-sectional view showing a lead frame 10B according to the present embodiment. Fig.43 2 is a cross-sectional view showing a semiconductor device 20B according to the present embodiment.

[0429] exist Fig.42 The lead frame 10B shown in FIG. Fig.43 In the semiconductor device 20B shown, a recess 18 is formed on the front surface of the lead portion 12, on the outer side of the metal layer 25 (on the opposite side of the chip pad 11). In addition, the portion adjacent to the outer side of the recess 18 (the third front surface portion 54c) is a rough surface. The inner surface of the recess 18 is a smooth surface. The portion located between the recess 18 and the metal layer 25 (the fourth front surface portion 54d) is a smooth surface.

[0430] The fourth front portion 54d is adjacent to the outer side of the metal layer 25 (the side opposite to the die pad 11). The fourth front portion 54d is directly in contact with the metal layer 25. The entire fourth front portion 54d is a smooth surface. The length L of the fourth front portion 54d along the long side direction of the lead portion 12 (the length in the X direction) is B The thickness may be 25 μm or more and 200 μm or less, and preferably 50 μm or more and 100 μm or less.

[0431] The recess 18 is adjacent to the outer side of the fourth front portion 54d (the opposite side of the chip pad 11). The recess 18 is directly connected to the fourth front portion 54d. The entire inner surface of the recess 18 is a smooth surface. The length L of the recess 18 along the long side direction of the lead portion 12 (the length in the X direction) is c It can be 50 μm or more and 150 μm or less, preferably 75 μm or more and 100 μm or less. The depth of the recess 18 can be 25 μm or more and 125 μm or less, preferably 50 μm or more and 100 μm or less. The planar shape of the recess 18 can be, for example, a polygon such as a circle or a quadrilateral. The recess 18 is provided in a portion of the width direction of the lead portion 12. However, it is not limited thereto, and the recess 18 can also be provided over the entire width direction of the lead portion 12.

[0432] The third front portion 54c is adjacent to the outer side of the recess 18 (the opposite side of the chip pad 11). The third front portion 54c is directly connected to the recess 18. The entire third front portion 54c is a rough surface. In the lead frame 10B, the third front portion 54c preferably extends continuously to the connection portion between the lead portion 12 and the connecting bar 13. The front surface of the connecting bar 13 may be a rough surface.

[0433] In the present embodiment, the definition and measurement method of “rough surface” and “smooth surface” are the same as those in the second embodiment.

[0434] (Lead frame manufacturing method)

[0435] Next, use Fig.44 (a)-(j) pairs Fig.42 A method for manufacturing the lead frame 10B shown in FIG. Fig.44 In (a)-(j), Fig.35 The same components as shown in (a) to (j) are denoted by the same reference numerals and detailed descriptions thereof are omitted.

[0436] First, with the above Fig.35 The steps (a) and (b) are substantially the same as those shown in the following examples. Fig.44 (a)), photosensitive resists 32a and 33a are formed on the front and back surfaces of the metal substrate 31, respectively. Fig.44 (b)).

[0437] Next, with the above Fig.35 The etching resist layers 32 and 33 having openings 32b and 33b are formed in substantially the same manner as in the step (c) of FIG. Fig.44 (c)). In addition, at this time, the opening 32b is also formed in the area corresponding to the recess 18.

[0438] Then, with the above Fig.35 The process (d) shown in FIG. 1 is substantially the same as that of FIG. 1 , and the outer shapes of the chip pad 11, the lead portion 12, and the connection bar 13 are formed by etching the metal substrate 31. Fig.44 (d)). In addition, at this time, a recess 18 is formed on the front surface of the lead portion 12. Next, Fig.35 The etching resist layers 32 and 33 are removed by stripping in substantially the same manner as in the step (e) of FIG. Fig.44 (e)).

[0439] Then, with the above Fig.35 The plating layer 36 ( Fig.44 (f)). In addition, at this time, the plating layer 36 is also formed in the recessed portion 18.

[0440] Next, the portions of the plating layer 36 corresponding to the first die pad side surface 11c, the second die pad side surface 11d, the third front surface portion 54c, the inner lead end surface 51c, and the inner lead back surface 51b of the metal substrate 31 are removed ( Fig.44 (g)).

[0441] During this period, if Fig.44 As shown in (g), first, elastic members 46 such as rubber pads are arranged on the front and back sides of the metal substrate 31, and the metal substrate 31 is clamped by the clamp 47E via the elastic members 46. In addition, the elastic member 46 on the front side of the metal substrate 31 covers the chip holder front side 11a, the recess 18, the area corresponding to the fourth front portion 54d, and the area where the metal layer 25 is provided in the lead portion 12. Next, the plating layer 36 of the portion not covered by the elastic member 46 is peeled off and removed. As a result, the first chip holder side surface 11c, the second chip holder side surface 11d, the third front portion 54c, the inner lead terminal surface 51c, and the inner lead back surface 51b are exposed. On the other hand, the plating layer 36 on the chip holder front side 11a, the chip holder back surface 11b, the inner surface of the recess 18, the fourth front portion 54d, and the external terminal 17 covered by the elastic member 46 remains.

[0442] Then, with the above Fig.35 The support layer 37 is provided on the back side of the metal substrate 31 in substantially the same manner as the step (h) shown in FIG. Next, the portion of the metal substrate 31 not covered by the plating layer 36 is roughened, thereby forming a rough surface ( Fig.44 (h)). As a result, the first die pad side surface 11c, the second die pad side surface 11d, the third front surface portion 54c, the inner lead terminal surface 51c, and the inner lead back surface 51b become rough surfaces.

[0443] Then, with Fig.35 The step (i) shown in FIG. 1 is similar to the step in which the support layer 37 and the plating layer 36 are sequentially peeled off and removed. Fig.44 (i)).

[0444] Then, with the above Fig.35 The metal layer 25 is formed on the chip pad 11 and the lead portion 12 in a substantially similar manner to the step (j) shown in FIG. Fig.42 The lead frame 10B shown ( Fig.44 (j)).

[0445] (Method for manufacturing semiconductor device)

[0446] The method for manufacturing the semiconductor device 20B of this embodiment can be used in conjunction with Fig.36 The method for manufacturing the semiconductor device 20 shown in (a) to (d) is performed in substantially the same manner.

[0447] According to the present embodiment, the fourth front surface portion 54d adjacent to the outer side of the metal layer 25 in the front surface of the lead portion 12 is formed into a smooth surface. Thus, when the semiconductor element 21 is mounted on the die pad 11, it is possible to suppress the tin contained in the bump 26 from flowing out along the fourth front surface portion 54d (see Fig.45 Arrow F C On the other hand, if the fourth front surface portion 54d is a rough surface, tin and the like contained in the bump 26 may flow out along the fourth front surface portion 54d due to surface tension.

[0448] In addition, according to the present embodiment, the recessed portion 18 is formed outside the metal layer 25 in the front surface of the lead portion 12. Thus, even if the tin or the like contained in the bump 26 flows out along the fourth front surface portion 54d, the flowing tin or the like can be received by the recessed portion 18. Thus, the flowing tin or the like can be prevented from reaching the third front surface portion 54c.

[0449] In addition, according to the present embodiment, the third front surface portion 54c adjacent to the outside of the recess 18 is a rough surface. Therefore, the distance of the moisture intrusion path at the interface between the surface of the lead portion 12 and the sealing resin 23 becomes longer. As a result, it is possible to suppress the moisture from intruding from the interface between the surface of the lead portion 12 and the sealing resin 23 to the semiconductor element 21 side (see Fig.45 Arrow F B ). As a result, the reliability of the semiconductor device 20B after long-term use can be improved.

[0450] According to the present embodiment, the third front surface portion 54c of the lead portion 12 is roughened, thereby improving the adhesion strength between the third front surface portion 54c and the sealing resin 23, and preventing the surface of the lead portion 12 and the sealing resin 23 from peeling off from each other.

[0451] In addition, according to the present embodiment, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 is lengthened on the back side of the semiconductor device 20B. This can suppress the moisture from intruding from the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 to the semiconductor element 21 side (see Fig.45 Arrow F A ). As a result, the reliability of the semiconductor device 20B after long-term use can be improved.

[0452] (Eighth Implementation Method)

[0453] Next, refer to Figure 46 to Figure 49 An eighth embodiment will be described. Figure 46 to Figure 49 It is a diagram showing the eighth embodiment. Figure 46 to Figure 49The main difference of the eighth embodiment shown is that the inner surface of the recess 18 is a rough surface, and the other structures are substantially the same as those of the seventh embodiment described above. Figure 46 to Figure 49 In, with Figures 8 to 45 The same parts in the illustrated embodiments are denoted by the same reference numerals and detailed description thereof will be omitted.

[0454] (Structure of lead frame and semiconductor device)

[0455] Fig.46 1 is a cross-sectional view showing a lead frame 10C according to the present embodiment. Fig.47 2 is a cross-sectional view showing a semiconductor device 20C according to the present embodiment.

[0456] exist Fig.46 The lead frame 10C shown and Fig.47 In the semiconductor device 20C shown, a recess 18 is formed on the front surface of the lead portion 12, on the outer side of the metal layer 25 (on the opposite side of the chip pad 11). In addition, the portion adjacent to the outer side of the recess 18 (the third front surface portion 54c) is a rough surface. The entire inner surface of the recess 18 is a rough surface. The portion located between the recess 18 and the metal layer 25 (the fourth front surface portion 54d) is a smooth surface.

[0457] In this embodiment, the definition and measurement method of "rough surface" and "smooth surface" are the same as those in the second embodiment.

[0458] (Lead frame manufacturing method)

[0459] Next, use Fig.48 (a)-(j) pairs Fig.46 A method for manufacturing the lead frame 10C shown in FIG. Fig.48 In (a)-(j), Fig.35 The same components as shown in (a) to (j) are denoted by the same reference numerals and detailed descriptions thereof are omitted.

[0460] First, with the above Fig.35 The steps (a) and (b) are similar to those shown in FIG. Fig.48 (a)), photosensitive resists 32a and 33a are formed on the front and back surfaces of the metal substrate 31, respectively. Fig.48 (b)).

[0461] Then, with the above Fig.35 The etching resist layers 32 and 33 having openings 32b and 33b are formed in substantially the same manner as in the step (c) of FIG. Fig.48 (c)). In addition, at this time, the opening 32b is also formed in the area corresponding to the recess 18.

[0462] Then, with the above Fig.35 The process (d) shown in FIG. 1 is substantially the same as that of FIG. 1 , and the outer shapes of the chip pad 11, the lead portion 12, and the connection bar 13 are formed by etching the metal substrate 31. Fig.48 (d)). In addition, at this time, a recess 18 is formed on the front surface of the lead portion 12. Next, Fig.35 The etching resist layers 32 and 33 are removed by stripping in substantially the same manner as in the step (e) of FIG. Fig.48 (e)).

[0463] Then, with the above Fig.35 The plating layer 36 ( Fig.48 (f)). In addition, at this time, the plating layer 36 is also formed in the recessed portion 18.

[0464] Next, the portions of the plating layer 36 corresponding to the first die pad side surface 11c, the second die pad side surface 11d, the third front surface portion 54c, the recess 18, the inner lead end surface 51c, and the inner lead back surface 51b of the metal substrate 31 are removed ( Fig.48 (g)).

[0465] During this period, if Fig.48 As shown in (g), first, elastic members 46 such as rubber pads are arranged on the front and back sides of the metal substrate 31, and the metal substrate 31 is clamped by the clamp 47F via the elastic members 46. In addition, the elastic member 46 on the front side of the metal substrate 31 covers the chip holder front side 11a, the area corresponding to the fourth front portion 54d, and the area where the metal layer 25 of the lead portion 12 is provided. Next, the plating layer 36 of the portion not covered by the elastic member 46 is peeled off and removed. As a result, the first chip holder side surface 11c, the second chip holder side surface 11d, the third front portion 54c, the recess 18, the inner lead terminal surface 51c, and the inner lead back surface 51b are exposed. On the other hand, the plating layer 36 on the chip holder front side 11a, the chip holder back surface 11b, the fourth front portion 54d, and the external terminal 17 covered by the elastic member 46 remains.

[0466] Then, with the above Fig.35 The support layer 37 is provided on the back side of the metal substrate 31 in substantially the same manner as the step (h) shown in FIG. Next, the portion of the metal substrate 31 not covered by the plating layer 36 is roughened, thereby forming a rough surface ( Fig.48 (h)). As a result, the first die pad side surface 11c, the second die pad side surface 11d, the third front surface portion 54c, the inner surface of the recess 18, the inner lead terminal surface 51c, and the inner lead back surface 51b become rough surfaces.

[0467] Then, with Fig.35The step (i) shown in FIG. 1 is similar to the step in which the support layer 37 and the plating layer 36 are sequentially peeled off and removed. Fig.48 (i)).

[0468] Then, with the above Fig.35 The metal layer 25 is formed on the chip pad 11 and the lead portion 12 in a substantially similar manner to the step (j) shown in FIG. Fig.46 The lead frame 10C shown ( Fig.48 (j)).

[0469] (Method for manufacturing semiconductor device)

[0470] The method for manufacturing the semiconductor device 20C of this embodiment can be Fig.36 The method for manufacturing the semiconductor device 20 shown in (a) to (d) is performed in substantially the same manner.

[0471] According to the present embodiment, the fourth front surface portion 54d adjacent to the outer side of the metal layer 25 in the front surface of the lead portion 12 is formed into a smooth surface. Thus, when the semiconductor element 21 is mounted on the die pad 11, it is possible to suppress the tin contained in the bump 26 from flowing out along the fourth front surface portion 54d (see Fig.49 Arrow F C On the other hand, if the fourth front surface portion 54d is a rough surface, tin and the like contained in the bump 26 may flow out along the fourth front surface portion 54d due to surface tension.

[0472] In addition, according to the present embodiment, the recessed portion 18 is formed outside the metal layer 25 in the front surface of the lead portion 12. Thus, even if the tin or the like contained in the bump 26 flows out along the fourth front surface portion 54d, the flowing tin or the like can be received by the recessed portion 18. Thus, the flowing tin or the like can be prevented from reaching the third front surface portion 54c.

[0473] In addition, according to the present embodiment, the inner surface of the recess 18 and the third front surface portion 54c are roughened. Therefore, the distance of the moisture intrusion path at the interface between the surface of the lead portion 12 and the sealing resin 23 becomes longer. Thus, it is possible to suppress the moisture from intruding from the interface between the surface of the lead portion 12 and the sealing resin 23 to the semiconductor element 21 side (see Fig.49 Arrow F B ). As a result, the reliability of the semiconductor device 20C after long-term use can be improved.

[0474] In addition, according to this embodiment, the inner surface of the recess 18 and the third front portion 54c are roughened, thereby improving the adhesion strength between the recess 18 and the third front portion 54c and the sealing resin 23, and preventing the surface of the lead portion 12 and the sealing resin 23 from peeling off from each other.

[0475] In addition, according to the present embodiment, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 is lengthened on the back side of the semiconductor device 20C. This can suppress the moisture from intruding from the interface between the sealing resin 23 and the die pad 11 or the lead portion 12 to the semiconductor element 21 side (see Fig.49 Arrow F A ). As a result, the reliability of the semiconductor device 20C after long-term use can be improved.

[0476] (Ninth Implementation Method)

[0477] Reference Figures 50 to 57 A ninth embodiment will be described. Figures 50 to 57 is a diagram showing a ninth embodiment. Figures 50 to 57 In, with Figures 8 to 49 The same parts in the illustrated embodiments are denoted by the same reference numerals and detailed description thereof will be omitted.

[0478] (Lead frame structure)

[0479] First, use Fig.50 and Fig.51 The outline of the lead frame according to the present embodiment will be described. Fig.50 and Fig.51 It is a diagram showing a lead frame according to this embodiment.

[0480] like Fig.50 and Fig.51 As shown, each packaging area 10a of the lead frame 10 includes a chip pad 11 and a lead portion 12 located around the chip pad 11. Among them, a part of the lead portion 12 is thinned from the back side. The thinned portion on the back side of the lead portion 12 becomes a rough surface. The non-thinned portion on the back side of the lead portion 12 becomes a smooth surface.

[0481] like Fig.51 As shown, the chip pad 11 has a chip pad front side 11a located on the front side and a chip pad back side 11b located on the back side. On the chip pad front side 11a, a semiconductor element 21 is mounted as described later. The chip pad back side 11b is exposed to the outside from the semiconductor device 20 (described later). In addition, a chip pad side surface 11h is formed on the side of the chip pad 11 facing the lead portion 12. The chip pad side surface 11h extends from the chip pad front side 11a to the chip pad back side 11b in the thickness direction (Z direction). In this case, the chip pad side surface 11h becomes a rough surface. That is, a third rough surface R3 is formed on the chip pad side surface 11h. On the other hand, the chip pad back side 11b is a smooth surface.

[0482] In the present embodiment, a "rough surface" refers to a surface with an S-ratio of 1.10 or more. A "smooth surface" refers to a surface with an S-ratio of less than 1.10. A rough surface is a surface that is rougher than a smooth surface. In addition, the S-ratio of the "rough surface" is preferably greater than 1.10 and less than 2.30. The S-ratio of the "smooth surface" is preferably greater than 1.00 and less than 1.10. Here, "S-ratio" represents the surface area ratio obtained by dividing the surface as the measurement object into multiple pixels and measuring using an optical interferometer measuring instrument. Specifically, using VertScan manufactured by Hitachi High-Tech Science, the surface as the measurement object is divided into multiple pixels for measurement, and the obtained surface area is divided by the observation area to calculate.

[0483] The rough surface can also be formed by roughening the outer surface of the metal substrate 31 described later using, for example, a micro-etching liquid. Examples of such micro-etching liquids include micro-etching liquids with sulfuric acid or hydrochloric acid as main components (e.g., the first micro-etching liquid described later). Alternatively, micro-etching liquids with hydrogen peroxide and sulfuric acid as main components (e.g., the second micro-etching liquid described later) can also be used as micro-etching liquids. The smooth surface can also be an unprocessed surface that is not subjected to such a roughening treatment on the metal substrate 31 described later. In addition, in Fig.51 In FIG. 1 , a rough surface with relatively smooth roughness (such as the first rough surface R1 described later) is represented by a thin dotted line. Fig.51 In FIG. 1 , rough surfaces having relatively rough roughness (eg, a second rough surface R2 , a third rough surface R3 , a fourth rough surface R4 , and a fifth rough surface R5 described later) are indicated by thick dotted lines (the same applies to other cross-sectional views).

[0484] The chip pad front surface 11a of the chip pad 11 is a region (internal terminal) bonded to the semiconductor element 21 via an adhesive 24 such as a die attach paste as described later. The chip pad front surface 11a may also be a region that has not been thinned by half etching or the like. In addition, a first rough surface R1 is formed on the chip pad front surface 11a. Here, the roughness of the first rough surface R1 is smoother (not rough) than the roughness of the second rough surface R2 of the lead portion 12 described later. Specifically, the S-ratio of the first rough surface R1 may be greater than 1.10 and less than 1.30.

[0485] In the present embodiment, the first rough surface R1 is formed over the entire area of ​​the chip pad front surface 11a. However, the present invention is not limited thereto, and the first rough surface R1 may be formed on a portion of the chip pad front surface 11a. It is particularly preferred that the first rough surface R1 is formed on the outer periphery of the mounting area of ​​the semiconductor element 21 in the chip pad front surface 11a. As a result, as described later, it is possible to suppress the phenomenon (bleeding) of the epoxy resin and other components in the adhesive 24 seeping out due to the capillary phenomenon of the chip pad front surface 11a. In addition, the first rough surface R1 may be formed along the entire area of ​​the periphery of the chip pad 11. In the case where the first rough surface R1 is formed on a portion of the chip pad front surface 11a, the portion other than the first rough surface R1 may also be a smooth surface. Alternatively, the portion other than the first rough surface R1 of the chip pad front surface 11a may also be a rough surface having a rougher roughness than the first rough surface R1. For example, the S-ratio of the portion other than the first rough surface R1 of the chip pad front surface 11a may also be greater than 1.30 and less than 2.30.

[0486] Reference Fig.51 The chip pad back surface 11b is not thinned by half etching, for example, and becomes a smooth surface similar to the metal substrate (metal substrate 31 described later) before processing. The chip pad back surface 11b is exposed to the outside of the semiconductor device 20 after the semiconductor device 20 (described later) is manufactured.

[0487] Each lead portion 12 is connected to the semiconductor element 21 via a connection wire 22 as described later, and is disposed with a space between the die pad 11. The plurality of lead portions 12 are disposed at intervals along the longitudinal direction of the connection bar 13. Each lead portion 12 extends from the connection bar 13.

[0488] like Fig.51 As shown, the lead portion 12 includes an inner lead 51 and a terminal portion 53. The inner lead 51 is located on the inner side (chip holder 11 side). The terminal portion 53 is located on the outer side (connection bar 13 side). The inner lead 51 extends from the terminal portion 53 to the chip holder 11 side. An internal terminal is formed on the front side of the inner lead 51. The internal terminal is a region electrically connected to the semiconductor element 21 via the connection wire 22 as described later. A metal layer 25 is provided on the internal terminal for improving the close contact with the connection wire 22.

[0489] In the present embodiment, the thin-walled portion of the back side of the lead portion 12 becomes a rough surface. Specifically, the inner lead 51 of the lead portion 12 is thin-walled from the back side. The entire area of ​​the inner lead back side 51b located on the back side of the inner lead 51 is a rough surface. That is, the fourth rough surface R4 is formed on the inner lead back side 51b. On the other hand, the non-thin-walled portion of the back side of the lead portion 12 becomes a smooth surface. Specifically, the terminal portion 53 of the lead portion 12 is not thin-walled from the back side. The entire area of ​​the external terminal 17 located on the back side of the terminal portion 53 is a smooth surface.

[0490] Furthermore, the entire area of ​​the inner lead end surface 51c of the lead portion 12 becomes a rough surface. That is, the fifth rough surface R5 is formed on the inner lead end surface 51c. In addition, although not shown, both side surfaces along the long side direction of the lead portion 12 may also be rough surfaces. On the other hand, the inner lead 51 of the lead portion 12 is not thinned from the front side. In addition, the terminal portion 53 of the lead portion 12 is not thinned from the front side.

[0491] The lead front surface 12a is formed by the inner lead front surface 51a of the inner lead 51 and the terminal portion front surface 53a of the terminal portion 53. The lead front surface 12a is a region that has not been thinned from the front side by half etching, etc. A smooth surface region S as a smooth surface region and a second rough surface R2 as a rough surface region are formed on the lead front surface 12a.

[0492] The smooth surface area S is located at the inner end (chip seat 11 side) of the lead portion 12. A metal layer 25 is formed on the smooth surface area S. In this case, the metal layer 25 covers the entire smooth surface area S when viewed from above. The metal layer 25 can be, for example, a plated layer formed by electroplating. The thickness of the metal layer 25 can be greater than 1 μm and less than 10 μm. As a metal constituting such a plated layer, silver, silver alloy, gold, gold alloy, platinum group, copper, copper alloy, palladium, etc. can be used. Depending on the metal constituting the metal layer 25, when base plating is required, it is sufficient to apply a known material such as nickel or copper.

[0493] In this case, one smooth surface region S is formed on the lead front surface 12a of each lead portion 12. However, the present invention is not limited thereto, and a plurality of smooth surface regions S may be formed on the lead front surface 12a of each lead portion 12. In addition, the smooth surface region S may not be formed on the lead front surface 12a of each lead portion 12. That is, the entire lead front surface 12a of each lead portion 12 may be the second rough surface R2.

[0494] The second rough surface R2 is located outside the smooth surface region S and the metal layer 25 (on the connecting bar 13 side). In this case, the second rough surface R2 is provided only at a position outside the smooth surface region S (on the connecting bar 13 side). However, the present invention is not limited thereto, and the second rough surface R2 may be provided so as to surround the smooth surface region S in a plan view. The lead front surface 12a may also be composed only of the smooth surface region S and the second rough surface R2.

[0495] In this embodiment, the roughness of the second rough surface R2 is greater than the roughness of the first rough surface R1 of the chip pad 11. Specifically, the S-ratio of the second rough surface R2 may be greater than 1.30 and less than 2.30. On the other hand, as described above, the S-ratio of the first rough surface R1 may be greater than 1.10 and less than 1.30.

[0496] The roughness of the third rough surface R3 of the chip seat 11 may be greater than the roughness of the first rough surface R1. The S-ratio of the third rough surface R3 may be greater than 1.30 and less than 2.30. In addition, the roughness of the fourth rough surface R4 of the lead portion 12 may be greater than the roughness of the first rough surface R1. The S-ratio of the fourth rough surface R4 may be greater than 1.30 and less than 2.30. In addition, the roughness of the fifth rough surface R5 of the lead portion 12 may be greater than the roughness of the first rough surface R1. The S-ratio of the fifth rough surface R5 may be greater than 1.30 and less than 2.30.

[0497] The roughness of the second rough surface R2, the third rough surface R3, the fourth rough surface R4 and the fifth rough surface R5 may be different or the same.

[0498] In addition, the structure of the lead frame 10 of this embodiment may be the same as the structure of the lead frame 10 of the second embodiment.

[0499] (Structure of Semiconductor Device)

[0500] Next, use Fig.52 and Fig.53 A semiconductor device according to this embodiment will be described. Fig.52 and Fig.53 It is a diagram showing a semiconductor device (QFN type) according to this embodiment.

[0501] like Fig.52 and Fig.53 As shown, the semiconductor device (semiconductor package) 20 includes a die pad 11 , a semiconductor element 21 , a plurality of lead portions 12 , a plurality of connection wires 22 , and a sealing resin 23 .

[0502] The semiconductor element 21 is mounted on the die pad 11. The plurality of connection wires 22 electrically connect the semiconductor element 21 to the metal layer 25 of the lead portion 12. In this case, the connection wires 22 constitute a connection member. The sealing resin 23 seals the die pad 11, the lead portion 12, the semiconductor element 21, and the connection wires 22 with resin.

[0503] The die pad 11 and the lead portion 12 are made of the lead frame 10. In this case, the first rough surface R1 is formed on the die pad front surface 11a of the die pad 11. In addition, the second rough surface R2 is formed on the lead front surface 12a of the lead portion 12 at a position outside the metal layer 25 (the side away from the die pad 11). The roughness of the second rough surface R2 of the lead portion 12 is greater than the roughness of the first rough surface R1 of the die pad 11.

[0504] In addition, a third rough surface R3 is formed on the chip seat side surface 11h of the chip seat 11. The roughness of the third rough surface R3 is greater than the roughness of the first rough surface R1. The sealing resin 23 is tightly attached to the chip seat side surface 11h. The inner lead 51 of the lead portion 12 is thinned from the back side. The inner lead back side 51b of the inner lead 51 becomes the fourth rough surface R4. The roughness of the fourth rough surface R4 is greater than the roughness of the first rough surface R1. The sealing resin 23 is tightly attached to the inner lead back side 51b. In addition, a fifth rough surface R5 is formed on the inner lead end surface 51c of the inner lead 51. The roughness of the fifth rough surface R5 is greater than the roughness of the first rough surface R1. The sealing resin 23 is tightly attached to the inner lead end surface 51c. The terminal portion 53 of the lead portion 12 is not thinned from the back side. The external terminal 17 located on the back side of the terminal portion 53 is a smooth surface. The external terminal 17 is exposed to the outside from the sealing resin 23 .

[0505] As the semiconductor element 21, various semiconductor elements commonly used in the past can be used without particular limitation, and for example, an integrated circuit, a large-scale integrated circuit, a transistor, a thyristor, a diode, etc. can be used. The semiconductor element 21 has a plurality of electrodes 21a, each of which is provided with a connection wire 22. In addition, the semiconductor element 21 is fixed to the front surface of the die holder 11 by an adhesive 24 such as a die attach paste. The adhesive 24 may also be an epoxy resin-based adhesive containing components such as silver paste and epoxy resin.

[0506] Each connection wire 22 is made of a material with good conductivity, such as gold or copper. One end of each connection wire 22 is connected to the electrode 21a of the semiconductor element 21, and the other end thereof is connected to the metal layer 25 located on each lead portion 12. As a connection member, a conductor such as a bump may be used instead of the connection wire 22. In this case, the semiconductor element 21 and the lead portion 12 can be connected by a flip chip bonding agent.

[0507] As the sealing resin 23, a thermosetting resin such as silicone resin or epoxy resin, or a thermoplastic resin such as PPS resin can be used. The overall thickness of the sealing resin 23 can also be set to about 300 μm or more and 1500 μm or less. In addition, one side of the sealing resin 23 (one side of the semiconductor device 20) can also be set to, for example, 0.2 mm or more and 20 mm or less. In addition, Fig.52 In FIG. 1 , the portion of the sealing resin 23 that is located on the front side of the lead portion 12 and the semiconductor element 21 is omitted.

[0508] In addition, the structure of the die pad 11 and the lead portion 12 is the same as that of the above-mentioned embodiment except for the region not included in the semiconductor device 20. Fig.50 and Fig.51 The structures shown are the same, so detailed description is omitted here.

[0509] (Lead frame manufacturing method)

[0510] Next, use Fig.54 (a)-(e) and Fig.55 (a)-(h) pairs Fig.50 and Fig.51 A method for manufacturing the lead frame 10 shown will be described. Fig.54 (a)-(e) and Fig.55 (a) to (h) are cross-sectional views showing a method for manufacturing the lead frame 10 (with Fig.51 corresponding figure).

[0511] First, compared with the second embodiment ( Fig.14 In the case of (a) to (e)), a metal substrate 31 having a chip pad 11 and a lead portion 12 located around the chip pad 11 is prepared in the same manner. Fig.54 (a)-(e)).

[0512] Next, a plating layer (covering layer) 36 ( Fig.55 (a)). At this time, the plating layer 36 can be formed on the entire portion of the chip seat 11, the lead portion 12 and the connecting bar 13 exposed to the outside. The thickness of the plating layer 36 can also be greater than 0μm and less than 2μm. As a metal constituting the plating layer 36, for example, silver can also be used. When the plating layer 36 is composed of a silver plating layer, a silver plating solution containing silver cyanide and potassium cyanide as main components can be used as a plating solution for electroplating.

[0513] Next, the plating layer 36 existing in the region where the first rough surface R1 is formed in the metal substrate 31 is removed. Specifically, the plating layer 36 located in the entire region of the die pad front surface 11a of the die pad 11 is removed ( Fig.55(b)). In this case, for example, the front and back sides of the metal substrate 31 other than the chip holder front side 11a are clamped by a clamp through an elastic member. Then, the plating layer 36 of the portion not covered by the elastic member and the clamp can be peeled off and removed. Thus, the plating layer 36 on the chip holder front side 11a is removed.

[0514] Next, by roughening the portion of the metal substrate 31 that is not covered by the plating layer 36, a first rough surface R1 ( Fig.55 (c)). Specifically, by supplying the first micro-etching liquid to the metal substrate 31, the first rough surface R1 is formed on the entire front surface 11a of the chip seat that is not covered by the plating layer 36. Here, the first micro-etching liquid refers to a surface treatment agent that slightly dissolves the metal surface to form the first rough surface R1 with fine irregularities. For example, when roughening the metal substrate 31 composed of copper or a copper alloy, a micro-etching liquid containing sulfuric acid or hydrochloric acid as a main component can be used as the first micro-etching liquid.

[0515] Next, the plating layer 36 existing in the metal substrate 31 in the area other than the smooth surface area S (area where the metal layer 25 is formed) of the lead front surface 12a is removed. In this case, for example, the front and back surfaces of the metal substrate 31 other than the smooth surface area S are clamped by a clamp through an elastic member. Next, the plating layer 36 of the portion not covered by the elastic member and the clamp may be peeled off and removed. Thus, the plating layer 36 of the chip holder back surface 11b and the chip holder side surface 11h of the chip holder 11 is removed. In addition, in the lead portion 12, the plating layer 36 of the portion other than the smooth surface area S of the lead front surface 12a, the inner lead back surface 51b, the inner lead end surface 51c, and the external terminal 17 is removed.

[0516] Next, a protective layer 37A ( Fig.55 (e)). The protective layer 37A may be, for example, a resist layer. The protective layer 37A on the front side covers the chip holder front side 11a of the chip holder 11 and the plating layer 36 on the smooth surface area S of the lead portion 12. In this case, the protective layer 37A on the front side covers the entire area of ​​the first rough surface R1 of the chip holder 11. In addition, the protective layer 37A on the front side may also cover a part or the entire area of ​​the plating layer 36 on the smooth surface area S. The protective layer 37A on the back side covers the chip holder back side 11b of the chip holder 11 and the external terminal 17 of the lead portion 12.

[0517] Next, by roughening the portion of the metal substrate 31 not covered by the plating layer 36 and the protective layer 37A, a rough surface ( Fig.55(f)). Specifically, the second rough surface R2 is formed on a portion of the lead front surface 12a of the lead portion 12. The third rough surface R3 is formed on the chip pad side surface 11h of the chip pad 11. In addition, the fourth rough surface R4 is formed on the inner lead back surface 51b of the lead portion 12. Furthermore, the fifth rough surface R5 is formed on the inner lead terminal end surface 51c of the lead portion 12.

[0518] During this period, the second micro-etching liquid is supplied to the metal substrate 31. Thus, a rough surface is formed on the entire metal substrate 31 except for the portion covered by the plating layer 36 and the protective layer 37A. Here, the second micro-etching liquid refers to a surface treatment agent that slightly dissolves the metal surface to form a rough surface with fine concave and convex shapes. For example, in the case of roughening the metal substrate 31 composed of copper or a copper alloy, a micro-etching liquid with hydrogen peroxide and sulfuric acid as main components can also be used as the second micro-etching liquid. The second micro-etching liquid can contain components different from the above-mentioned first micro-etching liquid. Compared with the first micro-etching liquid, the second micro-etching liquid makes the metal rougher. Therefore, the second rough surface R2, the third rough surface R3, the fourth rough surface R4 and the fifth rough surface R5 are respectively rougher than the first rough surface R1.

[0519] Next, the protective layer 37A and the plating layer 36 on the front side of the metal substrate 31 are peeled off and removed ( Fig.55 (g)). At this time, the plating layer 36 covering the front surface 12a of the lead is removed, and the smooth surface area S is exposed. In addition, the protective layer 37A on the back side remains on the metal substrate 31.

[0520] Then, a metal layer 25 ( Fig.55 (h)). In this case, first, a plating resist layer of a predetermined pattern (not shown) is formed on the chip base 11 and the lead portion 12 except for the smooth surface area S, for example, by photolithography. Next, a metal layer 25 composed of a plating layer is formed in the smooth surface area S not covered by the plating resist layer, for example, by electroplating. Then, the plating resist layer is removed, thereby obtaining Fig.50 and Fig.51 The lead frame 10 is shown.

[0521] (Method for manufacturing semiconductor device)

[0522] Next, use Fig.56 (a)-(e) Fig.52 and Fig.53 A method for manufacturing the semiconductor device 20 shown will be described. Fig.56 (a) to (e) are cross-sectional views showing a method for manufacturing the semiconductor device 20 (with Fig.53 corresponding figure).

[0523] First, by e.g. Fig.54 (a)-(e) and Fig.55 The lead frame 10 ( Fig.56 (a)).

[0524] Next, the semiconductor element 21 is mounted on the die pad 11 of the lead frame 10. In this case, the semiconductor element 21 is mounted and fixed on the die pad 11 using an adhesive 24 such as a die attach paste ( Fig.56 (b)). The adhesive 24 may also be an epoxy resin adhesive containing components such as silver paste and epoxy resin. At this time, the semiconductor element 21 is arranged on the first rough surface R1 of the chip pad front surface 11a via the adhesive 24. In addition, the first rough surface R1 is provided along the periphery of the semiconductor element 21 and the adhesive 24.

[0525] Next, each electrode 21a of the semiconductor element 21 and the metal layer 25 formed on each lead portion 12 are electrically connected to each other through a connection wire (connection member) 22 ( Fig.56 (c)).

[0526] Next, the lead frame 10 is injection molded or transfer molded with a thermosetting resin or a thermoplastic resin to form a sealing resin 23 ( Fig.56 (d)). Thus, the die pad 11, the lead portion 12, the semiconductor element 21, and the connection wires 22 are sealed with resin.

[0527] Then, the lead frame 10 and the sealing resin 23 are cut for each packaging region 10a. Thus, the lead frame 10 is separated for each semiconductor device 20 to obtain Fig.52 and Fig.53 The semiconductor device 20 ( Fig.56 (e)).

[0528] In addition, during the manufacturing of the semiconductor device 20, a step of heating and curing the adhesive 24 is performed ( Fig.56 (b)). Specifically, after the adhesive 24 such as the chip mounting paste is applied to the chip holder 11 and the semiconductor element 21 is mounted on the chip holder 11, the adhesive 24 is heated and cured. At this time, the epoxy resin and other components in the applied adhesive 24 may seep out due to the capillary phenomenon of the front surface 11a of the chip holder. Such a phenomenon is also called seepage or epoxy seepage.

[0529] In contrast, according to the present embodiment, the first rough surface R1 is formed on the chip pad front surface 11a of the chip pad 11. The roughness of the first rough surface R1 is suppressed compared to the roughness of the second rough surface R2. As a result, the phenomenon (bleeding) of the epoxy resin or the like in the adhesive 24 seeping out due to the capillary phenomenon caused by the unevenness of the chip pad front surface 11a can be suppressed (see Fig.57 Arrow E). On the other hand, it is also possible to make the chip holder front surface 11a around the adhesive 24 a smooth surface. However, if the viscosity of the epoxy resin in the adhesive 24 is low, the epoxy resin is more likely to flow along the chip holder front surface 11a, which is a smooth surface. Therefore, in this embodiment, the roughness of the chip holder front surface 11a is appropriately roughened to a degree that does not cause capillary phenomenon (set as the first rough surface R1). As a result, regardless of the viscosity of the epoxy resin in the adhesive 24, the epoxy resin can be suppressed from flowing along the chip holder front surface 11a.

[0530] If such a semiconductor device 20 is used for a long time, moisture in the air may enter from the side or back side of the semiconductor device 20. For example, moisture may enter through the interface between the sealing resin 23 and the die pad 11 or the lead portion 12.

[0531] In contrast, according to the present embodiment, the second rough surface R2 is formed on the lead front surface 12a of the lead portion 12. Therefore, the distance of the moisture intrusion path at the interface between the lead front surface 12a and the sealing resin 23 becomes longer. Thus, it is possible to suppress moisture from intruding from the interface between the lead front surface 12a and the sealing resin 23 to the semiconductor element 21 side (see Fig.57 Arrow F A ). As a result, the reliability of the semiconductor device 20 after long-term use can be improved.

[0532] In addition, according to the present embodiment, the die pad side surface 11h of the die pad 11 is formed into a third rough surface R3. The roughness of the third rough surface R3 is greater than the roughness of the first rough surface R1. Therefore, on the back side of the semiconductor device 20, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the die pad 11 becomes longer. As a result, it is possible to suppress the moisture from intruding from the interface between the sealing resin 23 and the die pad 11 to the semiconductor element 21 side (see Fig.57 Arrow F B As a result, the reliability of the semiconductor device 20 after long-term use can be improved. Furthermore, the adhesion strength between the die pad 11 and the sealing resin 23 can be improved, and the die pad 11 and the sealing resin 23 can be prevented from peeling off from each other.

[0533] In addition, according to the present embodiment, the inner lead back surface 51b of the lead portion 12 becomes the fourth rough surface R4. Furthermore, the inner lead end surface 51c of the lead portion 12 becomes the fifth rough surface R5. The roughness of the fourth rough surface R4 and the roughness of the fifth rough surface R5 are respectively greater than the roughness of the first rough surface R1. Therefore, on the back side of the semiconductor device 20, the distance of the moisture intrusion path at the interface between the sealing resin 23 and the lead portion 12 becomes longer. As a result, it is possible to suppress the moisture from intruding from the interface between the sealing resin 23 and the lead portion 12 to the semiconductor element 21 side (refer to Fig.57 Arrow F c As a result, the reliability of the semiconductor device 20 after long-term use can be improved. Furthermore, the adhesion strength between the lead portion 12 and the sealing resin 23 can be improved, and the lead portion 12 and the sealing resin 23 can be prevented from peeling off from each other.

[0534] (Variation Example)

[0535] Next, use Fig.58 Modifications of the lead frame 10 of the present embodiment will be described. Fig.58 is a cross-sectional view showing a lead frame 10 according to a modified example. Fig.58 In, with Figures 50 to 57 The same parts as shown in the above-mentioned embodiments are denoted by the same reference numerals and detailed description thereof will be omitted.

[0536] exist Fig.58 In the embodiment, the smooth surface region S and the second rough surface R2 are formed on the lead front surface 12 a of the lead portion 12 . In this case, the metal layer 25 is not provided on the smooth surface region S. Therefore, the smooth surface region S is exposed to the outside of the lead frame 10 .

[0537] In the making Fig.58 In the case of the lead frame 10 shown in the figure, when the above Fig.54 (a)-(e) and Fig.55 After the steps (a) to (g) shown in FIG. 1 , the step of forming the metal layer 25 is not performed ( Fig.55 Thus, we can get Fig.58 The lead frame 10 is shown.

[0538] Thus, by not providing the metal layer 25 in the smooth surface region S, the manufacturing process of the lead frame 10 can be reduced. In addition, by not providing the metal layer 25 composed of a plating layer of silver, silver alloy, gold, gold alloy, platinum group, copper, copper alloy, palladium, etc., the manufacturing cost of the lead frame 10 can be reduced. In addition, it is more effective in the case of a method of connecting the semiconductor element 21 and the lead portion 12 by a flip chip bonding agent instead of a method of connecting the semiconductor element 21 and the lead portion 12 by wire bonding.

[0539] A plurality of components disclosed in the above-mentioned embodiments and modified examples may be appropriately combined as needed. Alternatively, some components may be deleted from all the components disclosed in the above-mentioned embodiments and modified examples.

Claims

1. A lead frame, wherein: The lead frame comprises: A chip holder for mounting a semiconductor device; and A lead portion located around the chip base, A smooth surface area is formed on the front surface of the chip holder or the front surface of the lead portion, A rough surface region exists so as to surround the entire circumference of the smooth surface region, The smooth surface region is made of the same material as the rough surface region.

2. The lead frame according to claim 1, wherein: The rough surface region is formed along the entire periphery of the die pad or the entire periphery of the lead portion in a plan view.

3. The lead frame according to claim 1, wherein: The lead portion has an inner lead whose wall is thinned from the back side, An inner lead front surface is formed on the front side of the inner lead, an inner lead back surface is formed on the back side of the inner lead, and an inner lead terminal surface is formed on the surface of the inner lead facing the chip seat. An external terminal is formed on a portion of the back side of the lead portion that is not thinned. The back surface of the inner lead and the end surface of the inner lead are roughened. The external terminal has a smooth surface.

4. The lead frame according to claim 1, wherein: The back surface of the chip pad is a smooth surface, and the side surface of the chip pad is a rough surface.

5. The lead frame according to claim 1, wherein: The area of ​​the smooth surface is circular, elliptical or oblong when viewed from above.

6. The lead frame according to claim 1, wherein: The area of ​​the smooth surface is square or rectangular when viewed from above.

7. The lead frame according to claim 1, wherein: The smooth surface region is a closed figure including curves and line segments when viewed from above.

8. The lead frame according to claim 1, wherein: The shortest distance between the smooth surface region and the periphery of the die pad or the periphery of the lead portion is greater than or equal to 0.025 mm and less than or equal to 1.0 mm.

9. The lead frame according to claim 1, wherein: The S-ratio of the rough surface is greater than 1.30, and the S-ratio of the smooth surface is less than 1.

30.

10. A method for manufacturing a lead frame, wherein: The method for manufacturing the lead frame comprises: A process for preparing a metal substrate; A step of forming a die pad and a lead portion located around the die pad by etching the metal substrate; forming a plating layer on a portion of the metal substrate; A step of forming a rough surface on a portion of the metal substrate that is not covered by the plating layer; and a step of removing the coating, A smooth surface area is formed on the front surface of the chip holder or the front surface of the lead portion, The rough surface region exists so as to surround the entire circumference of the smooth surface region.

Citation Information

Patent Citations

  • Circuit member, circuit member manufacturing method, semiconductor device and multilayer structure on circuit member surface

    CN101164165A

  • Lead frame, lead frame package, and method for manufacturing same

    CN108352376A

  • Device for mounting semiconductor element, lead frame, and substrate for mounting semiconductor element

    CN111755407A

  • Resin-sealed semiconductor device