Functional laser engraving high-temperature PEEK composite material applied to antenna LDS and preparation method of functional laser engraving high-temperature PEEK composite material

By using copper to coat nano CaTiO3 powder, nanoboronitride powder and other components in antenna materials, combined with laser engraving and single-screw extrusion technology, the signal quality of existing antenna materials under 5G technology is solved. The best problem is that efficient metal plating is combined with the substrate and excellent electromagnetic properties.

CN119060495APending Publication Date: 2024-12-03GUANGDONG GERUI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411176460.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the context of the development of 5G technology, existing antenna materials are difficult to meet the needs of high dielectric constant, low dielectric loss and excellent wave transmissibility. At the same time, the strength of metal plating and substrate bonding is insufficient, resulting in poor signal quality.

Method used

High temperature PEEK composite material is used, containing copper-coated nano CaTiO3 powder, nano boron nitride powder, 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl) homotriazine and polysilicon oxygen Alkane, formed by laser engraving to form a rough surface to increase the coating bond strength, and was prepared by melt mixing by a single screw extruder.

Benefits of technology

An antenna material with a small dielectric constant, low dielectric loss factor and excellent wave transmissibility is realized, which ensures communication quality and improves the bonding strength between the metal plating and the substrate to prevent the plating from falling off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010853450000071
    Figure BDA0005010853450000071
  • Figure FDA0005010853440000021
    Figure FDA0005010853440000021
Patent Text Reader

Abstract

The invention discloses a functional laser engraving high-temperature PEEK (polyether-ether-ketone) composite material applied to antenna LDS (laser direct structuring) and a preparation method of the functional laser engraving high-temperature PEEK composite material, and the functional laser engraving high-temperature PEEK composite material comprises the following components: 95-100 parts of polyether-ether-ketone resin, 2-5 parts of copper-coated nano CaTiO3 powder, 1-3 parts of nano boron nitride powder, 0.5-1 part of 1, 3, 5-tri (3, 5-di-tert-butyl, 4-hydroxybenzyl) s-triazine and 0.5-1 part of polysiloxane. By modifying the material, the PEEK composite material for the antenna, which is small in dielectric constant and dielectric loss factor and excellent in wave permeability, is obtained; and the metal coating and the base material have excellent bonding strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polymer composite materials, and more specifically to a high-temperature PEEK composite material for LDS functional laser engraving used in antennas and a preparation method thereof. Background Art

[0002] Antennas are key components in the field of communications. Their function is to convert guided waves in transmission lines into electromagnetic waves radiated in space. The quality of their performance determines the signal quality of the communication system. Laser Direct Structuring (LDS) technology is a manufacturing technology that directly forms circuit patterns on the surface of three-dimensional plastic parts. With the development of 5G technology, laser direct structuring technology is also widely used in the production of antennas. By irradiating the surface of a plastic part with a laser, the metal is induced to nucleate on the surface, and then electroplating and thickening are performed to form the desired circuit pattern, thereby forming an antenna. The substrate of the antenna is usually a thermoplastic, including polymers such as polyetheretherketone (PEEK), polyphenylene sulfide, polyimide, and polycarbonate.

[0003] Patent CN 113773615 A ​​discloses a plastic for antenna vibrator, including the following components by weight: 25-90 parts of base resin; 1-60 parts of laser reflector; 0-70 parts of inorganic filler. By selecting a base resin that can be chemically corroded or an inorganic filler that can be chemically corroded, the plastic can obtain a surface with low surface roughness and good morphological consistency through chemical roughening, reducing the PIM source, and forming multiple fine corrosion hole structures on the plastic surface to improve the bonding strength of its surface coating; and adding a laser reflector can effectively weaken or eliminate the carbonization effect of the laser on the plastic during laser processing, avoid the formation of carbonized particles, reduce the formation of burrs on the edge of the metal coating, and further improve PIM.

[0004] Antenna substrates are generally made of polymer matrix, laser activator, and other additives. The performance of the substrate also determines the performance of the antenna. Dielectric constant, dielectric loss factor, and wave transmittance are parameters that measure the performance of the antenna. With the development of 5G technology, the demand for antenna materials is also increasing. Summary of the invention

[0005] Based on the deficiencies and needs of the prior art, the present invention provides a high-temperature PEEK composite material for LDS functional laser engraving used in antennas and a preparation method. By modifying the material, a PEEK composite material for antennas with small dielectric constant, dielectric loss factor and excellent wave transmittance is obtained; and the metal coating has excellent bonding strength with the substrate.

[0006] In order to achieve the purpose of the present invention and obtain the above technical effects, the present invention provides the following technical solutions:

[0007] A high-temperature PEEK composite material for LDS functional laser engraving of antennas, comprising the following components by weight:

[0008] 95-100 parts of polyetheretherketone resin,

[0009] Copper coated nano-CaTiO 3 2-5 parts powder,

[0010] 1-3 parts of nano boron nitride powder,

[0011] 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine 0.5-1 part,

[0012] 0.5 to 1 part of polysiloxane.

[0013] Furthermore, the PEEK composite material comprises the following components in parts by weight:

[0014] 97-98 parts of polyetheretherketone resin,

[0015] Copper coated nano-CaTiO 3 3-4 parts powder,

[0016] 2-3 parts of nano boron nitride powder,

[0017] 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine 0.7-0.8 parts,

[0018] Polysiloxane 0.7-0.8 parts.

[0019] Furthermore, the PEEK composite material is composed of the following components in parts by weight:

[0020] 97-98 parts of polyetheretherketone resin,

[0021] Copper coated nano-CaTiO 3 3-4 parts powder,

[0022] 2-3 parts of nano boron nitride powder,

[0023] 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine 0.7-0.8 parts,

[0024] Polysiloxane 0.7-0.8 parts.

[0025] Furthermore, the copper-coated CaTiO 3 The preparation steps of the powder are as follows: 3The powder is immersed in a 50-60 g / L copper nitrate solution, filtered, dried, placed in a quartz furnace, sealed, and evacuated; then argon is introduced and heated to a preset temperature, and hydrogen is introduced after the temperature stabilizes; maintained for a certain period of time; and the introduction of gas is stopped after cooling to room temperature. Chemical vapor deposition technology is a prior art and will not be described in detail in this application. In order to make the powder evenly coated, ultrasonic vibration is applied to the quartz tube during the reaction process.

[0026] Furthermore, the nano-CaTiO 3 The particle size of the powder is 200-300 nm, and the copper-coated CaTiO 3 The particle size of the powder is 400 to 500 nm.

[0027] Furthermore, the preset temperature is 280-350° C., the argon flow rate is 100-150 sccm, the hydrogen flow rate is 200-300 sccm, and the reaction time is 30-45 min.

[0028] Furthermore, the particle size of the nano boron nitride powder is 200-300 nm.

[0029] Furthermore, the structural formula of the polyetheretherketone is: The molecular weight is 800,000 to 1,000,000 and the melt viscosity is 140 to 160 Pa.s.

[0030] This application uses nano-CaTiO 3 The powder was immersed in a copper nitrate solution, and copper nitrate was adsorbed on the surface. Then, in a reducing atmosphere, a reaction occurred in a quartz furnace to form nano-CaTiO 3 The powder surface forms a single copper-coated nano-CaTiO 3 Powder. Preferably, CaTiO 3 The powder leaching, filtering and drying steps were repeated 3 to 5 times; the copper-coated nano-CaTiO in the composite material 3 During the laser engraving process of the powder, the substrate forms a rough surface and Cu particles are exposed, which can provide nucleation sites during the chemical plating of the metal layer and provide a guarantee for the formation of a dense copper layer in the early stage of chemical plating. At the same time, the rough surface formed by laser engraving is also conducive to improving the bonding strength between the metal coating and the substrate.

[0031] In this application, nano boron nitride is added to improve the thermal conductivity and heat resistance of the composite material by utilizing its high thermal conductivity, low dielectric constant, chemical corrosion resistance and other characteristics, and can maintain the electrical insulation performance of the composite material. In addition, nano boron nitride is also beneficial to improve the mechanical properties of the composite material.

[0032] Furthermore, the PEEK composite material has a dielectric constant of 2.6 to 2.9, a dielectric loss of 0.005 to 0.008, and a wave transmittance greater than 96%.

[0033] A method for preparing a high-temperature PEEK composite material for antenna-type LDS functional laser engraving, comprising the following steps:

[0034] (1) Weigh the components in proportion for later use;

[0035] (2) Pour the components into a stirring device and stir them evenly, then send them into a single screw extruder, and obtain a polycarbonate composite material PEEK composite material through melting, mixing and extrusion.

[0036] Furthermore, the set temperature of the single screw extruder is: section one: 325-335°C, section two: 330-340°C, section three: 335-345°C, section four: 345-355°C, section five: 355-365°C, section six: 325-335°C, section seven: 325-335°C, section eight: 330-340°C, section nine: 335-345°C, and die head: 345-355°C.

[0037] Furthermore, the rotation speed of the single screw extruder is 300-350 rpm.

[0038] An antenna comprises a matrix of the above-mentioned PEEK composite material.

[0039] The present invention provides a high-temperature PEEK composite material for antenna-type LDS functional laser engraving and a preparation method thereof, which has the following beneficial effects compared with the prior art:

[0040] (1) The present invention studies PEEK and obtains a corresponding composite material, which can be used as an antenna matrix. The antenna prepared from the composite material has a small dielectric constant and dielectric loss factor and excellent wave transmittance; it can ensure communication quality and can be used in the 5G field.

[0041] (2) By improving the laser engraving additive, the bonding strength between the metal coating and the substrate is effectively improved, which can prevent the coating from falling off. DETAILED DESCRIPTION

[0042] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0043] Main raw materials: Polyetheretherketone is from Shenzhen Kokuyo Plastic Materials Co., Ltd., PEEK-1000; nano boron nitride powder is a product of Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0044] The copper-coated nano-CaTiO 3 The powder preparation steps are as follows: CaTiO 3 The powder was immersed in a 60g / L copper nitrate solution, filtered, dried (repeated 4 times), and then placed in a quartz furnace, sealed and evacuated; then argon was introduced and heated to a preset temperature, and hydrogen was introduced after the temperature stabilized; maintained for a certain time; and stopped introducing gas after cooling to room temperature. The preset temperature was 300°C, the argon flow rate was 150sccm, the hydrogen flow rate was 300sccm, and the reaction time was 0045min.

[0045] Example 1

[0046] A high-temperature PEEK composite material for LDS functional laser engraving of antennas, comprising the following components by weight:

[0047] 97 parts of polyetheretherketone resin,

[0048] Copper nanoparticles coated with CaTiO 3 3 parts powder,

[0049] 2 parts of nano boron nitride powder,

[0050] 0.7 parts of 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine,

[0051] Polysiloxane 0.7 parts.

[0052] Wherein, the particle size of the nano boron nitride powder is 200-300 nm.

[0053] Wherein, the structural formula of the polyetheretherketone is: The molecular weight is 800,000 to 1,000,000 and the melt viscosity is 140 to 160 Pa.s.

[0054] A method for preparing a high-temperature PEEK composite material for antenna-type LDS functional laser engraving, comprising the following steps:

[0055] (1) Weigh the components in proportion for later use;

[0056] (2) Pour the components into a stirring device and stir them evenly, then send them into a single screw extruder, and obtain a polycarbonate composite material PEEK composite material through melting, mixing and extrusion.

[0057] Among them, the set temperatures of the single-screw extruder are: section one: 325°C, section two: 330°C, section three: 335°C, section four: 345°C, section five: 355°C, section six: 325°C, section seven: 325°C, section eight: 330°C, section nine: 335°C, and die head: 345°C.

[0058] Wherein, the rotation speed of the single screw extruder is 300 rpm.

[0059] Example 2

[0060] A high-temperature PEEK composite material for LDS functional laser engraving of antennas, comprising the following components by weight:

[0061] 98 parts of polyetheretherketone resin,

[0062] Copper nanoparticles coated with CaTiO 3 4 parts powder,

[0063] 3 parts of nano boron nitride powder,

[0064] 0.8 parts of 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine,

[0065] Polysiloxane 0.8 parts.

[0066] Wherein, the particle size of the nano boron nitride powder is 200-300 nm.

[0067] Wherein, the structural formula of the polyetheretherketone is: The molecular weight is 800,000 to 1,000,000 and the melt viscosity is 140 to 160 Pa.s.

[0068] A method for preparing a high-temperature PEEK composite material for antenna-type LDS functional laser engraving, comprising the following steps:

[0069] (1) Weigh the components in proportion for later use;

[0070] (2) Pour the components into a stirring device and stir them evenly, then send them into a single screw extruder, and obtain a polycarbonate composite material PEEK composite material through melting, mixing and extrusion.

[0071] Among them, the set temperatures of the single-screw extruder are: section one: 335°C, section two: 340°C, section three: 345°C, section four: 355°C, section five: 365°C, section six: 335°C, section seven: 335°C, section eight: 340°C, section nine: 345°C, and die head: 355°C.

[0072] Wherein, the rotation speed of the single screw extruder is 350rmp.

[0073] Example 3

[0074] A high-temperature PEEK composite material for LDS functional laser engraving of antennas, comprising the following components by weight:

[0075] 97 parts of polyetheretherketone resin,

[0076] Copper coated nano-CaTiO 3 4 parts powder,

[0077] 2 parts of nano boron nitride powder,

[0078] 0.8 parts of 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine,

[0079] Polysiloxane 0.7 parts.

[0080] Wherein, the particle size of the nano boron nitride powder is 200-300 nm.

[0081] Wherein, the structural formula of the polyetheretherketone is: The molecular weight is 800,000 to 1,000,000 and the melt viscosity is 140 to 160 Pa.s.

[0082] A method for preparing a high-temperature PEEK composite material for antenna-type LDS functional laser engraving, comprising the following steps:

[0083] (1) Weigh the components in proportion for later use;

[0084] (2) Pour the components into a stirring device and stir them evenly, then send them into a single screw extruder, and obtain a polycarbonate composite material PEEK composite material through melting, mixing and extrusion.

[0085] Among them, the set temperatures of the single-screw extruder are: section one: 330°C, section two: 335°C, section three: 340°C, section four: 350°C, section five: 360°C, section six: 330°C, section seven: 330°C, section eight: 335°C, section nine: 340°C, and die head: 350°C.

[0086] Wherein, the rotation speed of the single screw extruder is 320 rpm.

[0087] Comparative Example 1

[0088] Comparative Example 1 is basically the same as Example 3, except that no copper-coated nano-CaTiO 3 powder, but adding nano-CaTiO 3 powder.

[0089] Comparative Example 2

[0090] Comparative Example 2 is substantially the same as Example 3, except that no nano boron nitride powder is added in Comparative Example 2.

[0091] The properties of the high-temperature PEEK composite materials prepared in Examples 1-3 and Comparative Examples 1-2 were tested.

[0092] The high-temperature PEEK composite material prepared in Examples 1-3 and Comparative Examples 1-2 was made into a planar substrate, including selectively engraving a pattern on the surface of the substrate using a laser; and placing the substrate in a chemical copper plating solution to form a metal coating. The bonding strength between the metal coating and the substrate was tested. The bonding strength between the coating and the substrate was tested using a scratch test method, and the dielectric constant, dielectric loss factor, and wave transmission were measured according to industry standards in the communication field. The specific test data are recorded in Table 1.

[0093] Table 1

[0094]

[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A high-temperature PEEK composite material for LDS functional laser engraving of antennas, characterized in that: By weight, it includes the following components: 95-100 parts of polyetheretherketone resin, 2-5 parts of copper-coated nano-CaTiO3 powder, 1-3 parts of nano boron nitride powder, 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine 0.5-1 part, 0.5 to 1 part of polysiloxane.

2. The high temperature PEEK composite material according to claim 1, characterized in that: By weight, it includes the following components: 97-98 parts of polyetheretherketone resin, 3-4 parts of copper-coated nano-CaTiO3 powder, 2-3 parts of nano boron nitride powder, 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine 0.7-0.8 parts, Polysiloxane 0.7-0.8 parts.

3. The high temperature PEEK composite material according to claim 1, characterized in that: By weight, it is composed of the following components: 97-98 parts of polyetheretherketone resin, 3-4 parts of copper-coated nano-CaTiO3 powder, 2-3 parts of nano boron nitride powder, 1,3,5-tris(3,5-di-tert-butyl, 4-hydroxybenzyl)-s-triazine 0.7-0.8 parts, Polysiloxane 0.7-0.8 parts.

4. The high temperature PEEK composite material according to any one of claims 1 to 3, characterized in that: The preparation steps of the copper-coated CaTiO3 powder are as follows: immersing the nano-CaTiO3 powder in a 50-60 g / L copper nitrate solution, filtering, drying, placing in a quartz furnace, sealing and evacuating; then introducing argon gas and heating to a preset temperature, introducing hydrogen gas after the temperature stabilizes; maintaining for a certain time; and stopping introducing gas after cooling to room temperature; The particle size of the nano-CaTiO3 powder is 200-300nm, and the particle size of the copper-coated CaTiO3 powder is 400-500nm.

5. The high temperature PEEK composite material according to claim 4, characterized in that: The preset temperature is 280-350° C., the argon flow rate is 100-150 sccm, the hydrogen flow rate is 200-300 sccm, and the reaction time is 30-45 min.

6. The high temperature PEEK composite material according to any one of claims 1 to 3, characterized in that: The particle size of the nano boron nitride powder is 200-300 nm.

7. The high temperature PEEK composite material according to any one of claims 1 to 3, characterized in that: The structural formula of the polyetheretherketone is: The molecular weight is 800,000 to 1,000,000 and the melt viscosity is 140 to 160 Pa.s.

8. The high temperature PEEK composite material according to any one of claims 1 to 3, characterized in that: The PEEK composite material has a dielectric constant of 2.6-2.9, a dielectric loss of 0.005-0.008, and a wave transmittance greater than 96%.

9. A method for preparing a high-temperature PEEK composite material for antenna-type LDS functional laser engraving as claimed in any one of claims 1 to 8, comprising the following steps: (1) Weigh the components in proportion for later use; (2) pouring each component into a stirring device and stirring them evenly, and then sending them into a single screw extruder, melting, mixing, and extruding to obtain a polycarbonate composite material PEEK composite material; The temperature setting of the single screw extruder is: first section: 325-335°C, second section: 330-340°C, third section: 335-345°C, fourth section: 345-355°C, fifth section: 355-365°C, sixth section: 325-335°C, seventh section: 325-335°C, eighth section: 330-340°C, ninth section: 335-345°C, die head: 345-355°C; The rotation speed of the single screw extruder is 300-350 rpm.

10. An antenna comprising a matrix of the high temperature PEEK composite material according to any one of claims 1 to 8.