Star-shaped polycarbonate surfactant and preparation method thereof
Through the design of star-type polycarbonate surfactant, a stable oil-water interface is formed using multi-arm macromolecular initiator and polycarbonate chain, which solves the problem of insufficient lipophilicity of existing surfactants and improves the treatment of oily substances Efficiency and application effect.
Patent Information
- Application Number
- CN202411555119.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When existing surfactants treat relatively oily substances, they lack lipophilicity, resulting in difficulty in processing and dispersion, affecting production efficiency and application effect.
The star-type polycarbonate surfactant is used, and its structure includes a polycarbonate chain with a number average molecular weight of 200~3000 and a multi-arm macromolecular initiator residue. It has more than 3 molecular chains. It is prepared by a multi-head initiator to form a more Stable oil-water interface, balances hydrophilic and lipophilic properties.
It achieves better surfactant effects and a more stable oil-water interface, which improves the application effect and range of surfactants.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of surfactants, and in particular relates to a star-shaped polycarbonate surfactant and a preparation method thereof. Background Art
[0002] Surfactants (also known as interfacial agents) play a vital role in modern industry and science. These compounds have a unique molecular structure and can form an adsorption layer at the liquid interface, effectively combining two immiscible substances (such as oil and water). The presence of surfactants can significantly reduce the surface tension of the liquid surface and promote the occurrence of emulsification, dispersion and wetting.
[0003] Surfactants are widely used in many fields such as cosmetics, detergents, medicine, and food processing. They can not only adjust interfacial properties, but also improve emulsion stability, reduce particle size, improve solubility, etc., providing important support for the performance and quality of various products. Common types of surfactants include anionic surfactants, cationic surfactants, nonionic surfactants, and zwitterionic surfactants. Anionic surfactants such as sulfates and sulfates are widely used in detergents and cleaning products and can effectively remove dirt. Cationic surfactants such as quaternary ammonium salts are often used in softeners and disinfectants. Nonionic surfactants such as polyoxyethylene alcohol compounds have good wettability and permeability and are commonly found in detergents and personal care products. Zwitterionic surfactants have both anionic and cationic properties, which help to achieve emulsification and dispersion in different media.
[0004] Most of the surfactants in the prior art have a relatively high hydrophilicity and a relatively low lipophilicity. In industrial production, if relatively oily substances need to be processed, the insufficient lipophilicity of the surfactant may cause difficulties in processing and dispersion, affect production efficiency, and limit the application effect and scope of the surfactant. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a star-shaped polycarbonate surfactant with a more balanced hydrophilicity and lipophilicity and a preparation method thereof.
[0006] The technical solution adopted by the present invention to solve the technical problem is: a star-shaped polycarbonate surfactant having the following structure: A n —C, wherein A is a polycarbonate chain with a number average molecular weight of 200 to 3W, n is 3 to 20, C is a multi-arm macromolecular initiator residue, and the structural formula of the polycarbonate chain is:
[0007] ,
[0008] Wherein, m and n are both integers, and 1≤m≤90, 5≤n≤450; R is hydrogen, C1~C22 alkyl, C1~C22 alkyl ether, preferably R is hydrogen or methyl.
[0009] The present invention provides a star-shaped surfactant having more than three molecular chains and a better three-dimensional structure. Compared with a linear water reducer, it can form a more stable oil-water interface, thereby achieving a better surface activity effect.
[0010] Preferably, in the star-shaped polycarbonate surfactant, the ratio of b to a is 2 to 5: 1. Under the preferred segment length ratio, the hydrophilic and lipophilic properties of the surfactant can be better balanced.
[0011] Preferably, in the above star-shaped polycarbonate surfactant, the general formula of C is R(-L) n , R(-L) n It is an n-valent anionic group derived from (A) a nitrogen-free aliphatic or aromatic organic polycarboxylic acid, (B) a polyphenol, (C) polyacrylic acid, acrylic acid-methacrylic acid copolymer or polymaleic acid, (D) hydroxyaromatic carboxylic acid, or (E) a nitrogen-containing aliphatic or aromatic organic polycarboxylic acid; R is an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a nitrogen-containing aliphatic hydrocarbon group or a nitrogen-containing aromatic hydrocarbon group, and -L is -COO- (carboxylate) or -O- (oxygen).
[0012] The initiator having the general formula C is a stable multi-arm macromolecular onium salt initiator (I) used to prepare high molecular weight multi-arm star-shaped polycarbonate surfactants. It can also be used to prepare low molecular weight multi-arm polycarbonate polyols.
[0013] Therefore, according to the first embodiment, there is provided a polyfunctional onium salt initiator (or multi-arm macromolecular initiator) having the following general formula (I) which is not completely onium salted (i.e., not completely salified, not completely neutralized or partially neutralized, and contains H+):
[0014]
R(-L)n
(MR′x)bHc
[0015] n=b+c;
[0016] In the formula, R(-L)n is an n-valent anionic group derived from (A) a nitrogen-free aliphatic or aromatic organic polycarboxylic acid, (B) a polyphenol, (C) polyacrylic acid, acrylic acid-methacrylic acid copolymer or polymaleic acid, (D) hydroxy aromatic carboxylic acid, or (E) a nitrogen-containing aliphatic or aromatic organic polycarboxylic acid; -L is -COO- (carboxylate) or -O- (oxylate); MR'x is a cationic group ammonium ion (quaternary ammonium cation), sulfonium ion (quaternary uranium cation) or phosphonium ion (quaternary phosphonium cation) and H is a hydrogen ion (H+). R' is a C1-C30 hydrocarbon group, preferably a C2-C20 hydrocarbon group, more preferably a C2-C10 hydrocarbon group, more preferably a C2-C5 hydrocarbon group, such as ethyl, propyl or butyl.
[0017] x is 3 or 4. When MR'x is an ammonium ion (quaternary ammonium cation) or a phosphonium ion (quaternary phosphonium cation), x is 4, and when MR'x is a sulfonium ion (quaternary sarsenium cation), x is 3. M is N (nitrogen), P (phosphorus) or S (sulfur).
[0018] n is the total number of carboxylic acids and / or phenolic hydroxyl groups in the polycarboxylic acids or polyphenols (i.e., R(-L)nHn) of (A) to (E). n is generally an integer of 2 to 30, preferably 3 to 29, more preferably 4 to 28, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27.
[0019] b is an integer of 1 to 29, preferably 2 to 28, more preferably 3 to 27, for example 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26. c is an integer greater than or equal to 1 (i.e., the compound of formula I contains at least one COOH or phenolic OH group), more preferably c is 1 to 15, preferably 1 to 13, preferably 1 to 10, preferably 1 to 6, more preferably 1, 2 or 3.
[0020] Preferably, the nitrogen-free aliphatic or aromatic polycarboxylic acid (A) is (or is selected from): (A1) (hydroxyl-free or hydroxyl-containing) C6-C30 (preferably C8-C20, more preferably C10-C16) aliphatic or aromatic organic polycarboxylic acid (such as 1,4-butanedicarboxylic acid, pentane-1,3,5-tricarboxylic acid, citric acid, malic acid, o-, m-, p-terephthalic acid, benzene trimecartonic acid, pyromellitic acid, naphthalene dicarboxylic acid, naphthalene trimecartonic acid, naphthalene tetracarboxylic acid, naphthalene pentacarboxylic acid, naphthalene hexacarboxylic acid).
[0021] Preferably, the polyphenol (B) is (or is selected from) C6-C30 (preferably C6-C20) polyphenol. More preferably, the polyphenol (C) is (or is selected from): o-, m- and p-quinone, naphthalene-tetraphenol, bisphenol A, bisphenol F, bisphenol S.
[0022] Preferably, the polyacrylic acid, acrylic acid-methacrylic acid copolymer or polymaleic acid (C) is a polyacrylic acid, acrylic acid-methacrylic acid copolymer or polymaleic acid having a number average molecular weight of 220-2000 (preferably 290-1500, more preferably 350-1000 or 500-900, such as 216, 258, 348, 600, 700 or 800).
[0023] Preferably, the hydroxyaromatic carboxylic acid (D) is a hydroxyaromatic polycarboxylic acid or a polyhydroxyaromatic carboxylic acid. Preferably, the hydroxyaromatic carboxylic acid (D) is (or is selected from): hydroxyphthalic acid, ...
[0024] Preferably, the nitrogen-containing aliphatic or aromatic organic polycarboxylic acid (E) is (or is selected from): (E1) C2-C30 (preferably C3-C28, more preferably C4-C24) alkylenediaminetetra(C2-C6)carboxylic acid, or nitrilotri(C2-C6)carboxylic acid; for example, ethylenediaminetetraacetic acid, ethylenediaminetetrapropionic acid, ethylenediaminetetrabutyric acid, ethylenediaminetetrapentanoic acid, ethylenediaminetetrahexanoic acid, propylenediaminetetraacetic acid, propylenediaminetetrapropionic acid, propylenediaminetetrabutyric acid, propylenediaminetetrapentanoic acid, propylenediaminetetrahexanoic acid, butylene diamine tetraacetic acid, butanediaminetetrapropionic acid, butanediaminetetrabutyric acid, butanediaminetetrapentanoic acid, butanediaminetetrahexanoic acid, nitrilotriacetic acid, nitrilotripropionic acid, nitrilotributyric acid, nitrilotripovaleric acid, or nitrilotrihexanoic acid; or, (E2) N-C1-C4 alkyl-piperidinedicarboxylic acid (such as N-methyl-piperidine-3,5-dicarboxylic acid), N-C1-C4 alkyl-piperidinetricarboxylic acid (such as N-ethyl-piperidinetricarboxylic acid), or N-C1-C4 alkyl-piperidinetetracarboxylic acid (such as N-ethyl-piperidinetetracarboxylic acid).
[0025] Preferably, R is an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a nitrogen-containing aliphatic hydrocarbon group, or a nitrogen-containing aromatic hydrocarbon group.
[0026] According to a second embodiment of the present invention, there is provided a fully onium salted (i.e., fully salified, fully neutralized, and free of H+) multifunctional onium salt initiator (or multi-arm macromolecular initiator) having the following general formula (II):
[0027]
R(-L)n
(MR′x)n
[0028] Here, MR'x is a cationic group such as a sulfonium ion (quaternary sulfonium cation) or a phosphonium ion (quaternary phosphonium cation).
[0029] wherein R(-L)n, R, -L, M, R', n and x are as defined above.
[0030] The inventors of the present application have found that, despite being completely onium salted, the initiator of the general formula II containing a sulfonium ion (quaternary stibnium cation) or a phosphonium ion (quaternary phosphonium cation) still has a high reactivity.
[0031] According to a third embodiment of the present invention, there is provided a fully onium salted (i.e., fully salified, fully neutralized, and free of H+) multifunctional onium salt initiator (or multi-arm macromolecular initiator) having the following general formula (III):
[0032]
R(-L)n
(MR′x)n
[0033] In the formula, R(-L)n is an n-valent anionic group derived from the above-mentioned (E) nitrogen-containing aliphatic or aromatic organic polycarboxylic acid;
[0034] wherein R, -L, M, R', n and x are as defined above.
[0035] Here, MR'x is a cationic group such as ammonium ion (quaternary ammonium cation), sulfonium ion (quaternary stibnium cation) or phosphonium ion (quaternary phosphonium cation).
[0036] Since the compound of the general formula III contains N and is a Lewis base itself, it has higher activity. Therefore, even if it is completely onium salted, it still has high reactivity.
[0037] Specifically, in the above star-shaped polycarbonate surfactant, C is:
[0038] and One or a combination of both.
[0039] Specifically, in the above star-shaped polycarbonate surfactant, C is:
[0040] , , and One, two or more of the following.
[0041] The above two initiator residues are derived from aromatic or aliphatic polyacid initiators, the ammonium salt onium salt initiators are all incomplete onium salt initiators, and the coronium salt and phosphonium salt include "incomplete onium salt initiators" and "complete onium salt initiators".
[0042] Specifically, in the above star-shaped polycarbonate surfactant, C is:
[0043] , , , and One, two or more of the following.
[0044] The above-mentioned initiator residues are derived from nitrogen-containing polyacid onium salt initiators (including fully onium salted and incompletely onium salted ammonium salts, coronium salts, and phosphonium salts): since such initiators are Lewis bases themselves, they have higher initiation activity and can produce star-shaped polycarbonate surfactants with more arms and larger molecular weights, and are more effective as surfactants.
[0045] Specifically, in the above star-shaped polycarbonate surfactant, C is:
[0046] , and One, two or more of the following.
[0047] The above-mentioned initiator residues are derived from polymethacrylate onium salts (including fully onium salted and incompletely onium salted ammonium salts, coronium salts, phosphonium salts), polyacrylate onium salts, polymethacrylate onium salts, polyacrylate onium salts, polymethacrylate onium salts and onium salts of copolymers thereof. Such initiators can arbitrarily control the number of arms of star-shaped polycarbonate surfactants, and the structure is similar to the existing polycarboxylic acid type surfactants, but can have better hydrophilic and lipophilic effects, and the activity of the surfactant is better.
[0048] A method for preparing a star-shaped polycarbonate surfactant, characterized in that it comprises the following steps:
[0049] 1) Put the epoxy compound, catalyst and multi-head initiator into a high-pressure reactor, introduce carbon dioxide until the pressure reaches 2.5MPa~4.0MPa, carry out polymerization reaction at 40℃~50℃ for 5~10 hours, and evacuate the unreacted epoxy compound;
[0050] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, and the reaction temperature is increased to 55°C~75°C for polymerization reaction for 5~15 hours, and then post-treatment is performed to obtain the product.
[0051] Compared with the existing multi-arm polycarbonate, the surfactant is mainly used to adjust the hydrophobicity and hydrophilicity inside and outside. In the preparation process of the surfactant of the present invention, a multi-head initiator is used for initiation, and a polycarbonate chain segment with a low polyether content is first polymerized to obtain a stable hydrophobic group and form a better lipophilic effect; then the process conditions are changed to connect the PEO chain segment with good hydrophilicity to each chain arm. In the process, the length of the chain segment is controlled by the reaction conditions, catalyst and feed amount, and the side reaction is reduced to ensure the activity of the surfactant.
[0052] The epoxy compound is an epoxy compound having hydrogen, C1-C22 alkyl or C1-C22 alkyl ether chain, such as ethylene oxide, propylene oxide, dodecyl glycidyl ether, BGE, AGE. Preferably, the epoxy compound is ethylene oxide and / or propylene oxide.
[0053] Specifically, in the preparation method of the above-mentioned star-shaped polycarbonate surfactant, the catalyst is a metal catalyst or an organic boron compound, and the metal catalyst includes a zinc catalyst system, a metal porphyrin catalyst system, a β-diimine metal complex catalyst, a double metal cyanide complex catalyst, a SalenMX catalyst system, a rare earth catalyst system, and a multi-metal catalyst system.
[0054] Preferably, the catalyst is an organic boron compound. In the present invention, it is preferably the self-polymerization of ethylene oxide and propylene oxide with higher reaction activity or their copolymerization with carbon dioxide. The requirements for the catalyst are relatively low. When the organic boron compound is used as a catalyst, it has good selectivity, reduces the self-polymerization of the epoxy compound in step 1), and ensures the hydrophobic effect of this section. More preferably, the catalyst is a composite catalyst of triethyl boron and triphenyl boron in a molar ratio of 1:5 to 8. The more preferred catalyst is combined with the process conditions, which can basically eliminate the self-polymerization of the epoxy compound in step 1), better ensure the hydrophobic effect of this section, and at the same time ensure the efficient polymerization of the PEO section.
[0055] The star-shaped polycarbonate surfactant is mainly used as a concrete surfactant or a demulsifier.
[0056] Compared with the prior art, the carbon dioxide-based surfactant polymer monomer and the preparation method thereof of the present invention have the following beneficial effects: the present invention provides a surfactant with a star structure, which has more than 3 molecular chains connected to the initiator residue, the chain segment close to the initiator residue is a hydrophobic polypropylene carbonate (PPC) and / or polyethylene carbonate (PEC), and the chain segment far away from the initiator is a hydrophilic polyether segment of ethylene oxide self-polymerization. The shorter hydrophobic segments are concentrated together by the initiator residue to enhance the lipophilic effect. The chain segments of PPC and PEC are relatively soft, and with appropriate chain lengths, they can change direction more freely at the oil-water interface to form a shape similar to a badminton or a wooden comb, have a better three-dimensional structure, and can form a more stable oil-water interface relative to a straight-chain water reducer, thereby achieving a better surface active effect. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments.
[0058] Example 1
[0059] 1) Put propylene oxide, triethyl boron and triphenyl boron in a molar ratio of 1:6 composite catalyst and multi-head initiator into a high-pressure reactor. ammonium ion phosphonium ion onium salt, the average value of n is 10; carbon dioxide is introduced until the pressure reaches 3.0 MPa, and the polymerization reaction is carried out at 45°C for 7 hours;
[0060] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, wherein the molar ratio of ethylene oxide to propylene oxide in step 1) is 3:1. The reaction temperature is raised to 65°C for polymerization for 9 hours, and the reaction is terminated after the reaction is complete to obtain a glue solution; the glue solution is washed and devolatilized to obtain the obtained surfactant. The molecular weight of the obtained surfactant is detected to be 5W. According to nuclear magnetic resonance detection, the percentage of PPC repeating units in the obtained surfactant molecular chain is 24.99%, and the percentage of PEO repeating units is 75.01%.
[0061] Example 2
[0062] 1) Add an epoxy compound, a composite catalyst of triethyl boron and triphenyl boron in a molar ratio of 1:5, and a multi-head initiator into a high-pressure reactor. The epoxy compound is a mixture of propylene oxide and ethylene oxide in a molar ratio of 5:1, and the multi-head initiator is The average value of n1+n2 is 12; carbon dioxide is introduced until the pressure reaches 3.5 MPa, and the polymerization reaction is carried out at 45°C for 8 hours;
[0063] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, wherein the molar ratio of ethylene oxide to the epoxy compound in step 1) is 4:1. The reaction temperature is raised to 65°C for polymerization reaction for 10 hours, and the reaction is terminated after the reaction is complete to obtain a glue solution; the glue solution is washed and devolatilized to obtain the obtained surfactant. The molecular weight of the obtained surfactant is detected to be 7.2W. According to nuclear magnetic resonance detection, the percentage of PPC and PEC repeating units in the obtained surfactant molecular chain is 19.98% in total, and the percentage of PEO repeating units is 80.02%.
[0064] Example 3
[0065] 1) Add an epoxy compound, a composite catalyst of triethyl boron and triphenyl boron in a molar ratio of 1:8, and a multi-head initiator into a high-pressure reactor. The epoxy compound is a mixture of propylene oxide and ethylene oxide in a molar ratio of 1:5. The multi-head initiator is ammonium ion salt; introducing carbon dioxide until the pressure reaches 3.0MPa, and carrying out polymerization reaction at 45°C for 9 hours;
[0066] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, wherein the molar ratio of ethylene oxide to the epoxy compound in step 1) is 3:1. The reaction temperature is raised to 65°C for polymerization reaction for 10 hours, and the reaction is terminated after the reaction is complete to obtain a glue solution; the glue solution is washed and devolatilized to obtain the obtained surfactant. The molecular weight of the obtained surfactant is detected to be 6W. According to nuclear magnetic resonance detection, the percentage of PPC and PEC repeating units in the obtained surfactant molecular chain is 24.97% in total, and the percentage of PEO repeating units is 75.03%.
[0067] Example 4
[0068] 1) Put ethylene oxide, triethyl boron and triphenyl boron in a molar ratio of 1:6 composite catalyst and multi-head initiator into a high-pressure reactor. ammonium ion salt; introducing carbon dioxide until the pressure reaches 2.5MPa, and performing polymerization reaction at 40°C for 10 hours;
[0069] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, wherein the molar ratio of ethylene oxide to ethylene oxide in step 1) is 2:1. The reaction temperature is raised to 75°C for polymerization reaction for 5 hours, and the reaction is terminated after the reaction is complete to obtain a glue solution; the glue solution is washed and devolatilized to obtain the obtained surfactant. The molecular weight of the obtained surfactant is detected to be 9.6W. According to nuclear magnetic resonance detection, the percentage of PPC repeating units in the obtained surfactant molecular chain is 33.17%, and the percentage of PEO repeating units is 66.83%.
[0070] Example 5
[0071] 1) Put propylene oxide, triethyl boron and triphenyl boron in a molar ratio of 1:6 composite catalyst and multi-head initiator into a high-pressure reactor. The phosphonium ion onium salt was introduced into the reaction mixture until the pressure reached 4.0 MPa, and the polymerization reaction was carried out at 50°C for 5 hours;
[0072] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, wherein the molar ratio of ethylene oxide to propylene oxide in step 1) is 5:1. The reaction temperature is raised to 55°C for polymerization reaction for 15 hours, and the reaction is terminated after the reaction is complete to obtain a glue solution; the glue solution is washed and devolatilized to obtain the obtained surfactant. The molecular weight of the obtained surfactant is detected to be 4W. According to nuclear magnetic resonance detection, the percentage of PPC repeating units in the obtained surfactant molecular chain is 16.32%, and the percentage of PEO repeating units is 83.68%.
[0073] Example 6
[0074] 1) Put propylene oxide, triethyl boron and triphenyl boron in a molar ratio of 1:1 composite catalyst and multi-head initiator into a high-pressure reactor. The multi-head initiator is ammonium ion salt, the average value of n is 10; carbon dioxide is introduced until the pressure reaches 3.0 MPa, and the polymerization reaction is carried out at 45°C for 7 hours;
[0075] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, wherein the molar ratio of ethylene oxide to propylene oxide in step 1) is 3:1. The reaction temperature is raised to 65°C for polymerization for 9 hours, and the reaction is terminated after the reaction is complete to obtain a glue solution; the glue solution is washed and devolatilized to obtain the obtained surfactant. The molecular weight of the obtained surfactant is detected to be 5W. According to nuclear magnetic resonance detection, the percentage of PPC repeating units in the obtained surfactant molecular chain is 24.56%, and the percentage of PEO repeating units is 75.44%.
[0076] Example 7
[0077] 1) Put propylene oxide, triethyl boron and multi-head initiator into a high-pressure reactor. The multi-head initiator is ammonium ion salt, the average value of n is 10; carbon dioxide is introduced until the pressure reaches 3.0 MPa, and the polymerization reaction is carried out at 45°C for 7 hours;
[0078] 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, wherein the molar ratio of ethylene oxide to propylene oxide in step 1) is 3:1. The reaction temperature is raised to 65°C for polymerization for 9 hours, and the reaction is terminated after the reaction is complete to obtain a glue solution; the glue solution is washed and devolatilized to obtain the obtained surfactant. The molecular weight of the obtained surfactant is detected to be 5W. According to nuclear magnetic resonance detection, the percentage of PPC repeating units in the obtained surfactant molecular chain is 23.92%, and the percentage of PEO repeating units is 76.08%.
[0079] The properties of the star-shaped polycarbonate surfactants prepared in Examples 1 to 7 are shown in Table 1. The initial foam height was measured using the Ross-Miles foam height method; the surfactants in each example were diluted 200 times with purified water, and the surface tension of the surfactants at room temperature was tested using the platinum sheet method and a fully automatic surface tension meter; the surfactants in each example were prepared into an aqueous solution with a concentration of 1 g / L, 20 mL was measured, mixed with No. 5 white oil, poured into a container with a scale, homogenized at a speed of 500 r / min for 1 min, and then allowed to stand, and the time consumed to separate 5 mL of water phase was recorded, and the longer the time consumed, the better the emulsification ability of the surfactant was considered to be.
[0080] Table 1
[0081] .
[0082] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A star-shaped polycarbonate surfactant, characterized in that: Has the following structure: A n —C, wherein A is a polycarbonate chain with a number average molecular weight of 200 to 3W, n is 3 to 20, C is a multi-arm macromolecular initiator residue, and the structural formula of the polycarbonate chain is: , Wherein, m and n are both integers, and 1≤m≤90, 5≤n≤450; R is hydrogen, C1~C22 alkyl, C1~C22 alkyl ether.
2. A star-shaped polycarbonate surfactant according to claim 1, characterized in that: The ratio of b to a is 2~5:
1.
3. A star-shaped polycarbonate surfactant according to claim 1, characterized in that: The general formula of C is R(-L)n, where R(-L)n is an n-valent anionic group derived from (A) a nitrogen-free aliphatic or aromatic organic polycarboxylic acid, (B) a polyphenol, (C) polyacrylic acid, acrylic acid-methacrylic acid copolymer or polymaleic acid, (D) a hydroxyaromatic carboxylic acid, or (E) a nitrogen-containing aliphatic or aromatic organic polycarboxylic acid; R is an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a nitrogen-containing aliphatic hydrocarbon group or a nitrogen-containing aromatic hydrocarbon group, and -L is -COO- or -O-.
4. A star-shaped polycarbonate surfactant according to claim 3, characterized in that: The C is: and One or a combination of both.
5. A star-shaped polycarbonate surfactant according to claim 3, characterized in that: The C is: 、 、 and One, two or more of the following.
6. A star-shaped polycarbonate surfactant according to claim 3, characterized in that: The C is: 、 、 、 and One, two or more of the following.
7. A star-shaped polycarbonate surfactant according to claim 3, characterized in that: The C is: , and One, two or more of the following.
8. A method for preparing the star-shaped polycarbonate surfactant according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) Put the epoxy compound, catalyst and multi-head initiator into a high-pressure reactor, introduce carbon dioxide until the pressure reaches 2.5MPa~4.0MPa, carry out polymerization reaction at 40℃~50℃ for 5~10 hours, and evacuate the unreacted epoxy compound; 2) After the reaction is completed, the gas in the kettle is replaced with nitrogen, and then ethylene oxide is added to the kettle, and the reaction temperature is increased to 55°C~75°C for polymerization reaction for 5~15 hours, and then post-treatment is performed to obtain the product.
9. The method for preparing a star-shaped polycarbonate surfactant according to claim 8, characterized in that: The catalyst is a metal catalyst or an organic boron compound, and the metal catalyst includes a zinc catalyst system, a metal porphyrin catalyst system, a β-diimine metal complex catalyst, a double metal cyanide complex catalyst, a SalenMX catalyst system, a rare earth catalyst system, and a multi-metal catalyst system.
Citation Information
Patent Citations
Carbon dioxide-based dobby polycarbonate composition
CN118406361A
Surface-active agent