Method for continuously preparing silicon-carbon negative electrode material, silicon-carbon negative electrode material and battery

By performing silane gas adsorption and pyrolysis deposition on carbon supports in a step-by-step manner under vacuum, the stability problem in the preparation process of silicon-carbon anode materials was solved, and the amount of silane adsorption and deposition was effectively controlled, thereby improving the cycle performance of the material and the stability of the battery.

CN119050258APending Publication Date: 2024-11-29吴胜水 +3
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411188348.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing silicon-carbon anode material preparation process has poor stability. Silane adsorption and cracking dehydrogenation occur in the same reaction unit, resulting in a decrease in specific surface area. Silane deposition on the porous carbon surface leads to a decrease in cycle performance.

Method used

Saturated adsorption of carbon support is carried out in a vacuum environment, and adsorption and pyrolysis deposition of silane gas are performed in two separate reaction vessels. By cyclically controlling the amount of silane adsorption and deposition, the stability problem of adsorption and pyrolysis deposition in the same fluidized bed in existing processes is avoided.

Benefits of technology

This improved the stability of the process, avoided the "floating silicon" problem on the carbon support surface, and significantly enhanced the cycle performance of silicon-carbon anode materials and the stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050258A_ABST
    Figure CN119050258A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a method for continuously preparing a silicon-carbon negative electrode material, which comprises the following steps: putting a carbon carrier into a first reaction container, and introducing silane gas in a vacuum environment to obtain a saturated silane gas adsorption carbon material; putting a carbon material into a second reaction container, and carrying out pyrolytic deposition treatment to obtain a silicon-carbon composite material of cracked and deposited nano silicon; and coating the surface of the silicon-carbon composite material with carbon source gas to form a coating layer, thereby obtaining the silicon-carbon negative electrode material. According to the method provided by the embodiment of the invention, the carbon carrier is subjected to saturated adsorption in the first reaction container in a vacuum environment, so that pores of the carbon carrier are fully filled with the silane gas; and the carbon material is placed in the second reaction container for pyrolytic deposition treatment, so that the problem of poor process stability caused by adsorption and pyrolytic deposition treatment in the same fluidized bed body is avoided, the process complexity is reduced, the problem of floating silicon on the surface of the carbon carrier is avoided, the expansion rate of the material in the lithium intercalation and deintercalation process is reduced, and the cycle performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium ion battery negative electrode materials, and in particular to a silicon-carbon negative electrode material, a method for continuously preparing the silicon-carbon negative electrode material, and a battery. Background Art

[0002] In recent years, lithium-ion batteries have been widely used in portable electronic devices, large-scale energy storage equipment, electric vehicles and other fields. Compared with the graphite anode commonly used in lithium-ion batteries, silicon materials have ultra-high theoretical specific capacity and low lithium desorption potential, which makes silicon materials one of the most promising choices for upgrading the carbon-based anode of lithium-ion batteries. However, as a semiconductor material, silicon itself has low electrical conductivity. During the electrochemical cycle, the insertion and extraction of lithium ions will cause the volume of the material to expand and contract by more than 300%. The mechanical force generated will gradually pulverize the material, causing structural collapse, and eventually leading to the separation of the electrode active material from the current collector, loss of electrical contact, and greatly reduced battery cycle performance. In addition, due to this volume effect, it is difficult for silicon to form a stable solid electrolyte interface (SEI) film in the electrolyte. Along with the destruction of the electrode structure, a new SEI film is continuously formed on the exposed silicon surface, exacerbating the corrosion and capacity decay of silicon.

[0003] At present, most silicon-carbon negative electrode materials are prepared by using monosilane gas as a silicon source and porous carbon as a carrier. The porous carbon carrier is placed in a fluidized bed reaction unit, and then nitrogen is introduced into it to exclude oxygen. After the temperature is raised to a specified temperature, an appropriate amount of silane gas is introduced, and the porous carbon is fluidized by the introduced gas flow. During this process, the gas is adsorbed simultaneously. Due to the high activity of silane, the nano-silicon generated by the cracking and dehydrogenation of silane at this temperature is deposited in the porous carbon carrier.

[0004] However, the existing schemes are carried out in the same reaction unit because adsorption and cracking dehydrogenation are carried out. With the deposition of nano-silicon, the specific surface area of ​​the reaction product gradually decreases, the weight of the reaction product continues to increase, the powder state continues to change, and the fluidization state is affected. Therefore, processes such as gas flow rate and the ratio of reaction gas to carrier gas have to be adjusted to ensure sufficient fluidization, resulting in poor process stability. In addition, the adsorption of silane in porous carbon carriers is a process of diffusion from the surface to the porous interior. In addition, silane is easily decomposed by heat, which inevitably leads to the deposition of silane on the porous carbon surface. The surface "floating silicon" lacks the rigid restraint of the porous inner wall. In the later repeated charge and discharge and lithium insertion and extraction process, it is easy to cause the destruction of the surface carbon coating and SEI film, resulting in a significant reduction in cycle performance. Summary of the invention

[0005] In view of at least some of the problems and shortcomings in the prior art, embodiments of the present invention disclose a method for continuously preparing a silicon-carbon negative electrode material, a silicon-carbon negative electrode material and a battery.

[0006] On the one hand, an embodiment of the present invention provides a method for continuously preparing a silicon-carbon negative electrode material, comprising: an adsorption step: placing a carbon carrier into a first reaction container, and introducing silane gas into the first reaction container under a vacuum environment to obtain a carbon material saturated with silane gas adsorption; a deposition step: placing the carbon material saturated with silane gas adsorption into a second reaction container, and performing pyrolysis deposition treatment, and obtaining a silicon-carbon composite material with cracked and deposited nano-silicon after cooling; a coating step: heating the silicon-carbon composite material with cracked and deposited nano-silicon of silane under the protection of an inert atmosphere, and coating the surface of the silicon-carbon composite material with a carbon source gas to form a coating layer, and obtaining the silicon-carbon negative electrode material after cooling.

[0007] In the embodiment of the present invention, the carbon carrier is saturatedly adsorbed under a vacuum environment in a first reaction vessel, thereby avoiding the introduction of a large amount of nitrogen gas and achieving sufficient filling of the pores of the carbon carrier with silane gas; the carbon material saturated with the adsorption of silane gas is then placed in a second reaction vessel for pyrolysis and deposition treatment. Since the adsorption process and the deposition process are carried out in two reaction vessels, the problem of poor process stability caused by the adsorption and pyrolysis and deposition treatments in the same fluidized bed body is avoided, thereby greatly reducing the complexity of the existing process. The effective control of the silane adsorption and deposition amounts is achieved through a circulation method, thereby avoiding the problem of "floating silicon" on the surface of the carbon carrier, and significantly improving the stability of the process.

[0008] In one embodiment of the present invention, after the deposition step and before the coating step, the step is further included: judging whether the silicon content in the silicon-carbon composite material of the cracked and deposited nano-silicon reaches a first predetermined content; if so, performing the coating step; if not, repeating the adsorption step and the deposition step until the silicon content in the silicon-carbon composite material of the cracked and deposited nano-silicon reaches the first predetermined content.

[0009] In one embodiment of the present invention, the first predetermined content is 45-60%.

[0010] In one embodiment of the present invention, the step of placing the carbon carrier in a first reaction container and introducing silane gas into the first reaction container under a vacuum environment to obtain a carbon material saturated with silane gas specifically includes: placing the carbon carrier in the first reaction container using nitrogen as a carrier gas; evacuating the first reaction container to a first vacuum degree and then introducing nitrogen gas to a first air pressure; determining whether the oxygen content in the first reaction container reaches a second predetermined content; if so, evacuating the first reaction container to a second vacuum degree and then introducing the silane gas to the first air pressure.

[0011] In one embodiment of the present invention, the first vacuum degree is less than or equal to 100 Pa, the second vacuum degree is less than or equal to 10 Pa, and the first air pressure is 10 5 Pa, the second predetermined content is 20ppm.

[0012] In one embodiment of the present invention, the carbon material saturated with silane gas adsorption is placed in a second reaction vessel and subjected to pyrolysis and deposition treatment, and after cooling, a silicon-carbon composite material with cracked and deposited nano-silicon is obtained. Specifically, the carbon material saturated with silane gas adsorption is placed in the second reaction vessel and continuously stirred at a temperature of 480-600°C to obtain a first intermediate product, and the oxygen content in the second reaction vessel is less than 20ppm; the first intermediate product is placed in a third reaction vessel, and after cooling to 360°C, the silicon-carbon composite material with cracked and deposited nano-silicon is obtained, and the oxygen content in the third reaction vessel is less than 20ppm.

[0013] In one embodiment of the present invention, the silicon-carbon composite material of cracked and deposited nano-silicon is heated under the protection of an inert atmosphere, and the carbon source gas is coated on the surface of the silicon-carbon composite material of cracked and deposited nano-silicon to form a coating layer, and the silicon-carbon negative electrode material is obtained after cooling. Specifically, the silicon-carbon composite material of cracked and deposited nano-silicon is placed in a fourth reaction container and heated at a temperature of 500-750°C under the protection of the inert atmosphere, and the carbon source gas is introduced into the fourth reaction container to obtain a second intermediate product; wherein the inert atmosphere is nitrogen, the carbon source gas is one or more of acetylene, propylene, and methane, and the oxygen content in the fourth reaction container is less than 20ppm; the second intermediate product is placed in a fifth reaction container, cooled to 50°C to obtain the silicon-carbon negative electrode material, and the oxygen content in the fifth reaction container is less than 20ppm.

[0014] In one embodiment of the present invention, the carbon carrier is a porous carbon material, the first reaction container and the second reaction container are connected by a pipeline, and a valve is provided at the connection between the first reaction container and the pipeline, and the valve is used to control the connection and closing between the first reaction container and the second reaction container.

[0015] On the other hand, an embodiment of the present invention provides a silicon-carbon negative electrode material, which is prepared by, for example, any of the aforementioned methods for continuously preparing a silicon-carbon negative electrode material.

[0016] On the other hand, a battery provided by an embodiment of the present invention, for example, includes a lithium-ion battery negative electrode plate, wherein the lithium-ion battery negative electrode plate includes a current collector and an active layer coated on the current collector, wherein the active layer includes a silicon-carbon negative electrode material prepared by any of the aforementioned methods for continuously preparing silicon-carbon negative electrode materials.

[0017] It can be seen from the above that the above technical features of the present invention can have one or more of the following beneficial effects: In the embodiment of the present invention, the carbon carrier is saturatedly adsorbed under a vacuum environment in the first reaction vessel, thereby avoiding the need to introduce a large amount of nitrogen as a carrier gas in the mainstream process of using a fluidized bed, saving costs, and more importantly, achieving sufficient filling of the pores of the carbon carrier with silane gas; the carbon material saturated with silane gas is then placed in a second reaction vessel for pyrolysis and deposition treatment. Since the adsorption process and the pyrolysis and deposition process are carried out in two reaction vessels, the problem of poor process stability caused by the currently commonly used adsorption treatment and pyrolysis and deposition treatment in the same fluidized bed is avoided, thereby greatly reducing the complexity of the existing process, and achieving effective control of the amount of silane adsorption and deposition through a circulation method, thereby avoiding the problem of "floating silicon" on the surface of the carbon carrier, and significantly improving the stability of the process. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0019] Figure 1 A schematic flow chart of a method for continuously preparing silicon-carbon negative electrode materials provided in an embodiment of the present invention.

[0020] Figure 2 This is a schematic diagram of the structure of the silicon-carbon negative electrode material preparation device.

[0021] Figure 3a This is a SEM (scanning electron microscope) image of the silicon-carbon negative electrode material (experimental group) prepared in accordance with an embodiment of the present invention.

[0022] Figure 3b This is the SEM (scanning electron microscope) image of the control group.

[0023] Figure 4 This is a comparison chart of battery performance test results between the silicon-carbon negative electrode material (experimental group) prepared in an embodiment of the present invention and the control group. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0026] It should also be noted that the division of multiple embodiments in the present invention is only for the convenience of description and should not constitute a special limitation. The features in various embodiments can be combined and referenced to each other without contradiction.

[0027] See also Figure 1 , a method for continuously preparing a silicon-carbon negative electrode material provided by an embodiment of the present invention, for example, comprises the steps of:

[0028] S12: adsorption step: placing the carbon carrier in a first reaction container, and introducing silane gas into the first reaction container under a vacuum environment to obtain a carbon material saturated with silane gas;

[0029] S14: Deposition step: placing the carbon material saturated with silane gas into a second reaction container and performing pyrolysis deposition treatment, and obtaining a silicon-carbon composite material with cracked and deposited nano-silicon after cooling;

[0030] S18: Coating step: heating the silicon-carbon composite material of cracked and deposited nano-silicon under the protection of an inert atmosphere, coating the surface of the silicon-carbon composite material of cracked and deposited nano-silicon with a carbon source gas to form a coating layer, and obtaining the silicon-carbon negative electrode material after cooling.

[0031] The carbon carrier mentioned above is, for example, a porous carbon material, and the silane gas mentioned above is, for example, monosilane gas. The pyrolysis deposition treatment mentioned above is, for example, a dehydrogenation cracking reaction of silane in the saturated adsorbed carbon material at high temperature, and the silane will dehydrogenate at high temperature to generate nano-silicon deposited in the pores of the carbon carrier to obtain a silicon-carbon composite material with cracked and deposited nano-silicon.

[0032] In a specific implementation of this embodiment, the method for continuously preparing silicon-carbon negative electrode materials further includes the following steps after the deposition step and before the coating step:

[0033] S162: Determine whether the silicon content in the silicon-carbon composite material obtained by cracking and depositing nano-silicon reaches a first predetermined content;

[0034] S164: If reached, the coating step is performed;

[0035] S166: If not reached, repeating the adsorption step and the deposition step until the silicon content in the cracked and deposited nano-silicon silicon-carbon composite material reaches the first predetermined content.

[0036] Wherein, the first predetermined content in step S166 is 45-60%.

[0037] Based on the above, step S12 specifically includes:

[0038] S122: placing the carbon carrier into the first reaction container using nitrogen as a carrier gas;

[0039] S124: evacuating the first reaction container to a first vacuum degree and then introducing nitrogen gas to a first pressure;

[0040] S126: Determine whether the oxygen content in the first reaction container reaches a second predetermined content;

[0041] S128: If the pressure is reached, the first reaction container is evacuated to a second vacuum degree and then the silane gas is introduced to the first pressure.

[0042] The first vacuum degree is less than or equal to 100 Pa, the second vacuum degree is less than or equal to 10 Pa, the first gas pressure is 105 Pa, and the second predetermined content is 20 ppm. It should be noted that in step S126, if the oxygen content in the first reaction container reaches the second predetermined content, S124 is repeated until the total oxygen content in the first reaction container reaches 20 ppm.

[0043] Step S14 specifically includes:

[0044] S142: placing the carbon material saturated with silane gas into the second reaction container and continuously stirring at a temperature of 480-600° C. to obtain a first intermediate product, wherein the oxygen content in the second reaction container is less than 20 ppm;

[0045] S144: placing the first intermediate product into a third reaction container, cooling it to 360° C. to obtain the silicon-carbon composite material of cracked and deposited nano-silicon.

[0046] The oxygen content in the second reaction container and the third reaction container is less than 20 ppm, and the saturated adsorption carbon material is continuously stirred so that it can be evenly heated and cooled.

[0047] It should be noted that the temperature in the first reaction container is, for example, lower than the temperature at which silane undergoes thermal decomposition, and for example, the temperature in the first reaction container is, for example, 25° C. to 360° C. In this way, the porous carbon can achieve saturated adsorption of silane under cold vacuum.

[0048] Step S18 specifically includes:

[0049] S182: placing the silicon-carbon composite material obtained by cracking and depositing nano-silicon into a fourth reaction container under the protection of the inert atmosphere, heating the mixture at a temperature of 500-750° C., and introducing the carbon source gas into the fourth reaction container to obtain a second intermediate product;

[0050] S184: placing the second intermediate product into a fifth reaction container and cooling it to 50° C. to obtain the silicon-carbon negative electrode material.

[0051] Wherein, the inert atmosphere is nitrogen, the carbon source gas is one or more of acetylene, propylene, and methane, and the oxygen content in the fourth reaction container and the fifth reaction container is less than 20 ppm. For example, the second intermediate product is cooled by circulating cooling water.

[0052] In the embodiment of the present invention, the carbon carrier is saturatedly adsorbed in a vacuum environment in a first reaction vessel, thereby avoiding the need to introduce a large amount of nitrogen as a carrier gas in the mainstream process of using a fluidized bed, saving costs and, more importantly, achieving sufficient filling of the pores of the carbon carrier with silane gas; the carbon material saturated with silane gas is then placed in a second reaction vessel for pyrolysis and deposition treatment. Since the adsorption process and the pyrolysis and deposition process are carried out in two reaction vessels, the problem of poor process stability caused by the currently commonly used adsorption treatment and pyrolysis and deposition treatment in the same fluidized bed body is avoided, thereby greatly reducing the complexity of the existing process, and achieving effective control of the silane adsorption and deposition amounts in a circulating manner, thereby avoiding the problem of "floating silicon" on the surface of the carbon carrier, and significantly improving the stability of the process.

[0053] For example, the method for continuously preparing silicon-carbon negative electrode materials provided in this embodiment is implemented in a silicon-carbon negative electrode material preparation device 10, Figure 2For example, it is a structural schematic diagram of a silicon-carbon negative electrode material preparation device 10, which includes a first reaction container 11, a second reaction container 12, a third reaction container 13, a fourth reaction container 14 and a fifth reaction container 15 connected in sequence by pipelines. Each reaction container has a valve at the lower end, and the valve is used to control the connection and closure between each reaction container and the reaction container connected to it. For example, the first reaction container 11 and the pipeline connection have a valve, and the valve can be used to control the connection and closure between the first reaction container 11 and the second reaction container 12. The third reaction container 13 can also be connected to the first reaction container 11 through a pipeline.

[0054] Specifically, the carbon carrier is placed in the first reaction container 11, and silane gas is introduced into the first reaction container 11 under a vacuum environment. The carbon carrier saturates the silane gas to obtain a carbon material saturated with silane gas. Subsequently, the valve between the first reaction container 11 and the second reaction container 12 is opened so that the carbon material saturated with silane gas can enter the second reaction container 12 through a pipeline based on its own gravity. The carbon material saturated with silane gas undergoes a silane dehydrogenation cracking reaction in the second reaction container 12 so that the silane in the carbon material saturated with silane gas is cracked into nano-silicon and deposited in the pores of the carbon carrier to obtain a first intermediate product. The valve between the second reaction container 12 and the third reaction container 13 is opened so that the first intermediate product can enter the third reaction container 13 through a pipeline based on its own gravity. After the first intermediate product is cooled in the third reaction container 13, a silicon-carbon composite material with cracked and deposited nano-silicon is obtained. The silicon content in the silicon-carbon composite material of cracked and deposited nano-silicon is detected. If the silicon content does not reach 45-60%, the valve of the pipeline between the third reaction container 13 and the first reaction container 11 is opened to allow the silicon-carbon composite material of cracked and deposited nano-silicon to enter the first reaction container 11 through the pipeline, and the above steps are repeated until the silicon content in the silicon-carbon composite material of cracked and deposited nano-silicon in the third reaction container 13 reaches 45-60%.

[0055] According to the above, the valve of the pipeline between the third reaction container 13 and the fourth reaction container 14 is opened, so that the silicon-carbon composite material of cracked and deposited nano-silicon with the required silicon content enters the fourth reaction container 14 through the pipeline under the protection of nitrogen. The carbon source gas is introduced into the fourth reaction container 14 to carbon-coat the silicon-carbon composite material of cracked and deposited nano-silicon to obtain the second intermediate product. Subsequently, the valve between the fourth reaction container 14 and the fifth reaction container 15 is opened to allow the second intermediate product to enter the fifth reaction container 15 through the pipeline, and the second intermediate product is cooled in the fifth reaction container 15 to obtain the silicon-carbon negative electrode material.

[0056] In the embodiment of the present invention, the carbon carrier is saturatedly adsorbed in a vacuum environment in a first reaction vessel, thereby avoiding the need to introduce a large amount of nitrogen as a carrier gas in the mainstream process of using a fluidized bed, saving costs and, more importantly, achieving sufficient filling of the pores of the carbon carrier with silane gas; the carbon material saturated with silane gas is then placed in a second reaction vessel for pyrolysis and deposition treatment. Since the adsorption process and the pyrolysis and deposition process are carried out in two reaction vessels, the problem of poor process stability caused by the currently commonly used adsorption treatment and pyrolysis and deposition treatment in the same fluidized bed body is avoided, thereby greatly reducing the complexity of the existing process, and achieving effective control of the silane adsorption and deposition amounts in a circulating manner, thereby avoiding the problem of "floating silicon" on the surface of the carbon carrier, and significantly improving the stability of the process.

[0057] In order to better illustrate the advantages of the embodiments of the present invention, the silicon-carbon negative electrode material prepared by the above method of the present invention was tested for performance. The test methods used in the following experimental examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0058] Control group: Silicon-carbon negative electrode material prepared by the production device and preparation method of silicon-carbon negative electrode material of the prior art. Specifically, the production device is a fluidized bed reaction unit. The carbon material is first transported to the fluidized bed reaction unit. After the oxygen content in the fluidized bed reaction unit is less than 20ppm, the temperature is raised to 480-600°C, and a large amount of nitrogen is introduced as a carrier gas. Monosilane is used as a silicon source to make the monosilane effectively contact with the heated carbon material. When the silicon loading reaches 48-55%, stop the introduction of silane, continue to adjust the temperature to 500-750°C, and after keeping warm for a period of time, use nitrogen as a carrier gas and acetylene as an organic carbon source for carbon coating treatment. After completion, the material inside the fluidized bed is pressurized with nitrogen to transport the high-temperature material to the cooling tank for the cold zone to obtain the silicon-carbon negative electrode material.

[0059] 1. Experimental subjects: The silicon-carbon negative electrode materials prepared by the method for continuously preparing silicon-carbon negative electrode materials provided in the embodiment of the present invention formed an experimental group; control group: the silicon-carbon negative electrode materials prepared in the above control group.

[0060] 2. Experimental methods:

[0061] ① The experimental group and the control group were tested by SEM (scanning electron microscope). The obtained SEM images are shown in Figure 3a and 3b ,in Figure 3a The SEM image of the experimental group. Figure 3b It is the SEM picture of the control group.

[0062] ② Assemble the experimental group and the control group into button cells and test the battery performance. Specifically include the following steps: the battery is assembled in a German Braun glove box filled with argon, the battery model is 2430, the electrolyte is 1M LiPF6 (volume ratio EC:DEC:DMC=1:1:1), and the metal lithium sheet is used as the counter electrode (positive electrode). The half-cell is tested for rate charging capacity at 0.5C, 2C, and 5C in the Land test system, and the capacity retention rate is tested for 50 cycles of charge and discharge at 0.5C. Test of pole piece expansion rate: pole piece expansion rate (%) = (pole piece thickness after 100 cycles - pole piece thickness before assembly) / (pole piece thickness before assembly - copper foil thickness) * 100%. See the test results. Figure 4 , Figure 4 The blue line is the test result of the experimental group, and the red line is the test result of the control group.

[0063] Conclusion: Comparison Figure 3a and Figure 3b It can be seen that the silicon-carbon negative electrode material (experimental group) prepared in the embodiment of the present invention has less "floating silicon" on the surface than the control group. Figure 4 It can be seen that the battery prepared with the silicon-carbon negative electrode material (experimental group) prepared in the embodiment of the present invention has better cycle performance and smaller battery cell expansion than the battery prepared in the control group.

[0064] To summarize, the embodiment of the present invention performs saturated adsorption on the carbon carrier in a vacuum environment in the first reaction vessel, thereby avoiding the introduction of a large amount of nitrogen gas and achieving sufficient filling of the pores of the carbon carrier with silane gas; the saturated adsorbed carbon carrier after saturated adsorption is then placed in the second reaction vessel for pyrolysis and deposition treatment. Since the adsorption process and the deposition process are carried out in two reaction vessels, the problem of poor process stability caused by the adsorption and pyrolysis and deposition treatments in the same fluidized bed body is avoided, thereby greatly reducing the complexity of the existing process, effectively avoiding the problem of "floating silicon" on the surface of the carbon carrier, and significantly improving the stability of the process.

[0065] On the other hand, an embodiment of the present invention further provides a silicon-carbon negative electrode material, which is prepared, for example, by the method for continuously preparing a silicon-carbon negative electrode material provided by an embodiment of the present invention.

[0066] On the other hand, the embodiment of the present invention further provides a lithium-ion battery, which includes, for example, an electrolyte, a separator, a lithium-ion battery positive electrode plate, and a lithium-ion battery negative electrode plate. The lithium-ion battery negative electrode plate includes, for example, a current collector and an active layer coated on the current collector, the active layer includes a silicon-carbon negative electrode material prepared by the method for continuously preparing a silicon-carbon negative electrode material provided by the embodiment of the present invention, and the active layer also includes a conductive agent and an adhesive.

[0067] It can be understood that the aforementioned embodiments are merely exemplary descriptions of the present invention. The technical solutions of the various embodiments can be arbitrarily combined and used in combination, provided that the technical features do not conflict, the structures do not contradict, and the purpose of the present invention is not violated.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for continuously preparing a silicon-carbon negative electrode material, characterized in that: include: Adsorption step: placing the carbon carrier in a first reaction container, and introducing silane gas into the first reaction container under a vacuum environment to obtain a carbon material saturated with silane gas; Deposition step: placing the carbon material saturated with silane gas into a second reaction container and performing pyrolysis deposition treatment, and obtaining a silicon-carbon composite material with cracked and deposited nano-silicon after cooling; Coating step: heating the silicon-carbon composite material of cracked and deposited nano-silicon under the protection of an inert atmosphere, coating the surface of the silicon-carbon composite material of cracked and deposited nano-silicon with a carbon source gas to form a coating layer, and obtaining the silicon-carbon negative electrode material after cooling.

2. The method for continuously preparing silicon-carbon negative electrode material according to claim 1, characterized in that: After the deposition step and before the coating step, the method further comprises the following steps: Determining whether the silicon content in the cracked and deposited nano-silicon silicon-carbon composite material reaches a first predetermined content; If reached, the coating step is performed; If not, repeat the adsorption step and the deposition step until the silicon content in the silicon-carbon composite material of the cracked and deposited nano-silicon reaches the first predetermined content.

3. The method for continuously preparing silicon-carbon negative electrode material according to claim 2, characterized in that: The first predetermined content is 45-60%.

4. The method for continuously preparing silicon-carbon negative electrode material according to claim 2, characterized in that: The step of placing the carbon carrier in a first reaction container and introducing silane gas into the first reaction container under a vacuum environment to obtain a carbon material saturated with silane gas specifically includes: Using nitrogen as carrier gas, the carbon carrier is placed into the first reaction container; The first reaction container is evacuated to a first vacuum degree and then nitrogen is introduced to a first pressure; Determining whether the oxygen content in the first reaction container reaches a second predetermined content; If the pressure is reached, the first reaction container is evacuated to a second vacuum degree and then the silane gas is introduced to the first pressure.

5. The method for continuously preparing silicon-carbon negative electrode material according to claim 4, characterized in that: The first vacuum degree is less than or equal to 100Pa, the second vacuum degree is less than or equal to 10Pa, and the first pressure is 10 5 Pa, the second predetermined content is 20ppm.

6. The method for continuously preparing silicon-carbon negative electrode material according to claim 2, characterized in that: The step of placing the carbon material saturated with silane gas into a second reaction container and performing pyrolysis deposition treatment to obtain a silicon-carbon composite material with cracked and deposited nano-silicon after cooling specifically comprises: placing the carbon material saturated with silane gas into the second reaction container and continuously stirring at a temperature of 480-600° C. to obtain a first intermediate product, wherein the oxygen content in the second reaction container is less than 20 ppm; The first intermediate product is placed in a third reaction container, and after cooling to 360° C., the silicon-carbon composite material of cracked and deposited nano-silicon is obtained, and the oxygen content in the third reaction container is less than 20 ppm.

7. The method for continuously preparing silicon-carbon negative electrode materials according to claim 2, characterized in that: The method comprises heating the silicon-carbon composite material of cracked and deposited nano-silicon under the protection of an inert atmosphere, coating the surface of the silicon-carbon composite material of cracked and deposited nano-silicon with a carbon source gas to form a coating layer, and obtaining the silicon-carbon negative electrode material after cooling, specifically: Under the protection of the inert atmosphere, the silicon-carbon composite material of the cracked and deposited nano-silicon is placed in a fourth reaction container and heated at a temperature of 500-750° C., and the carbon source gas is introduced into the fourth reaction container to obtain a second intermediate product; wherein the inert atmosphere is nitrogen, the carbon source gas is one or more of acetylene, propylene, and methane, and the oxygen content in the fourth reaction container is less than 20 ppm; The second intermediate product is placed in a fifth reaction container and cooled to 50° C. to obtain the silicon-carbon negative electrode material, wherein the oxygen content in the fifth reaction container is less than 20 ppm.

8. The method for continuously preparing silicon-carbon negative electrode materials according to any one of claims 1 to 7, characterized in that: The carbon carrier is a porous carbon material. The first reaction container is connected to the second reaction container through a pipeline. A valve is provided at the connection between the first reaction container and the pipeline. The valve is used to control the connection and closing between the first reaction container and the second reaction container.

9. A silicon-carbon negative electrode material, characterized in that: The silicon-carbon negative electrode material is prepared by the method for continuously preparing the silicon-carbon negative electrode material according to any one of claims 1 to 8.

10. A battery, characterized in that: It comprises a negative electrode plate for a lithium-ion battery, wherein the negative electrode plate for the lithium-ion battery comprises a current collector and an active layer coated on the current collector, wherein the active layer comprises a silicon-carbon negative electrode material prepared by the method for continuously preparing a silicon-carbon negative electrode material according to any one of claims 1 to 8.

Citation Information

Cited By

  • System and process method capable of continuously preparing high-gram-volume and low-expansion silicon-carbon material

    CN120054376A

  • Nano-silicon-doped porous carbon for silicon-carbon negative electrode, preparation method of nano-silicon-doped porous carbon, silicon-carbon negative electrode material and battery

    CN121180972A