Ceramic coating and non-stick appliance comprising same
By using disordered porous or layered structures of sustained release particles and silicone oil in ceramic coatings, the problem of insufficient durable performance of ceramic coatings is solved, and the long-term non-stick effect of ceramic coatings is achieved, which is suitable for high temperatures and Non-stick appliances under wear conditions.
Patent Information
- Application Number
- CN202310649340.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The long-lasting non-stick properties of ceramic coatings are insufficient, resulting in a short service life of non-stick devices, which cannot meet consumers' non-stick needs for high-temperature cooking and wear conditions.
In ceramic coatings, the silicone oil is added with disordered porous or layered structures. The silicone oil is combined with the surface or pores of the sustained release material, and the release of the silicone oil is slowed down by the sustained release particles to form a long-lasting non-stick coating.
It significantly improves the long-lasting non-stick properties of ceramic coatings and extends the non-stick effect. It is suitable for high-temperature cooking and wear conditions.
Smart Images

Figure CN119060566A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of non-stick coatings, and in particular relates to a ceramic coating and a non-stick utensil comprising the same. Background Art
[0002] Currently, non-stick technologies mainly include PTFE coatings and ceramic coatings. Ceramic coatings are very limited in use due to their short non-stick lifespan. They are far less widely used than PTFE products and cannot meet consumers' daily demand for non-stick utensils. For example, non-stick pans will stick to the pan after about one month of use in an average household, especially in high-temperature cooking methods such as Chinese cooking, and under the condition of wear and tear of metal spatulas, the non-stick properties decay very quickly.
[0003] Therefore, improving the long-lasting non-stick properties of ceramic coatings has become a very meaningful and urgent technical need. Summary of the invention
[0004] Based on the above-mentioned deficiencies in the prior art, the present invention provides a ceramic coating formed by using a ceramic coating and a non-stick utensil comprising the same.
[0005] According to one aspect of the exemplary embodiment, a ceramic coating comprises: a ceramic coating precursor; slow-release particles dispersed in the ceramic coating precursor, wherein the slow-release particles comprise a slow-release material and silicone oil bound to the slow-release material, and
[0006] The sustained-release material comprises at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.
[0007] The particle size of the sustained-release particles may be less than or equal to 20 microns.
[0008] The particle size of the sustained-release particles may be less than or equal to 15 microns.
[0009] The ceramic coating may include a single layer, and the thickness of the single layer may be in the range of 10 microns to 80 microns.
[0010] The ceramic coating may include at least two sub-layers, and at least an uppermost sub-layer of the at least two sub-layers may include slow-release particles.
[0011] The thickness of each sub-layer may be no less than 10 micrometers, and the sum of the thickness of each sub-layer may be no more than 80 micrometers.
[0012] The content of the sustained-release particles included in each sub-layer may be different from each other.
[0013] The ceramic coating may be applied on a substrate, and the content of the slow-release particles in each sub-layer may increase in a direction away from the substrate.
[0014] The particle sizes of the sustained-release particles included in each sub-layer of the ceramic coating may be different from each other.
[0015] According to another aspect of the exemplary embodiment, a non-stick utensil includes the ceramic coating as described above.
[0016] The present invention forms a ceramic coating by adding a ceramic coating formed by slow-release particles including a slow-release material to a ceramic coating precursor. Since the slow-release material in the ceramic coating has a disordered porous structure, silicone oil is adsorbed and bonded on the surface and in the pores of the slow-release material. The ceramic coating formed by the ceramic coating has a silicone oil slow-release effect, thereby improving the long-lasting non-stick performance of the ceramic coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a schematic diagram showing a first embodiment of a ceramic coating according to an exemplary embodiment;
[0018] Figure 2 is a schematic enlarged view showing slow-release particles in a ceramic coating according to an exemplary embodiment;
[0019] Figure 3 is a schematic diagram showing a second embodiment of a ceramic coating according to an exemplary embodiment;
[0020] Figure 4 is a schematic diagram showing a third embodiment of a ceramic coating according to an exemplary embodiment;
[0021] Figure 5 is a schematic diagram illustrating a fourth embodiment of a ceramic coating according to an exemplary embodiment. DETAILED DESCRIPTION
[0022] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which embodiments are shown. However, the present invention may be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that the disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. The same reference numerals refer to the same elements throughout.
[0023] Ceramic coatings achieve non-stick properties mainly through the use of silicone methyl and doped silicone oil in the ceramic coating. As the product is heated and worn during use, the silicone oil in the coating will gradually be lost, destroying the silicone methyl groups on the surface, resulting in the loss of the non-stick effect, and finally the phenomenon of sticking to the pan when cooking. If the ceramic coating can store oil continuously, it can form an effective oil film to isolate the food and the coating surface, thereby achieving long-lasting non-stick properties.
[0024] Therefore, the present invention provides a ceramic coating, which includes slow-release particles having a slow-release material, wherein the slow-release material may have a disordered porous and / or layered structure, and silicone oil is combined (e.g., adsorbed, bonded) to the slow-release material. During the cooking process, the slow-release particles in the ceramic coating can slow down the release of silicone oil, so that the ceramic coating can maintain a long-lasting non-stick effect.
[0025] Figure 1 is a schematic diagram showing a first embodiment of a ceramic coating according to an exemplary embodiment, Figure 2 is a schematic diagram showing a slow-release particle in a ceramic coating according to an exemplary embodiment. Figure 1 and Figure 2 A first embodiment of the inventive concept will be described.
[0026] Reference Figure 1 and Figure 2 As shown, a ceramic coating 200 according to a first exemplary embodiment of the present inventive concept is applied on a substrate 100. The ceramic coating 200 is formed using a ceramic coating, and includes a ceramic coating precursor 1 and slow-release particles 2 dispersed in the ceramic coating precursor.
[0027] According to an exemplary embodiment, the substrate 100 may be a substrate known in the art for making cookware, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, a titanium substrate, etc. However, the present invention does not limit the material, use, and other properties of the substrate, that is, those skilled in the art may use any material on which a ceramic coating is to be applied as the substrate 100 as needed, so that the non-stick utensil of the present invention may be applicable to any scene requiring non-stick (such as a non-stick coating of a cooking pot (e.g., a frying pan, an inner pot of an electric rice cooker), an inner and outer coating of a transport pipeline, etc.).
[0028] The ceramic coating precursor 1 as the base layer of the ceramic coating may be a ceramic coating used in the art. However, the exemplary embodiment is not limited thereto, as mentioned in the method for manufacturing a ceramic coating using a ceramic coating according to the present inventive concept described below in conjunction with the exemplary embodiment, the ceramic coating precursor 1 may be a ceramic coating precursor prepared by the method of the present inventive concept.
[0029] The slow-release particles 2 dispersed in the ceramic coating precursor 1 include a slow-release material 21 and silicone oil 22 bound to the slow-release material.
[0030] According to an exemplary embodiment, the slow-release material 21 may have a layer gap and / or a pore structure, so that the silicone oil 22 may be, for example, bonded to the surface of the slow-release material and / or adsorbed in the pore and / or layer gap structure. According to an example, the slow-release material 21 may include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material 21 has a porous and / or layered structure and is combined with silicone oil, so that the silicone oil 22 combined with the slow-release material 21 can be slowly released during the use of the cookware with the non-stick coating formed by the ceramic coating of the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick coating formed by the ceramic coating.
[0031] According to an exemplary embodiment, the silicone oil 22 is combined (e.g., adsorbed, bonded) to the sustained-release material 21. And provides the main non-stickiness for the ceramic coating. Here, the silicone oil 22 can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil and polyether modified silicone oil. In addition, by weight percentage, the silicone oil 22 can include 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil, wherein the molecular weight of the low molecular weight silicone oil can be between 500-1000, the molecular weight of the medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of the high molecular weight silicone oil can be between 12000-30000. Here, the silicone oil 22 can be prepared by mixing different molecular weights, because: the silicone oil with a large molecular weight is more firmly bonded to the sustained-release material and the release speed is slower; the silicone oil with a small molecular weight has better free mobility, thereby having better non-stickiness; in addition, the silicone oil with a medium molecular weight takes into account both free mobility and bonding firmness. Therefore, by combining low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil, the sustained release and non-stick effects can be better exerted.
[0032] In addition, in order to improve the bonding strength between the silicone oil and the sustained-release material, a coupling agent may be provided between the sustained-release material and the silicone oil. Here, the coupling agent may include a silane coupling agent. However, the exemplary embodiment is not limited thereto, and the coupling agent may be omitted.
[0033] Preferably, the particle size of the sustained-release particles according to the exemplary embodiment may be less than or equal to 20 microns, preferably, may have a size less than or equal to 15 microns, and the particle size of the sustained-release particles may obey a normal distribution. This is because an excessively large particle size (e.g., greater than 20 microns) is likely to have a large impact on the appearance of the formed non-stick coating.
[0034] According to an exemplary embodiment, the content of the slow-release particles in the ceramic coating may include 5.15-32.97 parts by weight of the slow-release particles per 100 parts by weight of the ceramic coating 200 (i.e., when the ceramic coating is manufactured using the ceramic coating, 5.15-32.97 parts by weight of the slow-release particles may be included per 100 parts by weight of the ceramic coating). This is because when there is too much ceramic coating precursor, the content of the slow-release particles is relatively small, so the slow-release effect is poor, but when the content of the slow-release particles is relatively large, the strength and bonding force of the coating will be reduced.
[0035] Figure 1 A single-layer ceramic coating 200 is shown as being applied on a substrate 100, however, the exemplary embodiment is not limited thereto. Figure 3-Figure 5 As shown in , the ceramic coating may also include at least two layers (eg, two layers, three layers, etc.) of ceramic coating.
[0036] In addition, when the ceramic coating 200 is a single layer, the single layer of the ceramic coating 200 may have a thickness in the range of 10 micrometers to 80 micrometers. This is because when the thickness of the ceramic coating 200 is less than 10 micrometers, the wear resistance is insufficient and the ceramic coating is easily worn out; on the contrary, when the thickness of the ceramic coating is greater than 80 micrometers, the coating becomes loose, thereby reducing the impact strength.
[0037] Above, combined Figure 1 and Figure 2 The case where the ceramic coating 200 is a single layer is described, and in the following, reference will be made to Figure 3-Figure 5 The case where the ceramic coating 200 includes a plurality of sub-layers will be described.
[0038] Figure 3 is a schematic diagram showing a second embodiment of a ceramic coating according to an exemplary embodiment; Figure 4 is a schematic diagram showing a third embodiment of a ceramic coating according to an exemplary embodiment; Figure 5 is a schematic diagram showing a fourth embodiment of a ceramic coating according to an exemplary embodiment. Figures 3 to 5 In the figure, the ceramic coating 200 includes a first sublayer 201 and a second sublayer 202 . Figure 3 , Figure 4 and Figure 5 There are differences between them in the content and size of the sustained-release particles.
[0039] Reference Figure 3 , the ceramic coating 200 according to the second exemplary embodiment of the present inventive concept may include a first sub-layer 201 and a second sub-layer 202, where the first sub-layer 201 and the second sub-layer 202 may be the same as the reference Figure 1 The ceramic coating 200 described has the same structure, that is, each of the first sublayer 201 and the second sublayer 202 includes a matrix containing a ceramic material and slow-release particles dispersed in the matrix, and the size of the slow-release particles included in each sublayer is the same or not much different. In addition, each of the first sublayer 201 and the second sublayer 202 can have a thickness of not less than 10 microns, and the thickness difference between the first sublayer and the second sublayer is not particularly limited. For example, the first sublayer 201 can have a thickness of 20 microns, and the second sublayer can have a thickness of 30 microns, 40 microns or 50 microns. In addition, when multiple sublayers (for example, three, four, etc.) are provided, the sum of the thicknesses of the multiple sublayers can be less than or equal to 80 microns.
[0040] According to an exemplary embodiment, the first sublayer 201 and the second sublayer 202 may each include different contents of slow-release particles (i.e., the number of slow-release particles included in the sublayer per unit weight, for example, the density of the slow-release particles in the sublayer), and the content of the slow-release particles in the first sublayer 201 may be lower than the content of the slow-release particles in the second sublayer 201. That is, when a plurality of (e.g., two, three, four) sublayers are provided, the content of the slow-release particles included in each sublayer may increase in the direction away from the substrate 100. Furthermore, although the attached Figure 3 2 shows that the content of the slow-release particles included in the first sublayer 201 is less than the content of the slow-release particles included in the second sublayer 202, but the exemplary embodiment is not limited thereto. In other embodiments, the first sublayer may also include very few slow-release particles or no slow-release particles.
[0041] In addition, when the ceramic coating includes multiple sublayers (for example, two or three), the content of the sustained-release particles included in at least the topmost sublayer can be 5.15-32.97 parts by weight of sustained-release particles dispersed in every 100 parts by weight of the sublayer, and there is no specific limitation on the content (for example, density) of the sustained-release particles included in the sublayer disposed therebelow.
[0042] For example, when the ceramic coating includes two sublayers, the content of the slow-release particles arranged in the lower sublayer 201 can be 3 parts by weight of the slow-release particles dispersed in every 100 parts by weight of the sublayer 201, and the content of the slow-release particles arranged in the upper sublayer 202 can be 30 parts by weight of the slow-release particles dispersed in every 100 parts by weight of the sublayer 202.
[0043] For another example, when the ceramic coating includes three sublayers, the content of the slow-release particles arranged in the bottom sublayer may be 2 parts by weight of the slow-release particles dispersed in every 100 parts by weight of the sublayer, the content of the slow-release particles arranged in the middle sublayer may be 3 parts by weight of the slow-release particles dispersed in every 100 parts by weight of the sublayer, and the content of the slow-release particles arranged in the top sublayer may be 25 parts by weight of the slow-release particles dispersed in every 100 parts by weight of the sublayer.
[0044] That is, when a plurality of sublayers are provided, the content of the slow-release particles included in each sublayer may gradually (e.g., a gradient) increase in the direction away from the substrate 100 and satisfy that the sublayer (e.g., 202) provided at the top has 5.15-32.97 parts by weight of slow-release particles dispersed in every 100 parts by weight of the sublayer, or that the sublayers provided at the bottom of the top sublayer (e.g., 202) have the same or different content of slow-release particles that is less than the content of slow-release particles in the top sublayer (e.g., 202) and the top sublayer has 5.15-32.97 parts by weight of slow-release particles dispersed in every 100 parts by weight of the sublayer. That is, the content of slow-release particles in each sublayer provided at the bottom of the top sublayer is limited to a content of slow-release particles dispersed in every 100 parts by weight of the corresponding sublayer that is less than the content of slow-release particles distributed in the top sublayer having a range of 5.15-32.97 parts by weight of slow-release particles.
[0045] Reference Figure 4 , the ceramic coating according to the third embodiment and Figure 3 The ceramic coating of the second embodiment is different only in that the size of the slow-release particles included in the first sub-layer 201 is different from the size of the slow-release particles included in the second sub-layer. Figure 4 As shown in , the size of the slow-release particles included in the first sublayer 201 is smaller than the size of the slow-release particles included in the second sublayer 202. For example, the size of the slow-release particles included in the first sublayer 201 can be less than or equal to 11 microns and obey the normal distribution, while the size of the slow-release particles included in the second sublayer can be less than or equal to 15 microns and obey the normal distribution. Here, the size of almost all (most of) the slow-release particles included in each sublayer can not exceed 20 microns, and the slow-release particles included in the uppermost sublayer (e.g., 202) can have the optimal particle size.
[0046] Reference Figure 5 , the ceramic coating according to the fourth embodiment and Figure 4 The ceramic coatings of the three embodiments differ only in that the content of the slow-release particles included in each sub-layer is the same. That is, Figure 5In the fourth embodiment, the content of the sustained-release particles in the first sublayer 201 is the same as the content of the sustained-release particles in the second sublayer 202 , but the size of the sustained-release particles in the first sublayer 201 is smaller than that of the sustained-release particles in the second sublayer 202 .
[0047] Above, the ceramic coating according to the inventive concept is described in detail in conjunction with exemplary embodiments, and hereinafter, a method of manufacturing the ceramic coating will be described in detail.
[0048] The method of manufacturing a ceramic coating according to the inventive concept may include: providing a substrate 100 and a ceramic coating; and forming a ceramic coating 200 on the substrate 100 using the ceramic coating by a laying process.
[0049] According to an exemplary embodiment, the substrate 100 may be a substrate known in the art for making cookware, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, a titanium substrate, etc., and the present invention does not limit the material and other properties of the substrate. That is, those skilled in the art may use any material on which a ceramic coating is to be applied as the substrate 100 as needed, so that the non-stick utensil of the present invention can be applied to any scene requiring non-stick.
[0050] A ceramic coating may be provided before, during or after providing the substrate. According to an exemplary embodiment, the ceramic coating may include a ceramic coating precursor and slow-release particles dispersed in the ceramic coating. Therefore, the step of providing the ceramic coating may include the steps of separately preparing the ceramic coating precursor and the slow-release particles and mixing the ceramic coating precursor with the slow-release particles to obtain the ceramic coating. However, the exemplary embodiments are not limited thereto, that is, the step of preparing the ceramic coating precursor may be combined with the step of preparing the slow-release particles. Below, a method for preparing a ceramic coating according to the present invention by separately preparing a ceramic coating precursor and slow-release particles will be mainly described.
[0051] Preparation of ceramic coating precursors
[0052] According to an exemplary embodiment, the step of preparing the ceramic coating precursor may include a step of providing materials and a step of mixing.
[0053] The step of providing materials may include the steps of separately providing A material, B material and C material.
[0054] Here, material A may include a silane substance, material B may include silica sol and filler as essential components, optional pigments, wetting agents, thickeners and emulsifiers as unnecessary components, and a solvent, and material C may include an organic acid as an essential component, and optional pH buffers and catalysts (zirconium acetate) as unnecessary components.
[0055] In the A material, according to an exemplary embodiment, the silane substance is used to form polysiloxane during the formation of the ceramic coating, and therefore, the silane substance here may include a substance known in the art for polycondensation to form polysiloxane. According to an exemplary embodiment, the silane substance may include at least one of methyltrimethoxysilane, methyltriethoxysilane, and dimethyldimethoxysilane, but is not limited thereto. In addition, in addition to the silane substance, the A material may also include tetraethyl orthosilicate that is polycondensed to form polysiloxane, and in this case, in the A material, by weight percentage, the silane substance may account for 80%-97% of the A material, and the tetraethyl orthosilicate may account for 3%-20% of the A material.
[0056] Material B may necessarily include fillers and silica sol. The filler plays a role in increasing the wear resistance of the coating, etc. Therefore, the present invention does not limit the type of filler, and ordinary commonly used fillers can be selected, for example, at least one of mica powder, kaolin, montmorillonite, silicon carbide, alumina and silicon dioxide can be selected. In addition, silica sol is the main film-forming substance of ceramic coatings, which reacts with polysiloxane under acidic conditions to form a ceramic coating. Therefore, commercially available ordinary silica sol can be selected as the silica sol in material B of the present invention. For example, the silica sol can be Akzo Nobel 1050 (silica sol) or American Grace LUDIXAM-50.
[0057] The necessary components in the B material can be dispersed in a solvent. That is, the B material can also include a solvent. Here, the solvent can include deionized water, and in order to adjust the volatilization rate of the solvent during the coating drying process, the solvent can also include isopropanol. In addition, the ratio between isopropanol and water is unlimited, and the ratio between water and isopropanol can be selectively proportioned according to actual needs.
[0058] In the B material, in addition to the above-mentioned necessary components, one or more of a pigment, a wetting agent, a thickener and an emulsifier may be selectively included as an unnecessary component. Here, the pigment is mainly used to give the coating different colors, so ordinary inorganic pigments can be selected. Inorganic pigments have good temperature resistance and good safety, and inorganic pigments are preferably selected in the high temperature resistant field. According to an exemplary embodiment, at least one of carbon black, copper chrome black, titanium dioxide, iron oxide, etc. may be selected as a filler. In addition, during the preparation of the necessary components in the solvent, in order to provide the excellent properties of the material, at least one of a wetting agent, a thickener and an emulsifier may also be added to the material.
[0059] According to a specific example, the B material may include, by weight percent: 30wt%-48wt% of silica sol, 8wt%-13wt% of pigment, 8wt%-25wt% of filler, 0.2wt%-1wt% of wetting agent, 1wt%-3wt% of thickener, 3wt%-5wt% of emulsifier, and the balance is isopropyl alcohol and deionized water. However, exemplary embodiments are not limited thereto, and one or more of the unnecessary components may be omitted.
[0060] The C material is used as a strong acid catalyst, and may include an organic acid as an essential component, and an optional pH buffer and a catalyst (e.g., zirconium acetate) as an unnecessary component. Here, the organic acid is used to adjust the pH value of the silica sol in the subsequent process so that it can react with the A material in an acidic environment, and therefore, an organic acid commonly used in the art for ceramic coatings can be used. According to an exemplary embodiment, at least one of formic acid and acetic acid can be selected as an organic acid, and when both formic acid and acetic acid are included, the weight ratio between formic acid and acetic acid can be between 4:6 and 1:1. In addition, in the C material, a pH buffer and a catalyst may also be selectively included. Here, the pH buffer and the catalyst may be a pH buffer and a catalyst used in the process of preparing a strong acid catalyst for ceramic coatings known in the art, for example, the pH buffer may be a weak acid such as boric acid, and the catalyst is used to accelerate the reaction rate of the sol-gel, and may be zirconium acetate, etc. However, the exemplary embodiment is not limited to the types of pH buffers and catalysts, and suitable pH buffers and catalysts may be omitted or appropriately selected based on the prior art.
[0061] According to an exemplary embodiment, the C material may include 80-97 parts by weight of a mixture of formic acid and acetic acid, 1-2 parts by weight of a boric acid pH buffer, and 0.5 parts by weight of a zirconium acetate catalyst.
[0062] After providing the above-mentioned materials, a mixing step may be performed. Herein, the mixing step may include a first mixing step of mixing the B material with the C material to obtain the first material and a second step of mixing the result of the first mixing step (ie, the first material) with the A material.
[0063] Specifically, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidic (e.g., less than or equal to 4) by using the acidity of the C material to obtain the first material. Since the C material includes a solid filler and an optional pigment, the C material can be added to a grinder and ground for 0.5h-2h before mixing or during the preparation of the C material, so that it is fully dispersed and ground to a particle size of less than or equal to 15 microns to obtain a uniformly dispersed slurry.
[0064] After the B material and the C material are mixed, the mixture may be tumbling dispersed for a predetermined time (eg, 0.5 h) so that the first material has a high degree of dispersion.
[0065] After obtaining the first material, material A may be added to the first material. Here, the weight ratio of the added amount of material A to material B may be in the range of (20-30):(40-60). After adding material A, the mixture may be shaken evenly so that material A and material B undergo a sol-gel reaction in an acidic environment to form a ceramic coating precursor.
[0066] Preparation of sustained-release granules
[0067] During, before, or after the preparation of the ceramic coating, the slow-release particles can be prepared. The slow-release particles can be prepared by mixing the slow-release material with silicone oil.
[0068] According to an exemplary embodiment, the sustained-release particles may include the Figure 1 and Figure 2 The described sustained-release material 21 has a pore structure and / or a layer structure and the silicone oil 22 is combined with (eg, adsorbed, bonded to) the sustained-release material.
[0069] A slow-release material precursor of appropriate size (i.e., a slow-release material before grinding, when the grinding step is omitted, the slow-release material precursor can be considered as the slow-release material used in the end) can be selected to prepare slow-release particles. According to an exemplary embodiment, the slow-release material precursor can have a layer gap and / or pore structure. According to the example, the slow-release material precursor can include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material precursor has a porous and / or layered structure and the slow-release material formed after grinding is combined with silicone oil. The silicone oil combined with the slow-release material can be slowly released during the use of an appliance such as a non-stick coating formed by the ceramic coating conceived by the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick layer formed by the ceramic coating.
[0070] According to an exemplary embodiment, the particle size of the slow-release material precursor may be in the range of 100 meshes to 3000 meshes, and the particle size of the slow-release material precursor within this range may obey a normal distribution. However, when the particle size is too large (e.g., less than 100 meshes), the excessively large particle size is likely to increase the grinding process or make the particle size of the slow-release material after grinding too large, ultimately affecting the appearance of the non-stick coating made using the ceramic coating; on the contrary, the particle size is too small (e.g., greater than 3000 meshes, and the particle size will be smaller after grinding) It is not easy to effectively adsorb and bond silicone oil, and thus it is not easy to achieve a good silicone oil slow-release effect.
[0071] When the slow-release material precursor has the above-mentioned particle size distribution, the particle size of the slow-release material finally obtained can be made to be less than 20 microns by using two grinding processes as described below. However, the exemplary embodiment is not limited thereto, that is, when the slow-release material precursor is selected to have a smaller value within the range of 100 mesh-3000 mesh, one grinding process can be omitted; in addition, when the particle size of the slow-release material precursor is selected to have a smaller value within the above-mentioned range, two grinding processes can be omitted. When at least one of the grinding processes is omitted, the omitted grinding process can be replaced by a stirring process, or no treatment can be performed on the mixture.
[0072] Silicone oil can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, and polyether modified silicone oil, and can be mixed by silicone oils of different molecular weights in a certain proportion to form a silicone oil composition with a molecular weight normal distribution; wherein, by weight percentage, the content of low molecular weight silicone oil can be 20wt%-30wt%, the content of medium molecular weight silicone oil can be 40wt%-60wt%, and the content of high molecular weight silicone oil can be 20wt%-30wt%. Here, the molecular weight of low molecular weight silicone oil can be between 500-1000, the molecular weight of medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of high molecular weight silicone oil can be between 12000-30000. By utilizing a normally distributed silicone oil composition, the sustained release and non-stick effects can be better exerted. This is because: the large molecular weight silicone oil is more firmly bonded to the sustained release material and the release speed is slower; the free mobility of small molecular weight silicone oil is better, so it has better non-stickiness; in addition, the medium molecular weight silicone oil takes into account both free mobility and bonding firmness. Therefore, low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil can be combined to better exert the sustained release and non-stick effects.
[0073] According to an example, 35-58 parts by weight of a slow-release material precursor can be mixed with 42-60 parts by weight of silicone oil to obtain a mixture, and 1-3 parts by weight of a coupling agent (e.g., a methoxysilane coupling agent), 0.3 parts by weight of a catalyst (e.g., a titanate catalyst), and 1-1.5 parts by weight of a dispersant can be added to the mixture. However, exemplary embodiments are not limited thereto, and the coupling agent and the catalyst are used to enhance the bonding force between the silicone oil and the slow-release material, and the dispersant is used to improve the dispersion of the slow-release material in the silicone oil. However, exemplary embodiments are not limited thereto, and at least one of the coupling agent, the catalyst, and the dispersant can be omitted.
[0074] According to a specific example, silicone oil, a slow-release material precursor of 100 meshes-3000 meshes, and a silane coupling agent can be mixed evenly, and after grinding to a particle size of less than or equal to 30 microns, a catalyst is added, and the particle size is continued to be less than or equal to 20 microns, and then ultrasonic treatment is performed at room temperature for 0.5h-1h, so that slow-release particles can be obtained. Here, firstly, silicone oil is mixed with the slow-release material and then ground to a particle size of less than or equal to 30 microns, so that silicone oil and the slow-release material can be mixed evenly, and thereafter, grinding to a particle size of less than or equal to 20 microns under the condition of a catalyst can make silicone oil fully firmly adsorbed and bonded to its outside by the slow-release material. However, when the particle size of the slow-release material is less than 30 microns, the first grinding can be omitted, and a stirring process can be optionally provided, or a second grinding process can be directly performed. In addition, when the particle size of the slow-release material is less than 20 microns, the second grinding process can be further omitted, and a stirring process can be optionally provided.
[0075] Preparation of ceramic coatings
[0076] After the ceramic coating precursor and the slow-release particles are prepared, the slow-release particles may be mixed with the ceramic coating precursor to prepare a ceramic coating according to an exemplary embodiment.
[0077] For ceramic coatings including slow-release particles of different numbers and / or sizes, slow-release particles of required size and / or number can be selected and added to the ceramic coating, and after the ceramic coating precursor is mixed with the slow-release particles, the mixture can be stirred and reacted at a speed of 120 rpm to 200 rpm for 6 h to 8 h to obtain the required ceramic coating with different particle sizes and / or numbers.
[0078] Although the above describes a method of obtaining a ceramic coating by separately preparing a ceramic coating precursor and slow-release particles and mixing the ceramic coating precursor with the slow-release particles, in a method of combining the step of preparing a ceramic coating precursor with the step of preparing slow-release particles, as described above, after mixing the B material with the C material, the A material and the slow-release particles can be added to the mixture of the B material and the C material at the same time. For example, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, and the pH of the mixture can be adjusted to acidity (e.g., less than or equal to 4) by using the acidity of the C material to obtain the first material. Then, the A material and the slow-release particles can be added to the mixture, and the weight ratio between the A material and the B material can be in the range of (20-30): (40-60). Different addition amounts of the slow-release particles can be adaptively selected based on the requirements of different layers, and when the ceramic coating includes multiple sub-layers, when preparing the ceramic coating required for the top sub-layer, the addition amounts of material A, material B and slow-release particles can be in the range of (20-30): (40-60): (5-30). After mixing, the mixture can be stirred at a speed of 120-200 rpm for 6h-8h to obtain the desired various ceramic coatings.
[0079] After obtaining the ceramic material, the ceramic coating can be sprayed by air spraying; the air spraying parameters are as follows: the spraying distance is 160 mm; the air pressure is 0.3 MPa; the flow rate is 8 L / min. In addition, when multiple sub-layers are provided, the above spraying parameters can be applied to any sub-layer. In addition, the method of forming the ceramic coating is not limited to air spraying, and various suitable methods of forming layers in the art can be used.
[0080] After air spraying, a single-layer ceramic coating or a ceramic coating having multiple sub-layers can be formed on the substrate.
[0081] According to an exemplary embodiment, when a single ceramic coating layer 200 is provided, 5.15-32.97 parts by weight of the sustained-release particles may be dispersed per 100 parts by weight of the ceramic coating layer 200 . In addition, when multiple sublayers (for example, 201, 202) are provided, the content of the slow-release particles included in each sublayer can gradually (for example, gradient) increase in the direction away from the substrate 100 and satisfy the requirement that the sublayer provided at the top (for example, 202) has 5.15-32.97 parts by weight of slow-release particles dispersed in every 100 parts by weight of the sublayer, or the sublayers provided below the top sublayer (for example, 202) have the same or different contents of slow-release particles that are less than the content of the slow-release particles in the top sublayer (for example, 202) and the top sublayer has 5.15-32.97 parts by weight of slow-release particles dispersed in every 100 parts by weight of the sublayer, that is, the content of the slow-release particles in each sublayer provided below the top sublayer is not limited to the range of 5.15-32.97 parts by weight of slow-release particles dispersed in every 100 parts by weight of the sublayer (for example, 201).
[0082] Through the detailed description in combination with the exemplary embodiments above, the ceramic coating of the present invention includes slow-release particles, and therefore, during the cooking process, the release of silicone oil can be slowed down, thereby maintaining a long-lasting non-stick effect.
[0083] Hereinafter, the beneficial effects of the inventive concept will be described with reference to specific examples.
[0084] Example 1
[0085] The ceramic coating is formed by the following method.
[0086] S1: 80 wt % of methyltrimethoxysilane and 20 wt % of ethyl orthosilicate are mixed and stirred uniformly to obtain a silane composition of component A;
[0087] S2: 30wt% of Akzo Nobel 1050 (silica sol), 8wt% of titanium dioxide (pigment), 25wt% of kaolin (filler), 3wt% of Tween-80 (emulsifier), 1wt% of water-based modified bentonite (thickener), 0.3wt% of polyoxyethylene ether TRITON X-100 (wetting agent), 20wt% of isopropanol and the balance of deionized water were mixed evenly, then added to a grinder and ground for 2h, fully dispersed and ground to a particle size of not more than 15 microns, to obtain component B slurry;
[0088] S3: 48 parts by weight of formic acid, 48 parts by weight of acetic acid, 1 part by weight of boric acid (buffer), and 0.5 parts by weight of zirconium acetate (catalyst) are uniformly mixed to obtain component C strong acid catalyst;
[0089] S4: 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 and 42 parts by weight of vermiculite (slow-release material) with a particle size of 100 to 3000 meshes are mixed, and then 3 parts by weight of methoxysilane coupling agent are added and mixed evenly, and the mixture is ground to a particle size of no more than 30 microns, and then 0.3 parts by weight of titanate (catalyst) is added, and the mixture is further ground to a particle size of no more than 20 microns, and then ultrasonically treated at room temperature of 22° C. for 0.5 h to obtain a slow-release particle component D, and the particle size of the slow-release particle component D obeys a normal distribution;
[0090] S5: The above four components are mixed in order according to the weight ratio of A: B: C: D = 22: 40: 1: 20, and rolled to mature to obtain the ceramic coating. The mixing order and the maturation method are as follows: first, 40 parts by weight of component B and 1 part by weight of component C are mixed evenly, and the pH is adjusted to 4 by component C, and the mixture is rolled and dispersed for 0.5 hours, and then 22 parts by weight of component A are added and shaken evenly, and then 20 parts by weight of component D are added, and the reaction is stirred at a speed of 200 rpm for 8 hours to obtain the desired ceramic coating.
[0091] The non-stick cookware is manufactured by using the ceramic coating as follows.
[0092] S6: Substrate treatment. The stainless steel substrate is sandblasted with 60# brown corundum to form a surface roughness of 3 microns;
[0093] S7: Preheating. Clean the sandblasted substrate and preheat it to 60°C;
[0094] S8: Spraying. The ceramic coating is sprayed on the substrate by air spraying, and the spraying film thickness is 70 microns; the air spraying parameters are as follows: the spraying distance is 160mm; the air pressure is 0.3MPa; and the flow rate is 8L / min.
[0095] S9: Sintering: Curing at 250°C for 10 minutes.
[0096] Through the above method, the non-stick cookware of Example 1 is obtained.
[0097] Example 2
[0098] The difference from Example 1 is that the sustained-release material is bentonite.
[0099] Example 3
[0100] The difference from Example 1 is that the sustained-release material is alpha alumina.
[0101] Example 4
[0102] The difference from Example 1 is that the particle size of the slow-release particle component is not greater than 15 microns, and the particle size of the slow-release particle component D obeys a normal distribution.
[0103] Example 5
[0104] The difference from Example 1 is that the particle size of the slow-release particle component is not greater than 10 microns, and the particle size of the slow-release particle component D obeys a normal distribution.
[0105] Example 6
[0106] The difference from Example 1 is that the film thickness is 10 microns.
[0107] Example 7
[0108] The difference from Example 1 is that the film thickness is 40 microns.
[0109] Example 8
[0110] The difference from Example 1 is that component A, component B, component C and component D are mixed in sequence according to the weight ratio of A:B:C:D=30:60:2:5.
[0111] Example 9
[0112] The difference from Example 1 is that component A, component B, component C and component D are mixed in sequence according to the weight ratio of A:B:C:D=20:40:1:8.
[0113] Example 10
[0114] The difference from Example 1 is that component A, component B, component C and component D are mixed in sequence according to the weight ratio of A:B:C:D=20:40:1:15.
[0115] Embodiment 11
[0116] The difference from Example 1 is that component A, component B, component C and component D are mixed in sequence according to the weight ratio of A:B:C:D=20:40:1:25.
[0117] Example 12
[0118] The difference from Example 1 is:
[0119] (1) preparing ceramic coating 01 by using step S5;
[0120] (2) further comprising step S51, wherein the step S51 differs from step S5 only in that the components A, B, C and D obtained in steps S1 to S4 are sequentially mixed in a weight ratio of A:B:C:D=22:40:1:1 to prepare ceramic coating 02;
[0121] (3) A first sublayer with a thickness of 25 μm was formed on the substrate using ceramic coating 02 by the air spraying method of Example 1, and a second sublayer with a thickness of 45 μm was formed on the first sublayer using ceramic coating 01 by the air spraying method of Example 1.
[0122] Embodiment 13
[0123] The difference from Example 12 is that the thickness of the first sub-layer is 10 microns.
[0124] Embodiment 14
[0125] The difference from Example 12 is that the thickness of the first sub-layer is 30 microns.
[0126] Embodiment 15
[0127] The difference from Example 12 is that the thickness of the second sub-layer is 10 microns.
[0128] Example 16
[0129] The difference from Example 12 is that the thickness of the second sub-layer is 20 microns.
[0130] Embodiment 17
[0131] The difference from Example 12 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=22:40:1:10 to prepare ceramic coating 02.
[0132] Embodiment 18
[0133] The difference from Example 12 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=22:40:1:30 to prepare ceramic coating 01.
[0134] Embodiment 19
[0135] The difference from Example 1 is:
[0136] (1) preparing ceramic coating 01 by using step S5;
[0137] (2) step S52 is also included, and the difference between step S52 and step S5 is that the components A, B and C obtained in steps S1-S3 are mixed in order according to a weight ratio of A:B:C=22:40:1 to prepare a ceramic coating 03. That is, the difference between step S52 and step S5 is that step S4 is omitted;
[0138] (3) A first sublayer with a thickness of 25 μm was formed on the substrate using ceramic coating 03 by the air spraying method of Example 1, and a second sublayer with a thickness of 45 μm was formed on the first sublayer using ceramic coating 01 by the air spraying method of Example 1.
[0139] Embodiment 20
[0140] The difference from Example 19 is that the thickness of the first sub-layer is 10 microns.
[0141] Embodiment 21
[0142] The difference from Example 19 is that the thickness of the first sub-layer is 30 microns.
[0143] Embodiment 22
[0144] The difference from Example 19 is that the thickness of the second sub-layer is 10 microns.
[0145] Embodiment 23
[0146] The difference from Example 19 is that the thickness of the second sub-layer is 20 microns.
[0147] Embodiment 24
[0148] The difference from Example 19 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=22:40:1:30 to prepare ceramic coating 01.
[0149] Embodiment 25
[0150] The difference from Example 19 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=22:40:1:15 to prepare ceramic coating 01.
[0151] Embodiment 26
[0152] The difference from Example 1 is that the silicone oil is composed of 20 wt % of hydroxy silicone oil with a molecular weight of 800, 60 wt % of hydroxy silicone oil with a molecular weight of 3000 and 20 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0153] Embodiment 27
[0154] The difference from Example 1 is that the silicone oil is composed of 30 wt % of hydroxy silicone oil with a molecular weight of 800, 40 wt % of hydroxy silicone oil with a molecular weight of 3000 and 30 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0155] Embodiment 28
[0156] The difference from Example 1 is that the silicone oil is composed of 25 wt % of hydroxy silicone oil with a molecular weight of 800, 50 wt % of hydroxy silicone oil with a molecular weight of 3000 and 25 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0157] Comparative Example 1
[0158] The difference from Example 1 is that step S4 is omitted. That is, in step S5, components A, B and C are mixed in order according to a weight ratio of A:B:C=22:40:1, and the obtained ceramic material is used to manufacture non-stick cookware.
[0159] Comparative Example 2
[0160] The difference from Example 1 is that 30 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 60 parts by weight of vermiculite.
[0161] Comparative Example 3
[0162] The difference from Example 1 is that 60 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 40 parts by weight of vermiculite.
[0163] Comparative Example 4
[0164] The difference from Example 12 is that the second sublayer is located on the substrate, and the first sublayer is located on the second sublayer.
[0165] The non-stick properties of the non-stick cookware of the above-mentioned Examples 1-28 and Comparative Examples 1-4 were tested, and the test results are shown in the following table.
[0166]
[0167]
[0168] Performance index test
[0169] The above-obtained cookware was subjected to a performance test, and the specific performance test method is as follows:
[0170] (1) Long-lasting non-stick test method: refer to 4.2.1 Fried egg non-stick test in GB_T 32095.2-2015. The unit is the number of times. The higher the number, the longer the life. The non-stick result is evaluated once every 1000 times, and the number of times when the non-stickiness reaches Level III is recorded.
[0171] (2) Plane wear resistance test method: GB_T 32095.2-2015 4.3.1 Plane wear resistance test, use 3M7447 scouring pad, apply a force of 15N, the frequency is 33 times / minute, and the scouring pad is replaced every 500 times.
[0172] By comparing and analyzing the embodiments 1-28 of the present invention and the comparative examples 1-4, it is not difficult to find that: the conventional ceramic coating in comparative example 1 has a long-lasting non-stickiness of no more than 500 times, the silicone oil in comparative example 2 cannot effectively provide a sustained release effect due to its low content, and the sustained release material content in comparative example 3 is too low, and the combined silicone oil is less, and it cannot provide an effective sustained release effect. In addition, in comparative example 4, although it includes two sublayers, the content of the sustained release particles in the uppermost sublayer is lower than the content of the sustained release particles in the lower sublayer, so the test performance of the ceramic coating with a double-layer structure formed is lower than the test performance of the ceramic coating in the embodiment. Compared with comparative examples 1-4, the ceramic coating according to the present invention has excellent long-lasting non-stickiness.
[0173] Although one or more embodiments of the present invention have been described with reference to the drawings, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the claims.
Claims
1. A ceramic coating, characterized in that: The ceramic coating comprises: Ceramic coating precursors; Slow-release particles dispersed in a ceramic coating precursor, wherein: The sustained-release particles include a sustained-release material and silicone oil bound to the sustained-release material, and The sustained-release material comprises at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.
2. The ceramic coating according to claim 1, characterized in that: The particle size of the sustained-release particles is less than or equal to 20 microns.
3. The ceramic coating according to claim 2, characterized in that: The particle size of the sustained-release particles is less than or equal to 15 microns.
4. The ceramic coating according to claim 1, characterized in that The ceramic coating includes a single layer, and a thickness of the single layer is in a range of 10 micrometers to 80 micrometers.
5. The ceramic coating according to claim 1, characterized in that The ceramic coating includes at least two sub-layers, and at least an uppermost sub-layer of the at least two sub-layers includes slow-release particles.
6. The ceramic coating according to claim 5, characterized in that: The thickness of each sub-layer is not less than 10 micrometers, and the sum of the thickness of each sub-layer is not more than 80 micrometers.
7. The ceramic coating according to claim 6, characterized in that The contents of the sustained-release particles included in the respective sub-layers are different from each other.
8. The ceramic coating according to claim 7, characterized in that The ceramic coating is located on a substrate, and the content of the sustained-release particles in each sublayer increases in a direction away from the substrate.
9. The ceramic coating according to claim 1, characterized in that The particle sizes of the sustained-release particles included in each sub-layer of the ceramic coating are different from each other.
10. A non-stick utensil, characterized in that: The non-stick utensil comprises the ceramic coating according to any one of claims 1-9.
Citation Information
Patent Citations
Silicone oil microcapsule with slow-release characteristics and preparation method thereof
CN102030990A
Nano composite ice-covering-proof coating containing phase change silicone oil and preparation method thereof
CN102676056A
Sustained-release silicone oil hydrogel and application thereof in marine antifouling coatings
CN109370287A
Preparation method of slow-release antifouling composite coating with bionic structure
CN113278360A
Modified ceramic coating, composite coating, preparation methods of modified ceramic coating and composite coating, and cooker