Centrifugal casting method for eliminating shrinkage porosity defect of tin bronze alloy thick-wall casting
The centrifugal casting method addresses shrinkage defects in thick-walled tin-bronze alloy castings by adjusting solidification mode with a movable heating furnace and controlled pouring, achieving defect-free and efficient production.
Patent Information
- Application Number
- CN202310649982.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
Centrifugal casting of thick-walled tin-bronze alloy castings is prone to shrinkage defects, particularly band-shaped shrinkage, which affects the quality and increases machining requirements, leading to higher costs and reduced efficiency.
A centrifugal casting method involving a movable heating furnace that adjusts the solidification mode by heating the inner cavity of the casting, using a wide-diameter gate and controlled pouring speed, followed by machining to remove defects.
The method effectively eliminates band-shaped shrinkage defects, reduces slag inclusions, improves element segregation, and decreases material consumption while enhancing casting yield and reducing machining difficulty.
Smart Images

Figure CN119057033A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of centrifugal casting, in particular to a centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings. Background Art
[0002] Tin bronze alloy has the smallest casting shrinkage among non-ferrous metals, and has the advantages of corrosion resistance, wear resistance, good mechanical properties and processing performance. It is widely used in marine ship parts, wear-resistant parts, mining bearings and nuclear power sealing tiles.
[0003] Sealing bearings are one of the important components of hydrogen-cooled generators, and have high requirements for the airtightness of tin-bronze alloys. Compared with ordinary sand casting and metal mold casting, the centrifugal casting process for producing cylindrical bearings has simple equipment, high production efficiency, and the resulting casting microstructure is also denser.
[0004] Centrifugal casting is a technique and method of injecting liquid metal into a high-speed rotating mold, so that the molten metal performs centrifugal motion to fill the mold and form a casting. Centrifugal casting equipment is simple, with high production efficiency, low metal consumption, dense casting structure and good mechanical properties. However, the sealing shoe casting is a thick ring-shaped casting (thickness is more than 100mm). During the centrifugal casting process, the increase in the mold wall thickness or the water cooling method has extremely limited cooling capacity for the casting. In addition, the crystallization temperature range of tin bronze alloy is relatively wide, and the bidirectional solidification + paste solidification method makes it very easy for banded shrinkage to occur inside the casting, and shrinkage and slag inclusions often occur together, which seriously affects the quality of the casting. Summary of the invention
[0005] The purpose of the present invention is to provide a centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings, so as to solve the band-shaped shrinkage defects of thick annular castings such as sealing tiles, improve the quality of castings, reduce machining removal rate, and reduce costs and increase efficiency.
[0006] The technical solution of the present invention is as follows:
[0007] A centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings comprises the following steps: 1) the thickness of the casting mold is more than 1.5 times the thickness of the casting; 2) a wide-diameter gate is used for centrifugal pouring to ensure that the alloy liquid is uniform and continuous during the centrifugal process; 3) after the alloy liquid is poured, the pouring system is immediately taken out, and a heating device is placed in the centrifugal casting mold to heat the inner cavity; 4) the heating device is taken out, and the centrifugal operation is stopped after the casting is cooled and formed; 5) after demoulding, the inner surface of the annular casting is machined to remove surface casting defects.
[0008] In the centrifugal casting method for eliminating shrinkage defects of thick-walled tin bronze alloy castings, in step 2), the centrifuge speed is first determined according to the inner diameter of the casting, and then the alloy pouring speed is determined according to the speed and the size of the casting. The casting speed calculation formula is as follows:
[0009]
[0010] n——mold speed, r / min;
[0011] ρ——density of copper alloy, kg / m 3 ;
[0012] g——acceleration due to gravity, m / s 2 ;
[0013] r i ——Inner radius of annular casting, m;
[0014] The speed is adjusted within this range according to the different elements added to the copper alloy. The alloy pouring speed is proportional to the mold speed and the casting length, that is, the higher the mold speed, the longer the casting and the faster the pouring speed.
[0015] In the centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings, in step 3), the heating device is a movable heating furnace, including a central axis and a furnace shell, and the specific structure is as follows:
[0016] The central axis is placed horizontally and can move forward and backward in the horizontal direction. The main body is composed of a heating part and a supporting moving part coaxially connected by flanges; the heating part of the central axis is provided with a ceramic fiber thermal insulation module, a heating source, and a corundum tube I in sequence from the inside to the outside, and an insulating heat insulation disc is coaxially integrated at the front end of the heating part. The outer diameter of the insulating heat insulation disc is larger than the outer diameter of the corundum tube I, and a heat-resistant stainless steel sleeve is provided at the rear end of the heating part. A ceramic fiber thermal insulation disc is embedded in the heat-resistant stainless steel sleeve; the supporting moving part of the central axis is composed of a stainless steel tube embedded in a corundum tube and aluminum braided wire;
[0017] Center holes are provided at the front and rear ends of the furnace shell, and the center axis passes through the furnace shell in the horizontal direction. The front center hole of the furnace shell corresponds to the insulating heat-insulating disc and is in sliding fit, and the rear center hole of the furnace shell corresponds to the stainless steel pipe and is in sliding fit; the heat-resistant stainless steel sleeve corresponds to the rear center hole and inner wall of the furnace shell, and the thickness of the insulating heat-insulating disc is the same as that of the furnace shell; a hand-cranked gear is installed at the bottom of the center hole of the rear end outer wall of the furnace shell, and a transmission rack is installed at the bottom of the stainless steel pipe, and the hand-cranked gear corresponds to the transmission rack to form a gear rack transmission mechanism.
[0018] The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings is characterized in that a thermocouple is arranged on the heating part of the central axis, one end of the thermocouple is built into a ceramic fiber insulation disk embedded in a heat-resistant stainless steel sleeve, and the other end is located above the heating source; the heating source is a silicon-molybdenum rod or a silicon-carbon rod, and a threaded type or a straight rod type with uniform circumferential distribution is selected according to the heating power.
[0019] The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings comprises a stainless steel tube lined with a corundum tube II, a power input terminal clamp and an aluminum braided wire therein extend into the inner cavity of the corundum tube II, one end of the aluminum braided wire is connected to the power supply, and the other end of the aluminum braided wire passes through a flange and a central axis in sequence to be connected to a heating source.
[0020] The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings is characterized in that a connecting frame is installed at the bottom of the furnace body shell, and each connecting frame is an upper support frame and a lower support frame plug-in matching structure with upper and lower sections arranged vertically. The lower part of the upper support frame and the upper part of the lower support frame are respectively provided with more than two mounting holes for inserting knobs or bolts. The upper support frame and the lower support frame are connected and fixed at different positions by knobs or bolts to realize vertical movement of the furnace body shell to adjust the height of the furnace body shell; the lower end of each lower support frame is provided with a roller with a locking function, which supports the horizontal movement of the furnace body shell through the connecting frame.
[0021] The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings is as follows: when working, the front end of the furnace shell corresponds to the centrifuge casting mold, the centrifuge casting mold is composed of an annular casting mold sleeve, a disc-shaped casting mold pad and a disc-shaped casting mold cover with a center hole, the casting mold cover and the casting mold pad are arranged at the two ends of the annular casting mold sleeve relative to each other, the casting mold cover is located at one side opening of the centrifuge shell, and the casting mold pad is located at the inner wall of the other side of the centrifuge shell, and the centrifuge is surrounded by the casting mold cover, the annular casting mold sleeve, and the casting mold pad. The inner cavity of the centrifuge mold is filled with tin-bronze alloy melt in a ring shape under the action of centrifugal force after pouring; the front center hole of the furnace body shell is coaxial with the center hole of the mold cover, and the outer diameter of the insulating and heat-insulating disk is smaller than the diameter of the center hole of the mold cover; when in use, the furnace body shell is fixed, and the hand-cranked gear and the transmission rack are coordinated to make the stainless steel pipe drive the central axis and the heating source to extend from the inner cavity of the furnace body shell, and the central axis connected to the heating source is pushed forward, so that the heating source is placed in the inner cavity of the centrifuge mold.
[0022] In the centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings, the use of the heating device includes a preheating / slow cooling state and a working state, wherein: in the preheating / slow cooling state, the furnace shell is closed, the heating source is located in the furnace shell, and the heating source gradually heats up to a stable stage or gradually cools down; in the working state, the furnace shell is open, the central axis connected to the heating source is pushed forward, the heating source is placed in the inner cavity of the centrifuge casting, the air in the inner cavity of the centrifuge casting is heated by thermal radiation, and the heat is transferred to the casting in the centrifuge casting.
[0023] The centrifugal casting method for eliminating shrinkage defects of thick-walled tin bronze alloy castings requires that the temperature in the furnace be controlled to reach 800°C to 1100°C in the preheating state; in the working state, the temperature in the centrifuge casting cavity needs to be controlled at 800°C to 1100°C for 3 to 10 minutes, and the specific temperature and time are adjusted according to different alloys and different casting sizes.
[0024] In the centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings, in step 4), the casting is cooled and the molding temperature drops to 500°C±20°C and the machine is shut down. The removed heating device is continuously used for heating other centrifugal castings or slowly cooled to room temperature.
[0025] The design idea of the present invention is:
[0026] The present invention heats the inner cavity of the annular casting to change the solidification mode of the casting from bidirectional solidification from the inner surface and the outer surface to the center to sequential solidification from the outer surface to the inner surface, thereby adjusting the position of the loose area of the shrinkage cavity from the center of the thick wall to the inner surface ring, and finally removing it by machining, bringing the following beneficial effects 1, 2, and 4. The present invention controls the pouring speed and the speed of the centrifuge to ensure that the alloy liquid fills the mold smoothly and continuously, and the alloy elements do not aggregate due to the difference in specific gravity, bringing the following beneficial effects 2 and 3. The present invention can control the heating temperature and duration of the inner cavity of the casting through a matching movable heating furnace to ensure the change of the solidification mode, and bring the following beneficial effect 5.
[0027] The advantages and beneficial effects of the present invention are:
[0028] 1. The centrifugal casting method of the present invention can completely eliminate the band-shaped shrinkage defects inside the casting.
[0029] 2. The centrifugal casting method of the present invention can significantly reduce the slag inclusion defects inside the casting.
[0030] 3. The centrifugal casting method of the present invention can improve the element segregation defects of castings.
[0031] 4. The centrifugal casting method of the present invention can reduce the consumption of raw materials, reduce the difficulty of machining, and improve the casting yield rate.
[0032] 5. The movable heating furnace matched with the centrifugal casting method of the present invention has high utilization efficiency and wide application range, and is suitable for different copper alloys and horizontal centrifuges of different sizes. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1It is a schematic diagram of the heating device. In the figure, 1 is the central axis, 2 is the furnace shell, 10 is the insulating heat-insulating disc, 11 is the heating source, 12 is the corundum tube I, 13 is the ceramic fiber heat-insulating module, 14 is the thermocouple, 15 is the heat-resistant stainless steel sleeve embedded with the ceramic fiber heat-insulating disc, 16 is the flange, 17 is the stainless steel tube, 18 is the corundum tube II, 19 is the aluminum braided wire, 20 is the power input wiring clamp, 21 is the upper support frame, 22 is the lower support frame, 23 is the knob or bolt, 24 is the roller with locking function, 1a is the transmission rack, and 2a is the hand-cranked gear.
[0034] Figure 2 It is a schematic diagram of the heating state of the heating device. In the figure, 1 is a central axis, 2 is a furnace shell, 3 is a centrifuge mold, 4 is a tin bronze alloy melt, 31 is a mold cover, 32 is a mold sleeve, 33 is a mold pad, and 34 is a centrifuge shell.
[0035] Figure 3 The simulation results of the overall shrinkage defect of the casting are shown in Figure 1. (a) is a shrinkage defect of conventional centrifugal casting, and (b) is a shrinkage defect obtained by the centrifugal casting method provided by the present invention.
[0036] Figure 4 The simulation results of shrinkage defects on the center surface of the casting are shown in Figure 2. (a) is a shrinkage defect after conventional centrifugal casting, and (b) is a shrinkage defect obtained by the centrifugal casting method provided by the present invention. DETAILED DESCRIPTION
[0037] In a specific implementation process, the present invention proposes a centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings, comprising the following steps: 1) the thickness of the casting is more than 1.5 times the thickness of the casting, and the thickness of the casting can be adjusted by adding a casting mold sleeve; 2) a wide-diameter gate is used for centrifugal pouring to ensure that the alloy liquid is uniform and continuous during the centrifugal process, the position of the wide-diameter gate is the center position of the length direction of the casting, and the length of the wide-diameter gate is 1 / 2 of the length of the casting; 3) after the pouring of the alloy liquid is completed, the pouring system is immediately taken out, and a heating device is placed in the centrifuge casting cavity to heat it; 4) the heating device is taken out, and the casting is cooled and formed; 5) after demolding, the annular inner surface is machined and removed, and the inner wall of the obtained casting is rougher than the inner wall of the casting obtained by the conventional process, but the machining removal depth is correspondingly reduced.
[0038] In step 2), the centrifuge speed is first determined according to the inner diameter of the casting, and then the alloy pouring speed is determined according to the speed and the size of the casting. The mold speed is calculated using the following formula:
[0039]
[0040] n——mold speed, r / min;
[0041] ρ——density of copper alloy, kg / m 3 ;
[0042] g——acceleration due to gravity, m / s 2 ;
[0043] r i ——Inner radius of annular casting, m;
[0044] The speed can be adjusted within this range according to the different elements added to the copper alloy. For example, for high-lead tin copper, the speed can be appropriately reduced to improve the segregation of the lead element. The alloy pouring speed is proportional to the mold speed and the casting length, that is, the higher the mold speed, the longer the casting, and the faster the pouring speed.
[0045] like Figure 1-Figure 2 As shown, the heating device described in step 3) is a movable heating furnace, which mainly includes a central axis 1, a furnace shell 2, an insulating heat-insulating disc 10, a heating source 11, a corundum tube I 12, a ceramic fiber thermal insulation module 13, a thermocouple 14, a heat-resistant stainless steel sleeve embedded with a ceramic fiber thermal insulation disc 15, a flange 16, a stainless steel tube 17, a corundum tube II 18, an aluminum braided wire 19, a power input wiring clamp 20, an upper support frame 21, a lower support frame 22, a knob or bolt 23, a roller with a locking function 24, a transmission rack 1a, and a hand-cranked gear 2a. The specific structure is as follows:
[0046] The central shaft 1 is placed horizontally and can move forward and backward in the horizontal direction. The main body of the central shaft 1 is composed of a heating part and a supporting and moving part coaxially connected by a flange 16. The heating part of the central shaft 1 is provided with a ceramic fiber thermal insulation module 13, a heating source 11, and a corundum tube Ⅰ 12 from the inside to the outside. The front end of the heating part is coaxially provided with an insulating heat-insulating disc 10, and the rear end of the heating part is provided with a heat-resistant stainless steel sleeve embedded in a ceramic fiber thermal insulation disc 15. One end of the thermocouple 14 is built into the heat-resistant stainless steel sleeve embedded in the ceramic fiber thermal insulation disc 15, and the other end is located above the heating source 11, which is used to monitor and control the temperature of the heating source; the supporting and moving part of the central shaft 1 It is composed of a stainless steel tube 17 embedded with a corundum tube II 18 and an aluminum braided wire 19. The power input terminal 20 and the aluminum braided wire 19 extend into the inner cavity of the corundum tube II 18. One end of the aluminum braided wire 19 is connected to the power supply. The other end of the aluminum braided wire 19 passes through the flange 16 and the heat-resistant stainless steel sleeve embedded with a ceramic fiber heat-insulating disk 15 and is connected to the heating source 11 in sequence to supply power to the heating source 11. The heating source 11 is a silicon-molybdenum rod or a silicon-carbon rod. The specific specifications are selected according to the heating power. The threaded type or the straight rod type with uniform distribution around the circumference. Among them, the outer diameter of the insulating disk 10 is greater than the outer diameter of the corundum tube I 12.
[0047] A connecting frame is installed at the bottom of the furnace body shell 2, and each connecting frame is an upper support frame 21 and a lower support frame 22 plug-in matching structure arranged in two upper and lower sections along the vertical direction. The lower part of the upper support frame 21 and the upper part of the lower support frame 22 are respectively provided with more than two mounting holes for inserting knobs or bolts 23. The upper support frame 21 and the lower support frame 22 are connected and fixed at different positions by knobs or bolts 23 to realize the vertical movement of the furnace body shell 2 to adjust the height of the furnace body shell 2; the lower end of each lower support frame 2 is provided with a roller 24 with a locking function, which supports the horizontal movement of the furnace body shell 2 through the connecting frame.
[0048] like Figure 1 As shown, the front and rear ends of the furnace shell 2 are provided with center holes, the center axis 1 is horizontally arranged in the furnace shell 2, the front center hole of the furnace shell 2 corresponds to the insulating heat-insulating disc 10 and is in sliding fit, and the rear center hole of the furnace shell 2 corresponds to the stainless steel tube 17 and is in sliding fit; the heat-resistant stainless steel sleeve is embedded with a ceramic fiber heat-insulating disc 15 corresponding to the rear center hole and the inner wall of the furnace shell 2, and the thickness of the insulating heat-insulating disc 10 is the same as that of the furnace shell 2, so that the inner cavity of the furnace shell 2 forms a closed heat-insulating space. At this time, it is a preheating state, and the corundum tube I 12 can be preheated by the heating source 11. The furnace shell 2 is in a closed state, and the heating source 11 gradually heats up to a stable stage.
[0049] A hand-cranked gear 2a is installed at the bottom of the center hole of the rear end outer wall of the furnace body shell 2, and a transmission rack 1a is installed at the bottom of the stainless steel tube 17. The hand-cranked gear 2a and the transmission rack 1a correspond to each other to form a gear rack transmission mechanism; when working, the front end of the furnace body shell 2 corresponds to the centrifuge mold 3, and the centrifuge mold 3 is composed of an annular mold sleeve 32 installed in the centrifuge shell 34, a disc-shaped mold pad 33 and a disc-shaped mold cover 31 with a center hole, the mold cover 31 and the mold pad 33 are arranged at the two ends of the annular mold sleeve 32, the mold cover 31 is located at one side opening of the centrifuge shell 34, and the mold pad 33 is located at the inner wall of the other side of the centrifuge shell 34 The inner cavity of the centrifuge mold 3 is surrounded by a mold cover 31, an annular mold sleeve 32, and a mold pad 33. After being poured, the tin-bronze alloy melt 4 is filled in the inner cavity of the centrifuge mold 3 in an annular shape under the action of centrifugal force; the front end center hole of the furnace body shell 2 is coaxially corresponding to the center hole of the mold cover 31, and the outer diameter of the insulating and heat-insulating disk 10 is smaller than the diameter of the center hole of the mold cover 31; when in use, the furnace body shell 2 is fixed, and the hand-cranked gear 2a and the transmission rack 1a are matched to drive, so that the stainless steel pipe 17 drives the central shaft 1 and the heating source 11 to extend from the inner cavity of the furnace body shell 2, and the central shaft 1 connected to the heating source 11 is pushed forward, so that the heating source 11 is placed in the inner cavity of the centrifuge mold 3.
[0050] When in use, the furnace shell 2 is fixed, and the hand-cranked gear 2a and the transmission rack 1a are matched to drive the central shaft 1 to drive the heating source 11 to extend from the inner cavity of the furnace shell 2, and the central shaft 1 connected to the heating source 11 is pushed forward, so that the heating source 11 is placed in the inner cavity of the centrifuge mold 3, and the heat-resistant stainless steel sleeve is embedded with a ceramic fiber insulation plate 15, which is located in the opening of the mold cover 31 at one end of the centrifuge mold 3, and plays a role in sealing and heat preservation. At this time, it is in the working state, and the air in the inner cavity of the centrifuge mold 3 is heated by the heat radiation of the heating source 11 and the corundum tube Ⅰ12, and the heat is transferred to the casting in the centrifuge mold 3.
[0051] The present invention is further described in detail below through examples and drawings.
[0052] Example
[0053] In this embodiment, the alloy grade is ZCuSn5Pb5Zn5, and the casting diameter is (outer diameter 600mm, inner diameter 400mm), casting length 300mm. Figure 1-Figure 2 As shown, a centrifugal casting method for eliminating shrinkage defects of thick-walled tin bronze alloy castings comprises the following steps:
[0054] (1) Calculate the mold thickness L
[0055] L≥1.5×(600-400) / 2=150mm. Here, the wall thickness of the centrifuge shell + the wall thickness of the casting mold sleeve should be greater than 150mm. This thickness ensures the heat storage capacity of the casting mold.
[0056] (2) Calculate the mold speed n
[0057] ρ:8400kg / m 3 , g: 9.81m / s 2 , r i :0.2m, calculated to be 516≤n≤602. Because this grade of alloy is prone to lead segregation, a lower speed n=530rpm is selected within this range, and the alloy liquid pouring speed is 32kg / s. This speed can ensure that the alloy liquid fills the mold smoothly and continuously without splashing and interruption, and reduces defects such as segregation and slag inclusion.
[0058] (3) Preparation before pouring
[0059] Turn the knob or bolt 23 to adjust the height of the heating device to correspond to the height of the centrifuge casting cavity, connect the power input terminal 20 to the power supply, and preheat the heating device to 800°C. Figure 1After the alloy liquid is poured (the pouring temperature is 1090℃), take out the pouring system immediately, align the movable heating furnace with the inner cavity of the centrifuge mold, and adjust the roller 24 with locking function to a fixed position, push the central axis 1 connected to the heating source 11 forward, and pay attention to this process to ensure that the heating device does not contact the centrifuge mold, so that the heating source 11 is placed in the inner cavity of the centrifuge mold, as shown in the figure. Figure 2 state, ensuring that the inner cavity temperature of the centrifuge casting mold is 800℃ for 7 minutes.
[0060] (4) Remove the heating device and wait for the casting to cool to 500°C. Then stop the centrifuge and control the total operation time of the centrifuge to be around 25 minutes. Cooling to this temperature can prevent defects such as casting deformation and "tin sweating" caused by early demolding.
[0061] (5) After demolding, the casting defects on the inner surface of the annular casting are machined to remove the casting defects. The removal depth is greater than 23 mm. This depth can ensure that all shrinkage positions are removed and the finished casting has no shrinkage defects.
[0062] like Figure 3 and Figure 4 The shrinkage defect distribution of the whole casting and the center surface obtained by simulation is shown in the figure. The shrinkage area of the casting obtained by conventional centrifugal casting method is axially concentrated in the center position and has a large width. It is located radially between the inner and outer rings of the casting and close to the inner ring and has a wide range. The machining removal amount must reach 47mm to completely remove the shrinkage defect, and the inner ring diameter of the finished product is After machining, at least 20mm deep shrinkage defects remain near the inner ring of the finished product, seriously affecting the quality of the casting. The shrinkage area obtained by the centrifugal casting method provided by the present invention is also located in the center axially but has a narrow width, and is located on the surface of the inner ring of the casting radially with a small range. As long as the machining removal amount is more than 23mm, the shrinkage defects can be completely eliminated, significantly improving the quality of the finished casting.
[0063] The implementation results show that the present invention uses a movable heating furnace to extend into the inner cavity of the centrifuge casting to heat the poured copper alloy, and changes the solidification mode of the casting from bidirectional solidification to sequential solidification, thereby adjusting the position of the shrinkage area to move closer to the inner surface of the casting and removing it through machining. The present invention can completely eliminate the banded shrinkage defects inside the tin bronze alloy casting, significantly reduce the slag inclusions inside the casting, improve the segregation of casting elements, reduce the consumption of raw materials, reduce the difficulty of machining, and improve the casting yield rate.
[0064] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent methods or equivalent structural changes made using the contents of the present invention's specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings. It is characterized in that The method comprises the following steps: 1) the thickness of the casting mold is more than 1.5 times the thickness of the casting; 2) a wide-diameter gate is used for centrifugal pouring to ensure that the alloy liquid is uniform and continuous during the centrifugal process; 3) after the alloy liquid is poured, the pouring system is immediately taken out, and a heating device is placed in the centrifuge casting mold to heat the inner cavity; 4) the heating device is taken out, and the centrifugal operation is stopped after the casting is cooled and formed; 5) after demoulding, the inner surface of the annular casting is machined to remove surface casting defects.
2. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 1, It is characterized in that In step 2), the centrifuge speed is first determined according to the inner diameter of the casting, and then the alloy pouring speed is determined according to the speed and the size of the casting. The mold speed calculation formula is as follows: n——mold speed, r / min; ρ——density of copper alloy, kg / m 3 ; g——acceleration due to gravity, m / s 2 ; r i ——Inner radius of annular casting, m; The speed is adjusted within this range according to the different elements added to the copper alloy. The alloy pouring speed is proportional to the mold speed and the casting length, that is, the higher the mold speed, the longer the casting and the faster the pouring speed.
3. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 1, It is characterized in that In step 3), the heating device is a movable heating furnace, including a central axis and a furnace shell, and the specific structure is as follows: The central axis is placed horizontally and can move forward and backward in the horizontal direction. The main body is composed of a heating part and a supporting moving part coaxially connected by flanges; the heating part of the central axis is provided with a ceramic fiber thermal insulation module, a heating source, and a corundum tube I in sequence from the inside to the outside, and an insulating heat insulation disc is coaxially integrated at the front end of the heating part. The outer diameter of the insulating heat insulation disc is larger than the outer diameter of the corundum tube I, and a heat-resistant stainless steel sleeve is provided at the rear end of the heating part. A ceramic fiber thermal insulation disc is embedded in the heat-resistant stainless steel sleeve; the supporting moving part of the central axis is composed of a stainless steel tube embedded in a corundum tube and aluminum braided wire; Center holes are provided at the front and rear ends of the furnace shell, and the center axis passes through the furnace shell in the horizontal direction. The front center hole of the furnace shell corresponds to the insulating heat-insulating disc and is in sliding fit, and the rear center hole of the furnace shell corresponds to the stainless steel pipe and is in sliding fit; the heat-resistant stainless steel sleeve corresponds to the rear center hole and inner wall of the furnace shell, and the thickness of the insulating heat-insulating disc is the same as that of the furnace shell; a hand-cranked gear is installed at the bottom of the center hole of the rear end outer wall of the furnace shell, and a transmission rack is installed at the bottom of the stainless steel pipe, and the hand-cranked gear corresponds to the transmission rack to form a gear rack transmission mechanism.
4. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin bronze alloy castings according to claim 3, It is characterized in that The heating part of the central axis is arranged with a thermocouple, one end of which is built into a ceramic fiber insulation disk embedded in a heat-resistant stainless steel sleeve, and the other end is located above the heating source; the heating source is a silicon-molybdenum rod or a silicon-carbon rod, and a threaded type or a straight rod type with uniform circumferential distribution is selected according to the heating power.
5. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 3, It is characterized in that The stainless steel tube is lined with a corundum tube II, and the power input terminal clamp together with the aluminum braided wire therein extends into the inner cavity of the corundum tube II. One end of the aluminum braided wire is connected to the power source, and the other end of the aluminum braided wire passes through the flange and the center axis in sequence to be connected to the heating source.
6. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 3, It is characterized in that A connecting frame is installed at the bottom of the furnace body shell, and each connecting frame is an upper support frame and a lower support frame plug-in matching structure with two upper and lower sections arranged vertically. The lower part of the upper support frame and the upper part of the lower support frame are respectively provided with more than two mounting holes for inserting knobs or bolts. The upper support frame and the lower support frame are connected and fixed at different positions by knobs or bolts to realize the vertical movement of the furnace body shell to adjust the height of the furnace body shell; the lower end of each lower support frame is provided with a roller with a locking function, which supports the horizontal movement of the furnace body shell through the connecting frame.
7. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 3, It is characterized in that During operation, the front end of the furnace shell corresponds to the centrifuge mold, and the centrifuge mold consists of an annular mold sleeve, a disc-shaped mold pad and a disc-shaped mold cover with a center hole. The mold cover and the mold pad are arranged at two ends of the annular mold sleeve relatively, the mold cover is located at one opening of the centrifuge shell, and the mold pad is located at the inner wall of the other side of the centrifuge shell. The mold cover, the annular mold sleeve and the mold pad form an inner cavity of the centrifuge mold. After pouring, the tin-bronze alloy melt is filled in the inner cavity of the centrifuge mold in an annular shape under the action of centrifugal force; the front center hole of the furnace shell corresponds to the center hole of the mold cover coaxially, and the outer diameter of the insulating heat-insulating disk is smaller than the diameter of the center hole of the mold cover; during use, the furnace shell is fixed, and the hand-cranked gear and the transmission rack are matched to drive the stainless steel pipe to drive the central axis and the heating source to extend from the inner cavity of the furnace shell, and the central axis connected to the heating source is pushed forward, so that the heating source is placed in the inner cavity of the centrifuge mold.
8. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 3, It is characterized in that The use of the heating device includes a preheating / slow cooling state and a working state, wherein: in the preheating / slow cooling state, the furnace shell is closed, the heating source is located inside the furnace shell, and the heating source gradually heats up to a stable stage or gradually cools down; in the working state, the furnace shell is open, and the central axis connected to the heating source is pushed forward, so that the heating source is placed in the inner cavity of the centrifuge mold, and the air in the inner cavity of the centrifuge mold is heated by thermal radiation, and the heat is transferred to the casting in the centrifuge mold.
9. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 8, It is characterized in that In the preheating state, the temperature in the furnace needs to be controlled to 800℃~1100℃; in the working state, the temperature of the inner cavity of the centrifuge mold needs to be controlled at 800℃~1100℃ for 3~10min. The specific temperature and time are adjusted according to different alloys and different casting sizes.
10. The centrifugal casting method for eliminating shrinkage defects of thick-walled tin-bronze alloy castings according to claim 1, It is characterized in that In step 4), the casting is cooled and the molding temperature drops to 500°C ± 20°C and the machine is shut down. The removed heating device is continuously used for heating other centrifugal castings or slowly cooled to room temperature.
Citation Information
Cited By