Preparation method of catalyst for realizing metal self-reduction and uniform dispersion by using carbon-containing molecule modified inert carrier

The low-carbon molecular gas mixture treatment carrier forms reducing groups, and achieve uniform dispersion and reduction of metal particles under mild conditions, solving the danger and complexity of high-temperature hydrogenation and liquid phase reduction methods in the prior art. Improves the performance and preparation efficiency of the catalyst.

CN119056430APending Publication Date: 2024-12-03QUZHOU INSTITUTE FOR INNOVATION IN RESOURCE CHEMICAL ENGINEERING +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411230652.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the preparation of existing supported metal catalysts, high-temperature hydrogenation reduction and liquid phase reduction methods have problems such as hazards, difficulty in removing protective agents and inhibiting catalytic activity, and the addition of reducing agents is required, resulting in complex preparation process and high cost.

Method used

The carrier is pretreated with low-carbon molecular mixture to form a group with reducing properties. The uniform dispersion and reduction of metal particles is achieved under mild conditions by impregnation method, and the loading and reduction process are completed simultaneously.

Benefits of technology

The catalyst preparation process is simplified, production costs are reduced, the risk of high-temperature hydrogenation and protective agent residue problems are avoided, the overall performance of the catalyst is improved, and the uniform dispersion and efficient reduction of metal particles are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005026010740000011
    Figure HDA0005026010740000011
  • Figure HDA0005026010740000012
    Figure HDA0005026010740000012
  • Figure HDA0005026010740000021
    Figure HDA0005026010740000021
Patent Text Reader

Abstract

The invention provides a preparation method of a catalyst for realizing metal self-reduction and uniform dispersion by using a carbon-containing molecule modified inert carrier. The preparation method of the active carrier with the reduction function and the catalyst comprises the following steps: (1) placing an inert carrier in a reactor, carrying out a contact reaction on a carbon molecule-containing mixed gas and the inert carrier at 150-450 DEG C, controlling the gas flow to be 10-100 mL / min and the reaction time to be 1-10 h, cooling to room temperature after the reaction is finished, taking out a sample, collecting the sample with a vacuum packaging bag, and carrying out sealed storage, and (2) loading metal through an impregnation method, and performing in-situ reduction on the metal in the loading process to obtain the noble metal catalyst. According to the technology for preparing the active carrier with the reduction function by using the carbon-containing molecule modified inert carrier, in-situ reduction of the noble metal on the carrier can be accurately controlled and uniform dispersion can be realized in the process of impregnating and loading the noble metal, so that a high-energy-consumption and dangerous traditional unit operation process of firstly loading and then carrying out hydrogenation reduction is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalyst preparation, and in particular to the preparation of an active carrier with a reducing function and a simple preparation technology of a uniformly dispersed noble metal catalyst. Background Art

[0002] Catalytic materials play a key role in improving reaction efficiency, achieving efficient resource utilization and environmental protection, and are widely used in 90% of chemical processes. Among them, supported metal catalysts account for more than 70% of the use due to their easy separation and recyclability. In particular, precious metal catalysts are highly valued for their excellent activity, selectivity and stability. They are widely used in hydrogenation, dehydrogenation, oxidation, reduction, isomerization, aromatization, cracking, synthesis and other reactions, and play a very important role in the fields of chemical industry, petroleum refining, petrochemicals, medicine, environmental protection and new energy.

[0003] The preparation process of supported metal catalysts often requires loading and reduction processes. As a key step in the preparation of metal catalysts, the use of reducing agents is indispensable. Currently, the reduction process is mainly carried out by high-temperature hydrogenation or by adding liquid reducing agents (such as NaBH 4 ) and protective agent for reduction. However, there are certain disadvantages. For example, in patent CN104399537A, Pd / Al 2 O 3 The catalyst also needs to be reduced in a hydrogen atmosphere at 200°C for 3 to 50 hours; as in patent CN 117531503A, Pd / Al is obtained by liquid phase reduction 2 O 3 The catalyst needs to be calcined at 400-500℃ for 2h to remove the protective agent. This will inevitably face the problems of the danger of high-temperature hydrogenation process, the difficulty of removing the protective agent, the inhibition of catalytic activity by the residual protective agent, and the thermodynamic instability of the metal.

[0004] The supported catalyst is mainly composed of a carrier and an active metal. Common carriers include alumina, zeolite molecular sieves, activated carbon, hydrotalcite, etc. The carrier is an important component of the catalyst, but its main function is only to stabilize the active components and provide suitable mechanical strength and mass transfer diffusion channels. If the carrier material can be designed or modified to give it a reduction function, so that it can directly reduce the active metal without adding a reducing agent and achieve uniform dispersion, it can not only simplify the catalyst preparation process and reduce production costs, but also effectively avoid the problems caused by traditional reduction methods and improve the overall performance of the catalyst. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing an active carrier with a reducing function by treating the carrier with a low-carbon molecular mixed gas.

[0006] The present invention provides a method for preparing an active carrier with a reducing function using a carbon-containing gas, which is to pretreat the carrier with a low-carbon molecular mixed gas. During the treatment process, the low-carbon mixed gas can promote the change of the metal-oxygen structure on the surface of the carrier to form defects. Subsequently, the low-carbon gas molecules enter the defects and combine with oxygen to form a reducing group. When the active carrier with a reducing group is used to prepare a supported metal catalyst by an impregnation method, the reducing group on the surface of the active carrier can directly reduce the active metal precursor and induce it to fall into place, effectively maintaining the uniform dispersion of metal particles, and realizing the simultaneous completion of loading and reduction. The invention can achieve uniformly dispersed self-reduction of metals under mild conditions without the addition of a reducing agent, effectively simplifying the preparation process and improving the performance of the catalyst.

[0007] The method for preparing an active carrier with a reducing function using a low-carbon molecular mixed gas comprises the following specific steps:

[0008] A: Place the carrier in a reactor and seal it. First, allow the protective gas to enter the reactor through a deoxygenator, then pass the N gas through the deoxygenator and then pass it into the reactor after deoxygenation. Use a mass flow meter to control the flow rates of the N gas and the protective gas to adjust the ratio of the reaction gas. After the reaction gas is passed for 15-30 minutes, the reactor is heated by a programmed temperature increase, the heating rate is 2-20°C / min, the reaction temperature is 150-450°C, the reaction time is 1-10h, preferably 2-6h; the reaction gas flow rate is 10mL / min-100mL / min, preferably 10mL / min-60mL / min; after the reaction is completed, cool to room temperature, quickly take out the sample and vacuum pack it for standby use to obtain a reducing active carrier.

[0009] The reaction gas is composed of carbon-containing gas N and protective gas, wherein the volume content of N is 5%-60% and the rest is protective gas, and the preferred volume content of N is 10%-40%.

[0010] The protective gas is an inert gas, such as nitrogen or helium.

[0011] The deoxidizing device is a drying tube to which 401 manganese-based deoxidizer is added.

[0012] The N is CH 4 , C 2 H 2 ,CO,CO 2 , C 2 H 4 , C 2 H 6 One or more of. Preferably CH 4 , C 2 H 2 ,CO,CO2 , C 2 H 4 , C 2 H 6 Any 1 to 3 of the following.

[0013] The oxygen-containing carrier is one of molecular sieve, magnesium aluminum hydrotalcite and magnesium oxide.

[0014] In the above reaction process, the low-carbon molecular mixed gas in the low-carbon molecular mixed gas is adsorbed on the surface of the carrier to induce the change of its metal-oxygen bonding structure and generate defects. Subsequently, the low-carbon gas molecules enter the defects and combine with oxygen to form reducing groups.

[0015] B: mixing the active support of step A with a metal precursor impregnation solution, wherein the concentration of the metal precursor impregnation solution is determined according to the content of active metal required for the final product;

[0016] For the powdered active carrier, add the mixture of the powdered active carrier and the metal precursor solution into a beaker, place it in a water bath, add a magnetic bar for stirring, and the rotation speed is 100-1000 rpm. When the solution is almost dry, put it into an oven to dry, and finally obtain a powdered supported catalyst.

[0017] For the formed active carrier, a mixture of the formed active carrier and the metal precursor solution is evenly mixed in a sample tube, and placed in an oven for drying at a temperature of 20-90° C. for 6-36 hours to finally obtain a formed supported catalyst.

[0018] During the impregnation process, the metal cations gradually approach the surface of the carrier and migrate to the vicinity of the reducing groups due to charge interactions. The reducing groups give electrons to the metal cations, thereby reducing the metal cations to form metal atoms, and finally obtaining the reduced precious metal catalyst, achieving the simultaneous completion of loading and reduction.

[0019] The above-mentioned device used for preparing the active carrier with reduction function is mainly composed of the following parts: multiple (the number is n, depending on the number of types of N gas selected, and the value range of n is 1 to 5) N gas storage tanks, a protective gas storage tank, a deoxygenation device, a reactor, and a tail gas collection bottle. Among them, the N gas storage tank and the protective gas storage tank are connected to the deoxygenation device through a mass flow meter. The deoxygenation device is then connected to the reactor through a gas path. The air inlet and outlet of the reactor are both provided with pressure gauges to monitor the gas pressure. In addition, a waste gas collection container is also connected to the bottom of the reactor to collect the waste gas generated during the reaction.

[0020] The prepared catalyst was characterized and the results are as follows:

[0021] Depend on Figure 2There is no obvious Pd particle peak in the XRD pattern, indicating that Pd is dispersed more evenly.

[0022] Depend on Figure 3 , 4 From the XPS spectra of and 5, it can be seen that Ru, Pd and Au have been reduced.

[0023] Depend on Figure 6 HRTEM shows that Pd is well dispersed and relatively uniform.

[0024] Depend on Figure 7 HRTEM shows that Pt is well dispersed and relatively uniform.

[0025] Depend on Figure 8 The CO-DRIFTS indicates that Ir is well dispersed and relatively uniform.

[0026] Depend on Fig. 9 From the performance comparison, it can be seen that the Pd / ZSM-48 molecular sieve catalyst prepared by this method has a certain improvement in the acetylene semi-hydrogenation performance.

[0027] Depend on Fig.10 From the performance comparison, it can be seen that the Ru / MgO catalyst prepared by this method has a certain improvement in the performance of carbon dioxide hydrogenation.

[0028] Beneficial effects:

[0029] The characteristics of this preparation method are: using low-carbon molecular mixed gas to specially treat the oxygen-containing carrier to obtain a series of active carriers with special reduction functions. The characteristics of this type of active carrier are: it can achieve the simultaneous completion of active metal loading and reduction under mild conditions when loading metal salts. This in-situ reduction process is completely different from the technology of reduction after loading, avoiding the traditional operation process of high-temperature hydrogenation, which is dangerous and energy-intensive, and has brought a series of revolutionary improvements to the loaded metal catalyst. In addition, this method has good universality for carriers, and has good effects on carriers such as molecular sieves, hydrotalcites, and magnesium oxide. It can be widely used in various fields of chemical production, has broad market promotion prospects, and is expected to promote the green and efficient development of the chemical industry.

[0030] The provided device for preparing an active carrier with a reducing function can control the proportion of the reaction gas by adjusting the proportion of the flow meter. The gas enters the reactor through the gas path and fully contacts the sample. The reaction gas is finally collected by a gas collection device for repeated use.

[0031] The catalytic performance of the catalyst prepared by the method was tested in the acetylene semi-hydrogenation reaction and the carbon dioxide hydrogenation reaction. Compared with the catalyst reduced by the traditional method, the catalytic performance of the catalyst prepared by the present invention was improved to a certain extent. This finding further confirms the superiority and practicality of the preparation method of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The invention relates to a device for preparing an active carrier with reducing function.

[0033] Figure 2 This is the XRD spectrum of the ZSM-48 support prepared in Examples 2 and 3.

[0034] Figure 3 This is the Pd3d XPS spectrum of Pd-loaded magnesium oxide in Example 6.

[0035] Figure 4 This is the Ru3p XPS spectrum of the Ru-loaded magnesium oxide in Example 4.

[0036] Figure 5 This is the Au4f XPS spectrum of Au-loaded ZSM-48 in Example 2.

[0037] Figure 6 This is the HRTEM image of Pd-loaded ZSM-48 in Example 5.

[0038] Figure 7 This is the HRTEM image of Pt-loaded ZSM-48 in Example 3.

[0039] Figure 8 This is the CO-DRIFTS spectrum of Ir-loaded magnesium oxide in Example 7.

[0040] Fig. 9 The catalytic performance of acetylene semi-hydrogenation of the Pd / ZSM-48 molecular sieve catalyst prepared in Example 5 is compared with that of the Pd / ZSM-48 molecular sieve catalyst prepared by conventional hydrogenation reduction.

[0041] Fig.10 The carbon dioxide hydrogenation performance of the Ru / MgO catalyst prepared in Example 4 is compared with that of the Ru / MgO catalyst prepared by conventional hydrogenation reduction. DETAILED DESCRIPTION

[0042] In the following examples, the gas percentages are by volume.

[0043] Example 1

[0044] A. Weigh 10g of powdered magnesium aluminum hydrotalcite sample and place it in the reactor. Tighten the device, introduce protective gas into the reactor, and check the air tightness of the device. Select methane and acetylene as N2 gas, pass it through the deoxygenation device and enter the reactor. The flow rate ratio of methane, acetylene and protective gas is controlled by the mass flow meter to be 4:7:9, so that the gas ratio flowing through the reactor is 20% CH 4 / 35%C 2 H 2 / 45%N 2 (protective gas). The temperature was raised to 150°C at a heating rate of 5°C / min by programmed heating, the gas flow rate was adjusted to 15mL / min, and the reaction time was 3h. After the reaction was completed, the sample was cooled to room temperature and quickly taken out to obtain an active magnesium-aluminum hydrotalcite carrier with reducing properties, which was vacuum packed for standby use. The deoxidation device uses a 401 manganese-based deoxidizer for deoxidation.

[0045] B. Weigh 2 g of the product in step A and place it in a 100 mL beaker, add 10 mL of ruthenium chloride solution with a mass concentration of 8.2 g / L, and place it in a 40°C water bath. Adjust the magnetic speed to 500 r / min. After the water in the beaker is quickly dried, place the sample in an oven at 80°C to dry, and obtain a magnesium-aluminum hydrotalcite catalyst loaded with Ru with a metal mass percentage of 2%.

[0046] Example 2

[0047] A. Weigh 5g of strip-shaped ZSM-48 molecular sieve sample and place it in the reactor, tighten the device. Deoxygenate the protective gas and then pass it into the reactor, and check the air tightness of the device. Select acetylene and methane as N gas, pass it through the deoxygenation device and enter the reactor. Use a mass flow meter to control the flow rate ratio of acetylene, methane and protective gas to be 1:4:5, so that the gas ratio flowing through the reactor is 10%C 2 H 2 / 40%CH 4 / 50%N 2 (protective gas). The temperature was raised to 250°C at a rate of 10°C / min by programmed heating, the gas flow rate was adjusted to 25mL / min, and the reaction time was 2h. After the reaction was completed, the sample was cooled to room temperature and quickly taken out to obtain a reducing active molecular sieve carrier, which was vacuum packed for standby use. The deoxidation device uses a 401 manganese-based deoxidizer for deoxidation.

[0048] B. Weigh 2 g of the product in step A and place it in a 50 mL sample tube, add 10 mL of sodium chloroaurate solution with a mass concentration of 3.46 g / L, and after ultrasonication for 5 minutes, immerse the sample in an oven at 80°C for 16 hours to obtain a molecular sieve catalyst loaded with Au with a metal mass percentage of 1%.

[0049] Example 3

[0050] A. Weigh 10g of strip-shaped ZSM-48 molecular sieve sample and place it in the reactor, tighten the device. Deoxygenate the protective gas and then pass it into the reactor, and check the air tightness of the device. Select methane and carbon monoxide as N gas, pass it through the deoxygenation device and enter the reactor. The flow rate ratio of methane, carbon monoxide and protective gas is controlled by a mass flow meter to be 2:3:5, so that the gas ratio flowing through the reactor is 20% CH 4 / 30%CO / 50%N 2 (protective gas). The temperature was raised to 300°C at a heating rate of 5°C / min by programmed heating, the gas flow rate was adjusted to 20mL / min, and the reaction time was 2h. After the reaction was completed, the sample was cooled to room temperature and quickly taken out to obtain a reducing active molecular sieve carrier, which was vacuum packed for standby use. The deoxidation device uses a 401 manganese-based deoxidizer for deoxidation.

[0051] B. Weigh 2 g of the product in step A and place it in a 50 mL sample tube, add 10 mL of 4.2 g / L chloroplatinic acid solution, and after ultrasonication for 5 minutes, immerse the sample in an oven at 80°C for 16 hours to obtain a Pt-loaded molecular sieve catalyst with a metal mass percentage of 1%.

[0052] Example 4

[0053] A. Weigh 10g of powdered magnesium oxide sample and place it in the reactor. Tighten the device, introduce protective gas into the reactor, and check the air tightness of the device. Select ethane and acetylene as N2 gas, pass them through the deoxygenation device and enter the reactor. The flow rate ratio of ethane, acetylene and protective gas is controlled by the mass flow meter to be 7:4:9, so that the gas ratio flowing through the reactor is 35%C. 2 H 6 / 20%C 2 H 2 / 45%N 2 (protective gas). The temperature was raised to 250°C at a heating rate of 5°C / min by programmed heating, the gas flow rate was adjusted to 35mL / min, and the reaction time was 2h. After the reaction was completed, the sample was cooled to room temperature and quickly taken out to obtain a reducing active magnesium oxide carrier, which was vacuum packed for standby use. The deoxidation device uses a 401 manganese-based deoxidizer for deoxidation.

[0054] B. Weigh 2 g of the product in step A and place it in a 100 mL beaker, add 10 mL of 4.1 g / L ruthenium chloride solution, and place it in an 80°C water bath. Adjust the magnetic speed to 400 r / min. After the water in the beaker is quickly dried, place the sample in an 80°C oven to dry, and a magnesium oxide catalyst loaded with Ru with a metal mass percentage of 1% is obtained.

[0055] Example 5

[0056] A. Weigh 15g of strip-shaped ZSM-48 molecular sieve sample and place it in the reactor, tighten the device. Deoxygenate the protective gas and then pass it into the reactor, and check the air tightness of the device. Select methane and carbon monoxide as N gas, pass it through the deoxygenation device and enter the reactor. The mass flow meter controls the flow rate ratio of methane, carbon monoxide and protective gas to 4:1:5, so that the gas ratio flowing through the reactor is 40% CH 4 / 10%CO / 50%N 2 (protective gas). The temperature was raised to 200°C at a rate of 10°C / min by programmed heating, the gas flow rate was adjusted to 20mL / min, and the reaction time was 2h. After the reaction was completed, the sample was cooled to room temperature, and the sample was quickly taken out to obtain a reducing active molecular sieve carrier, which was vacuum packed for standby use. The deoxidation device uses 401 manganese-based deoxidizer for deoxidation.

[0057] B. Weigh 2 g of the product in step A and place it in a 50 mL sample tube, add 10 mL of sodium chloropalladate solution with a mass concentration of 5.52 g / L, and after ultrasonication for 5 minutes, immerse the sample in an oven at 80°C for 16 hours to obtain a molecular sieve catalyst loaded with Pd with a metal mass percentage of 1%.

[0058] Example 6

[0059] A. Weigh 15g of powdered magnesium oxide sample and place it in the reactor. Tighten the device, introduce protective gas into the reactor, and check the air tightness of the device. Select methane and ethane as N gas, pass them through the deoxygenation device and enter the reactor. The flow rate ratio of methane, acetylene and protective gas is controlled by the mass flow meter to be 1:1:3, so that the gas ratio flowing through the reactor is 20% CH 4 / 20%C 2 H 6 / 60%N 2 (protective gas). The temperature was raised to 200°C at a heating rate of 10°C / min by programmed heating, the gas flow rate was adjusted to 15mL / min, and the reaction time was 3h. After the reaction was completed, the sample was cooled to room temperature and quickly taken out to obtain a reducible active magnesium oxide carrier, which was vacuum packed for standby use. The deoxidation device uses a 401 manganese-based deoxidizer for deoxidation.

[0060] B. Weigh 2 g of the product in step A and place it in a 100 mL beaker, add 10 mL of sodium chloropalladate solution with a mass concentration of 11.04 g / L, and place it in a 60°C water bath. Adjust the magnetic speed to 500 r / min. After the water in the beaker is quickly dried, place the sample in a 70°C oven to dry, and obtain a magnesium oxide catalyst loaded with Pd with a metal mass percentage of 2%.

[0061] Example 7

[0062] A. Weigh 10g of powdered magnesium oxide sample and place it in the reactor. Tighten the device, introduce protective gas into the reactor, and check the air tightness of the device. Select methane and ethane as N gas, pass them through the deoxygenation device and enter the reactor. The flow rate ratio of methane, carbon monoxide and protective gas is controlled by the mass flow meter to be 1:3:6, so that the gas ratio flowing through the reactor is 10% CH 4 / 30%CO / 60%N 2 (protective gas). The temperature was raised to 250°C at a heating rate of 10°C / min by programmed heating, the gas flow rate was adjusted to 10mL / min, and the reaction time was 2h. After the reaction was completed, the sample was cooled to room temperature and quickly taken out to obtain a reducible active magnesium oxide carrier, which was vacuum packed for standby use. The deoxidation device uses a 401 manganese-based deoxidizer for deoxidation.

[0063] B. Weigh 2 g of the product in step A and place it in a 100 mL beaker, add 10 mL of 8.53 g / L chloroiridic acid solution into the 100 mL beaker, and place it in a 60°C water bath. Adjust the magnetic speed to 500 r / min. After the water in the beaker is quickly dried, place the sample in a 70°C oven to dry, and obtain an Ir-loaded magnesium oxide catalyst.

[0064] Comparative Example 1

[0065] The comparative sample was prepared according to the parameters of Example 5, except that the carbon-containing mixed gas treatment was not performed.

[0066] A. Weigh 15g of strip-shaped ZSM-48 molecular sieve sample and place it in a reactor. Pass protective gas into the reactor through a deoxygenator. Use programmed temperature heating to raise the temperature to 200°C at a heating rate of 10°C / min. Adjust the gas flow rate to 20mL / min and the reaction time to 2h. Obtain a ZSM-48 molecular sieve carrier.

[0067] B. Weigh 2 g of the product in step A and place it in a 50 mL sample tube. Add a sodium chloropalladate solution with a mass concentration of 5.52 g / L. After ultrasonication for 5 minutes, immerse the sample in an oven at 80°C for 16 hours to obtain a Pd-loaded molecular sieve.

[0068] C. Place the Pd-loaded ZSM-48 molecular sieve obtained in step B in a tube furnace, set the reaction temperature to 300°C, and heat under 10% H 2 / N 2 The catalyst was reduced under an atmosphere of 3 h to obtain a Pd / molecular sieve catalyst with a metal mass percentage of 1%.

[0069] Comparative Example 2

[0070] The comparative sample was prepared according to the parameters of Example 4, except that the carbon-containing mixed gas treatment was not performed.

[0071] A. Weigh 15g of powdered magnesium oxide sample and place it in a reactor. Pass the protective gas into the reactor through the deoxygenation device. Use programmed temperature heating to raise the temperature to 250°C at a heating rate of 5°C / min. Adjust the gas flow rate to 35mL / min and the reaction time to 2h. Obtain a ZSM-48 molecular sieve carrier.

[0072] B. Weigh 2 g of the product in step A and place it in a 100 mL beaker. Add ruthenium chloride solution with a mass concentration of 4.1 g / L, and place it in an 80°C water bath. Adjust the magnetic speed to 400 r / min. After the water in the beaker is quickly dried, place the sample in an 80°C oven to dry, and Ru-loaded magnesium oxide is obtained.

[0073] C. Place the Ru-loaded magnesium oxide obtained in step B in a tube furnace, set the reaction temperature to 300°C, and heat under 10% H 2 / N 2 The catalyst was reduced under an atmosphere of for 3 h to obtain a Ru / magnesium oxide catalyst with a metal mass percentage of 1%.

[0074] Application Example 1

[0075] The catalysts prepared in Example 5 and Comparative Example 1 were respectively used in the acetylene semi-hydrogenation reaction experiment:

[0076] Weigh 0.2g of catalyst and put it into a quartz reaction tube with a diameter of 10mm. The catalytic performance test temperature is 50-150℃, and the gas composition in the reaction raw gas is 0.71%C 2 H 2 / 2.86%H 2 / 70.72%C 2 H 4 / 25.71%N 2 (Balance gas). Test pressure is 1 bar, air speed is 3800h -1 The composition and content of reactants and products were analyzed by gas chromatography, and the data processing method was normalization. To ensure the accuracy of the test, the results were recorded after reaching the specified temperature and maintaining it for 30 minutes. The test was carried out for 3 groups, and the average value was the catalytic performance data at the catalytic temperature. The results are shown in Figure 8 .

[0077] Depend on Figure 8 It can be seen that compared with the Pd / ZSM-45 zeolite catalyst prepared by the traditional method, the Pd / ZSM-45 zeolite catalyst prepared by the in-situ self-reduction method of impregnation has better hydrogenation activity in the low temperature zone.

[0078] Application Example 2

[0079] The catalysts prepared in Example 4 and Comparative Example 2 were respectively used in the carbon dioxide hydrogenation reaction experiment:

[0080] Weigh 0.1g of catalyst and mix it with 1.9g of quartz sand with a particle size of 40-70 mesh. Put the catalyst mixture into a quartz reaction tube with a diameter of 10mm. The catalytic performance test temperature is 50-550℃, and the gas composition in the reaction raw gas is 3% CO 2 / 9%H 2 / 87%N 2 (Balance gas). Test pressure is 1 bar, air velocity is 54000h -1 The composition and content of reactants and products were analyzed by gas chromatography, and the data processing method was normalization. To ensure the accuracy of the test, the results were recorded after reaching the specified temperature and maintaining it for 30 minutes. The test was carried out for 3 groups, and the average value was the catalytic performance data at the catalytic temperature. The results are shown in Fig. 9 .

[0081] Depend on Fig. 9 It can be seen that compared with the Ru / MgO catalyst prepared by the traditional method, the Ru / MgO catalyst prepared by the in-situ self-reduction method of impregnation has higher activity and selectivity.

Claims

1. A method for preparing a catalyst for achieving metal self-reduction and uniform dispersion by modifying an inert carrier with carbon-containing molecules, characterized in that Prepare according to the following steps: A: Place an inert carrier in a reactor and seal it. First, allow the protective gas to enter the reactor through a deoxygenator, then pass the N gas through the deoxygenator and then pass it into the reactor after deoxygenation. Use a mass flow meter to control the flow rates of N gas and protective gas to adjust the ratio of the reaction gas. After the reaction gas is passed for 15-30 minutes, use a programmed temperature increase to heat the reactor. The heating rate is 2-20°C / min, the reaction temperature is 150-450°C, the reaction time is 1-10h, and the reaction gas flow rate is 10mL / min-100mL / min. After the reaction is completed, cool to room temperature, quickly take out the sample and vacuum pack it for standby use to obtain a reducing active carrier. The reaction gas is composed of carbon-containing gas N and protective gas, wherein the volume content of N is 5%-60% and the rest is protective gas; The protective gas is an inert gas, such as nitrogen or argon; The deoxidizing device is a drying tube to which a 401 manganese-based deoxidizer is added; The N is any one or more of CH4, C2H2, CO, CO2, C2H4, and C2H6; The inert carrier is any one of molecular sieve, magnesium aluminum hydrotalcite, graphene oxide, and magnesium oxide; In the above reaction process, the low-carbon molecular mixed gas in the low-carbon molecular mixed gas is adsorbed on the surface of the carrier to induce the change of its metal-oxygen bonding structure and generate defects. Subsequently, the low-carbon gas molecules enter the defects and combine with oxygen to form reducing groups. B: adding an equal volume of a metal precursor impregnation solution to the active support of step A, wherein the concentration of the metal precursor impregnation solution is determined according to the content of the active metal required for the final product; For the powdered active carrier, add the mixture of the powdered active carrier and the metal precursor solution into a beaker, place it in a water bath, add a magnetic bar for stirring, and the rotation speed is 100-1000 rpm. When the solution is almost dry, put it into an oven to dry, and finally obtain a powdered supported catalyst. For the formed active carrier, a mixture of the formed active carrier and the metal precursor solution is evenly mixed in a sample tube, and placed in an oven for drying at a temperature of 20-90° C. for 6-36 hours to finally obtain a formed supported catalyst. During the impregnation process, the metal cations gradually approach the surface of the carrier and migrate to the vicinity of the reducing groups due to charge interactions. The reducing groups give electrons to the metal cations, thereby reducing the metal cations to form metal atoms, and finally obtaining the reduced precious metal catalyst, achieving the simultaneous completion of loading and reduction.

2. The method for preparing a catalyst for achieving metal self-reduction and uniform dispersion by modifying an inert carrier with carbon-containing molecules according to claim 1, characterized in that: The programmed temperature process of step A has a reaction time of 2-6 hours and a reaction gas flow rate of 10 mL / min-60 mL / min; The volume content of N in the reaction gas is 10%-40%, and the rest is protective gas; The N is any one, two or three of CH4, C2H2, CO, CO2, C2H4, and C2H6.

Citation Information

Patent Citations

  • Supported bimetal nanocrystal catalyst and preparation method thereof

    CN103157469A

  • Porous carbon self-reduction preparation method of porous carbon loaded small-size precious metal nanoparticle composite material

    CN112705193A

  • Method and device for preparing alumina carrier and catalyst with reduction function by using carbon-containing mixed gas

    CN118105962A