Sodium metal negative electrode material with high rate capability and preparation method and application thereof
By covering metal powder on the surface of sodium metal to form a suspension, the problem of poor cycle stability and rate performance of sodium metal negative electrode materials is solved, and the performance of high-speed and long-life sodium metal battery is achieved, and the polarization voltage and Energy consumption.
Patent Information
- Application Number
- CN202411263923.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-03
AI Technical Summary
The sodium metal negative electrode materials have problems with short life and poor performance during circulation, mainly because the artificial solid electrolyte interface film is prone to rupture and sodium dendrites grow, resulting in a decrease in circulation stability, and traditional planar electrodes limit sodium ion transport. dynamics.
By dispersing metal powders such as Sn, Sb, Bi, etc. into the solvent to form a suspension, covering the surface of the sodium metal in an inert atmosphere, and obtaining a sodium metal negative electrode material after the solvent evaporates, increasing the specific surface area and nucleation position of the electrode To inhibit sodium dendrites growth, improve electrolyte wettability and sodium ion diffusion kinetics.
It realizes the high-rate performance and long-cycle stability of sodium metal negative electrode materials, can stabilize deposition/peel at high current density, low polarization voltage and low energy consumption, low equipment requirements, and simple preparation process.
Smart Images

Figure CN119057059A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium metal batteries, and in particular relates to a sodium metal negative electrode material with good rate performance and stable cycle, and a preparation method and application thereof. Background Art
[0002] At present, with the depletion of global fossil energy and the increase in carbon emissions, people have begun to pay attention to the use of renewable energy. For example, more and more countries are promoting the use of new energy electric vehicles, and lithium-ion batteries have been successfully put into practical use so far. However, in recent years, the shortage of lithium resources and the soaring prices have triggered people's exploration of the next generation of energy storage technology. Lithium resources account for only 0.002% of the earth's crust, while sodium reserves are as high as 2.74%, which is more than 400 times that of lithium. More importantly, sodium is widely distributed in the ocean and is almost inexhaustible. This gives sodium metal batteries (SMBs) a clear advantage in raw material costs, which helps to reduce the overall cost of batteries. The metallic sodium anode has a high theoretical specific capacity (1166 mAh g -1 ), low redox potential (-2.71 V compared to the standard hydrogen electrode) and abundant sodium resources show greater competitiveness.
[0003] However, the sodium metal anode still faces key problems such as sodium dendrite growth, huge volume expansion and fragile solid electrolyte interface (SEI) film, which seriously hinders its commercial application. Studies have shown that constructing a relatively stable artificial SEI on the electrode surface can improve the mechanical strength of the interface, withstand the huge volume changes during sodium deposition / stripping, and protect metallic sodium from electrolyte corrosion. In addition, it can also reduce the current density and promote the uniform deposition / stripping of sodium, effectively inhibiting the growth of sodium dendrites. However, the artificial SEI is prone to rupture and gradually fail as the cycle progresses, resulting in interface deterioration. Therefore, it is difficult to maintain long-term stability, and dendrite growth will still occur, and the cycle stability will decrease. On the other hand, due to the limited interface of the traditional planar electrode, its sodium ion transport kinetics are poor, and it is difficult to achieve extremely high rate deposition / stripping. Summary of the invention
[0004] Aiming at the technical problems of short cycle life and poor high rate performance of sodium metal negative electrode, the present invention proposes a sodium metal negative electrode material and its preparation method and application. The preparation method can be obtained by simple dropwise addition, which solves the problems of high requirements for production equipment, high energy consumption and high cost in traditional methods. The sodium metal negative electrode material has high rate performance, long cycle stability and low polarization voltage.
[0005] In order to achieve the above object, the technical solution of the present invention is achieved as follows: A sodium metal negative electrode material, the specific preparation method of which is as follows: (1) Dispersing metal powder into a solvent to prepare a suspension; (2) In an inert atmosphere, evenly cover the surface of the sodium metal with the suspension; (3) After the solvent is completely evaporated, the sodium metal negative electrode material is obtained.
[0006] The solvent in step (1) is at least one of tetrahydrofuran, acetone, and diethanol dimethyl ether; the metal powder is at least one of Sn, Sb, Bi, In, and Ga; and the concentration of the suspension is 0.01-0.6 g / mL.
[0007] Beneficial effects of the present invention: (1) The sodium metal negative electrode material described in the present invention has a larger specific surface area than traditional planar electrodes. The sodium-philic alloy formed in situ on the surface of the metal powder provides a large number of nucleation sites, achieving uniform sodium flux on the electrode surface and ensuring uniform deposition / stripping of sodium, thereby effectively inhibiting the growth of sodium dendrites and improving the electrode cycle stability. Secondly, the excellent wettability of the electrolyte can effectively reduce the interface resistance and accelerate the diffusion kinetics of sodium ions. At the same time, the large electrode surface can significantly increase the exchange current density and achieve uniform sodium deposition / stripping at high rates. In addition, the present invention has the characteristics of simple operation, low equipment requirements, low energy consumption, and short preparation process; (2) The prepared sodium metal anode material has a high conductivity at 170 mA cm -2 The deposition / stripping can be stably and reversibly performed at ultra-high current density with a polarization voltage not exceeding 100 mV. -2 , the deposition stripping amount is 10 mA cm -2 Under the conditions of , it can be stably cycled for 2500 h, which shows that the sodium metal anode material successfully achieves high rate performance and long stable cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] In order to more clearly illustrate the technical solutions in the embodiments or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0009] Figure 1 The SEM images of Example 1 and Comparative Example 1 of the present invention are shown in FIG.
[0010] Figure 2 2 are XRD diagrams of Example 1 and Comparative Example 1 of the present invention.
[0011] Figure 3It is a schematic diagram of the implementation of the present invention.
[0012] Figure 4 This is a rate performance diagram of Example 1 of the present invention and Comparative Example 1.
[0013] Figure 5 The negative electrode materials prepared in Example 1 and Comparative Example 1 of the present invention are -2 Deposition stripping 10 mA hcm -2 performance under conditions.
[0014] Figure 6 The Tafel curves of Example 1 and Comparative Example 1 are shown in FIG. DETAILED DESCRIPTION
[0015] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] Example 1 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal Sn powder is dispersed in tetrahydrofuran solvent to prepare a 0.04 g / mL suspension; in an inert atmosphere, 150 μL of the suspension is evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet is 8 mm; after the solvent is completely evaporated, the sodium metal negative electrode material can be obtained.
[0017] Example 2 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.2 g of metal Sn powder is dispersed in tetrahydrofuran solvent to prepare a 0.02 g / mL suspension; in an inert atmosphere, 150 μL of the suspension is evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet is 10 mm; after the solvent is completely evaporated, the sodium metal negative electrode material can be obtained.
[0018] Example 3 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.6 g of metal Sn powder is dispersed in tetrahydrofuran solvent to prepare a 0.06 g / mL suspension; in an inert atmosphere, 150 μL of the suspension is evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet is 12 mm; after the solvent is completely evaporated, the sodium metal negative electrode material can be obtained.
[0019] Example 4 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.1 g of metal Sn powder is dispersed in tetrahydrofuran solvent to prepare a 0.01 g / mL suspension; in an inert atmosphere, 150 μL of the suspension is evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet is 10 mm; after the solvent is completely evaporated, the sodium metal negative electrode material can be obtained.
[0020] Example 5 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 6 g of metal Sn powder was dispersed in tetrahydrofuran solvent to prepare a 0.6 g / mL suspension; in an inert atmosphere, 150 μL of the suspension was evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet was 10 mm; after the solvent was completely evaporated, the sodium metal negative electrode material was obtained.
[0021] Example 6 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal Bi powder was dispersed in tetrahydrofuran solvent to prepare a 0.04 g / mL suspension; in an inert atmosphere, 150 μL of the suspension was evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet was 11 mm; after the solvent was completely evaporated, the sodium metal negative electrode material was obtained.
[0022] Example 7 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal Sb powder was dispersed in tetrahydrofuran solvent to prepare a 0.04 g / mL suspension; in an inert atmosphere, 150 μL of the suspension was evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet was 9 mm; after the solvent was completely evaporated, the sodium metal negative electrode material was obtained.
[0023] Example 8 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal In powder was dispersed in tetrahydrofuran solvent to prepare a 0.04 g / mL suspension. In an inert atmosphere, 150 μL of the suspension was evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet was 12 mm. After the solvent was completely evaporated, the sodium metal negative electrode material was obtained.
[0024] Example 9 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal Sn powder was dispersed in acetone solvent to prepare a 0.04 g / mL suspension. In an inert atmosphere, 150 μL of the suspension was evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet was 6 mm. After the solvent was completely evaporated, the sodium metal negative electrode material was obtained.
[0025] Example 10 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal Sn powder was dispersed in diethanol dimethyl ether solvent to prepare a 0.04 g / mL suspension; in an inert atmosphere, 150 μL of the suspension was evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet was 8 mm; after the solvent was completely evaporated, the sodium metal negative electrode material was obtained.
[0026] Embodiment 11 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal Sn powder is dispersed in tetrahydrofuran solvent to prepare a 0.04 g / mL suspension; in an inert atmosphere, 50 μL of the suspension is evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet is 8 mm; after the solvent is completely evaporated, the sodium metal negative electrode material can be obtained.
[0027] Example 12 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: 0.4 g of metal Sn powder is dispersed in tetrahydrofuran solvent to prepare a 0.04 g / mL suspension; in an inert atmosphere, 500 μL of the suspension is evenly covered on the surface of sodium metal, and the diameter of the sodium metal sheet is 8-10 mm; after the solvent is completely evaporated, the sodium metal negative electrode material can be obtained.
[0028] Comparative Example 1 This comparative example uses pure sodium metal that has not been modified in Example 1 as the negative electrode material.
[0029] Comparative Example 2 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: A symmetric cell was assembled by directly covering a Sn foil with a diameter of 12 mm on a Na metal surface with a diameter of 12 mm.
[0030] Comparative Example 3 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: Sn powder was mixed with a binder and conductive carbon black in a ratio of 8:1:1 and evenly coated on the surface of copper foil. The mixture was then dried in a vacuum drying oven at 60°C and used as the negative electrode to assemble a symmetrical battery.
[0031] Comparative Example 4 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: Sodium metal with a diameter of 12 mm was directly physically mixed with 0.4 g Sn powder, that is, the Sn powder was rolled on the surface of the sodium metal to assemble a symmetrical battery.
[0032] Comparative Example 5 A sodium metal negative electrode material with high rate performance, the preparation method steps are as follows: Sodium metal with a diameter of 12 mm was evenly mixed with 0.4 g of Sn powder so that the Sn powder was also evenly present inside the sodium metal, and a symmetrical battery was assembled.
[0033] Application Examples The negative electrode material prepared in the embodiment of the present invention is directly used as the pole piece of the sodium metal battery. A button cell is assembled in a glove box, and the button cell model is CR2032. The counter electrode is also the prepared material, the diaphragm is glass fiber, and the electrolyte is 1 mol / LNaPF6 dissolved in ethylene glycol dimethyl ether. The assembled battery is placed for more than 8 hours to perform a deposition and stripping cycle process.
[0034] In the figure below, the sample prepared in Example 1 is denoted as Sn-Na, and the sample prepared in Comparative Example 1 is denoted as Na-Na.
[0035] Figure 1 It is the SEM picture of the sample prepared in comparative example 1 and the sample prepared in embodiment 1. It can be seen from the picture that the Sn powder is successfully loaded on the surface of the sodium metal.
[0036] Figure 2 2 are the X-ray powder diffraction patterns of Example 1 and Comparative Example 1 of the present invention. It can be seen from the X-ray powder diffraction patterns that the negative electrode material in Example 1 shows obvious peaks corresponding to Sn, indicating successful modification, while the unmodified material only has peaks corresponding to pure Na.
[0037] Figure 3 It is a schematic diagram of the implementation of the present invention.
[0038] Figure 4 The figure is a rate performance diagram of Example 1 of the present invention and Comparative Example 1. The current density of Example 1 can reach 170 mA cm -2 , and the polarization voltage is only 78 mV, the rate performance is significantly improved, showing excellent stability under high current density. -2, the polarization voltage increased to 200 mV, and the subsequent current density continued to increase, and the polarization voltage began to fluctuate sharply.
[0039] Figure 5 The negative electrode material prepared in Example 1 of the present invention is 10 mA cm -2 Deposition stripping 10 mA h cm -2 The performance under the conditions of 100 h can be stably cycled for 2500 h, showing its excellent stability. However, under the same conditions, the polarization voltage of Comparative Example 1 increased sharply after less than 100 h of cycling, and the voltage fluctuated thereafter.
[0040] Figure 6 1 and 2 are Tafel curves of Example 1 and Comparative Example 1. It can be seen from the figure that the exchange current density of the modified Sn-Na symmetric battery is larger, indicating its faster kinetics and also highlighting the positive effect of the modification.
[0041] The present invention conducted experiments on the negative electrode material performance of Examples 1-12 and Comparative Example 1, and the results are shown in Table 1: Table 1 Performance test of negative electrode materials prepared in Examples 1-12 and Comparative Example 1 Table 2 Performance test of negative electrode materials prepared in Comparative Examples 2-5 and Example 1 Anode Materials Sn form Cycle time (h) Polarization voltage (mV) Comparative Example 2 Sn foil 1040 60 Comparative Example 3 Coating on copper foil 890 78 Comparative Example 4 Sn powder rolled on the surface of sodium metal 980 80 Comparative Example 5 Sn powder and sodium metal are rolled together evenly 680 97 Example 1 Evenly cover the surface of sodium metal 2500 10 Table 1 shows the negative electrode materials of Examples 1-12 and Comparative Example 1 at 1 mA cm -2 , deposition and stripping 1mA h cm -2 From the performance experiment under the conditions, it can be seen from the table that the concentration of Sn powder solution has a certain influence on its performance. Too low or too high concentration is not good for the battery cycle. Compared with other metal powders, adding them to the surface will also increase the performance accordingly, but only when Sn powder is added, the rate performance is the best.
[0042] Table 2 shows the negative electrode materials prepared in Comparative Examples 2-5 and Example 1 at 1 mA cm -2 , deposition and stripping 1 mA h cm -2 From the table, we can see that the form of Sn also has a great influence on the battery performance. Only when it is uniformly covered on the surface of sodium metal in the form of powder, the performance is optimal. In short, from the experimental results in the table, we can see that the present invention achieves a sodium metal negative electrode with long cycle stability at high rate by adjusting the drop concentration and the battery assembly method.
[0043] In summary, it can be proved that the preparation method of the present invention can achieve a high efficiency of up to 170 mA cm -2The current density is 20000, and the negative electrode material has the advantages of long cycle stability, low polarization voltage and high rate performance when applied to sodium metal batteries. At the same time, the present invention has the characteristics of easy preparation, simple operation, low energy consumption and low equipment requirements.
Claims
1. A method for preparing a sodium metal negative electrode material with high rate performance, characterized in that: The steps include: (1) Dispersing metal powder into a solvent to prepare a suspension; (2) In an inert atmosphere, evenly cover the surface of the sodium metal with the suspension; (3) After the solvent is completely evaporated, the sodium metal negative electrode material is obtained.
2. The method for preparing a sodium metal negative electrode material with high rate performance according to claim 1, characterized in that: The solvent of step (1) is at least one of tetrahydrofuran, acetone and diethanol dimethyl ether.
3. The method for preparing a sodium metal negative electrode material with high rate performance according to claim 1, characterized in that: The metal powder in step (1) is at least one of Sn, Sb, Bi, In, and Ga.
4. The method for preparing a sodium metal negative electrode material with high rate performance according to claim 1, characterized in that: The concentration of the suspension in step (1) is 0.01-0.6 g / mL.
5. A sodium metal negative electrode material with high rate performance, characterized in that: Prepared by the method according to any one of claims 1 to 4.
6. A negative electrode plate for a secondary battery, characterized in that: Contains the sodium metal negative electrode material with high rate as claimed in claim 5.