Preparation method of ceramic coating and non-stick appliance
By using the combination of sustained release particles and silicone oil in the ceramic coating, a multi-layer structure is formed, which solves the problem of short non-stick life of ceramic coatings, and achieves the long-lasting non-stickness and high-temperature stability of the ceramic coating, and extends the service life.
Patent Information
- Application Number
- CN202310643141.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
The non-stick life of ceramic coatings is not long-lasting and cannot meet consumers' needs for the use of non-stick appliances. Especially under high-temperature cooking and wear conditions, it is easy to stick to the pot.
Using a multi-layer ceramic coating structure, including ceramic coating with sustained release particles, the ceramic coating with gradient sustained release particles is formed by forming a ceramic coating with a gradient sustained release particle content, and the combination of sustained release materials and silicone oil is used to form a disordered porous structure, delaying the release of silicone oil and improving Non-stick properties and bonding power.
It significantly improves the long-lasting non-stick properties and service life of ceramic coatings, ensures long-term non-stick effects under high-temperature cooking conditions, and enhances the bonding force between the ceramic coating and the substrate.
Smart Images

Figure CN119056720A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of non-stick coatings, and in particular relates to a method for preparing a ceramic coating and a non-stick utensil comprising the ceramic coating. Background Art
[0002] Currently, non-stick technologies mainly include PTFE coatings and ceramic coatings. Ceramic coatings are very limited in use due to their short non-stick lifespan. They are far less widely used than PTFE products and cannot meet consumers' daily demand for non-stick utensils. For example, non-stick pans will stick to the pan after about one month of use in an average household, especially in high-temperature cooking methods such as Chinese cooking, and under the condition of wear and tear of metal spatulas, the non-stick properties decay very quickly.
[0003] Therefore, improving the long-lasting non-stick properties of ceramic coatings has become a very meaningful and urgent technical need. Summary of the invention
[0004] Based on the above-mentioned deficiencies of the prior art, the present invention provides a method for forming a ceramic coating using different ceramic coatings and a non-stick utensil including the ceramic coating.
[0005] According to one aspect of an exemplary embodiment, a method for preparing a ceramic coating including a first sublayer and a second sublayer disposed on a substrate includes: preparing a ceramic coating, the ceramic coating including: a first ceramic coating including a ceramic coating precursor and optional slow-release particles; and a second ceramic coating including a ceramic coating precursor and slow-release particles; and using a layer-forming process, forming a first sublayer on the substrate using the first ceramic coating, and forming a second sublayer on the first sublayer using the second ceramic coating, and the content of the slow-release particles included in the first sublayer is different from the content of the slow-release particles included in the second sublayer. The slow-release particles include a slow-release material and silicone oil bound to the slow-release material, and the slow-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate, and layered sulfate.
[0006] The content of the sustained-release particles included in the first sub-layer may be lower than the content of the sustained-release particles included in the second sub-layer.
[0007] The first sub-layer may not include sustained-release particles.
[0008] The content of the sustained-release particles in the first sublayer may be 0 to less than 32.97 parts by weight per 100 parts by weight of the first sublayer, and the content of the sustained-release particles in the second sublayer may be 5.15-32.97 parts by weight per 100 parts by weight of the second sublayer.
[0009] The sustained-release granules may be prepared by mixing 35-58 parts by weight of a sustained-release material precursor with 42-60 parts by weight of silicone oil.
[0010] The ceramic coating precursor may be formed by a sol-gel reaction using an A material including a silane substance, a B material including a silica sol and a filler, and a C material including an organic acid.
[0011] The ceramic coating may further include a third sublayer disposed between the first sublayer and the second sublayer.
[0012] The ceramic coating may further include a third ceramic coating.
[0013] The third ceramic coating may include a ceramic coating precursor and slow-release particles, and the method may further include forming a third sublayer on the first sublayer using the third ceramic coating, and then forming a second sublayer on the third sublayer. The content of the slow-release particles included in the third ceramic coating may be different from the content of the slow-release particles included in each of the first sublayer and the second sublayer.
[0014] The thickness of the ceramic coating may be no greater than 80 microns.
[0015] The thickness of each of the sublayers including the sustained-release particles in the first sublayer and the second sublayer is not less than 10 μm.
[0016] The particle size of the sustained-release particles may be less than or equal to 20 microns.
[0017] In terms of weight percentage, the silicone oil may include 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil. The molecular weight of the low molecular weight silicone oil may be between 500-1000, the molecular weight of the medium molecular weight silicone oil may be between 3000-6000, and the molecular weight of the high molecular weight silicone oil may be between 12000-30000.
[0018] According to another aspect of the exemplary embodiment, a non-stick utensil includes a ceramic coating formed on a substrate using the above method.
[0019] The uppermost sublayer of the ceramic coating formed by the method of the present invention includes a slow-release material. Since the slow-release material in the ceramic coating has a disordered porous structure, silicone oil is adsorbed and bonded on the surface and pores of the slow-release material. The ceramic coating formed by this ceramic coating has a slow-release effect of silicone oil, thereby improving the long-lasting non-stick performance of the ceramic coating. In addition, by forming a ceramic coating including a gradient slow-release particle content, the bonding force between the ceramic coating and the substrate can be enhanced while ensuring excellent non-stick performance, so as to improve the service life of the ceramic coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a schematic diagram showing a first embodiment of a ceramic coating according to an exemplary embodiment;
[0021] Figure 2 is a schematic enlarged view showing slow-release particles in a ceramic coating according to an exemplary embodiment;
[0022] Figure 3 is a schematic diagram showing a second embodiment of a ceramic coating according to an exemplary embodiment;
[0023] Figure 4 is a schematic diagram illustrating a third embodiment of a ceramic coating according to an exemplary embodiment. DETAILED DESCRIPTION
[0024] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which embodiments are shown. However, the present invention may be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that the disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. The same reference numerals refer to the same elements throughout.
[0025] Ceramic coatings achieve non-stick properties mainly through the use of silicone methyl and doped silicone oil in the ceramic coating. As the product is heated and worn during use, the silicone oil in the coating will gradually be lost, destroying the silicone methyl groups on the surface, resulting in the loss of the non-stick effect, and finally the phenomenon of sticking to the pan when cooking. If the ceramic coating can store oil continuously, it can form an effective oil film to isolate the food and the coating surface, thereby achieving long-lasting non-stick properties.
[0026] Therefore, the present invention provides a method for preparing a ceramic coating, wherein the ceramic coating formed by the method includes slow-release particles having a slow-release material, wherein the slow-release material may have a disordered porous and / or layered structure, and silicone oil is combined (e.g., adsorbed, bonded) to the slow-release material. During the cooking process, the slow-release particles in the ceramic coating can slow down the release of silicone oil, so that the ceramic coating can maintain a long-lasting non-stick effect. In addition, since the ceramic coating includes a plurality of sublayers, it is possible to ensure non-stick properties while also improving the bonding performance between the ceramic coating and the substrate, thereby increasing the life of the ceramic coating.
[0027] Figure 1 is a schematic diagram showing a first embodiment of a ceramic coating according to an exemplary embodiment, Figure 2 is a schematic diagram showing slow-release particles in a ceramic coating according to an exemplary embodiment, Figure 3 is a schematic diagram showing a second embodiment of a ceramic coating according to an exemplary embodiment, and Figure 4 is a schematic diagram showing a third embodiment of a ceramic coating according to an exemplary embodiment. Figures 1 to 4 A method for preparing a ceramic coating according to an embodiment of the present inventive concept will be described.
[0028] Reference Figure 1 and Figure 2 , the ceramic coating 200 according to the first embodiment of the inventive concept is disposed (eg, directly disposed) on the substrate 100 , and includes at least two sub-layers, for example, a first sub-layer 201 and a second sub-layer 202 .
[0029] According to an exemplary embodiment, the substrate 100 may be a substrate known in the art for making cookware, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, etc. However, the present invention does not limit the material, use, and other properties of the substrate, that is, those skilled in the art may use any material on which a ceramic coating is to be applied as the substrate 100 as needed, so that the non-stick utensil of the present invention may be applicable to any scene requiring non-stick.
[0030] At least two sublayers are formed on the substrate 100, and at least the uppermost sublayer (e.g., the second sublayer 202) of the at least two sublayers included in the ceramic coating 200 is used to provide non-stick properties. Although the first embodiment shows two sublayers, the exemplary embodiment is not limited thereto, and those skilled in the art may set other sublayers (e.g., a third sublayer, a fourth sublayer, etc.) between the two sublayers (the first sublayer and the second sublayer) based on the inventive concept, so that the ceramic coating 200 of the inventive concept may include at least two sublayers.
[0031] According to an exemplary embodiment, referring to Figure 1, each of the at least two sub-layers (e.g., the first sub-layer 201 and the second sub-layer 202) may include a ceramic coating precursor 1 and slow-release particles 2 dispersed in the ceramic coating precursor, and the content of the slow-release particles 2 in the at least two sub-layers (e.g., the number of slow-release particles included in the sub-layer per unit weight, for example, the density of the slow-release particles in the sub-layer) is different. However, exemplary embodiments are not limited to Figure 1 That is, the first sub-layer 201 may not include the slow-release particles or include very few slow-release particles, but only include the ceramic coating precursor 1.
[0032] According to an exemplary embodiment, in a direction away from the substrate 100, the at least two sub-layers may have different (e.g., increased) contents of slow-release particles. Therefore, the method for preparing a ceramic coating 200 according to the first embodiment of the present inventive concept may include: preparing a first ceramic coating for a sub-layer (e.g., a first sub-layer 201) closest to the substrate 100 and preparing a second ceramic coating for a sub-layer (e.g., a second sub-layer 202) farthest from the substrate 100; using a layer forming process, forming a first sub-layer 201 on the substrate 100 using the first ceramic coating, and forming a second sub-layer 202 on the first sub-layer 201 using the second ceramic coating. In addition, although not shown, when the ceramic coating includes three or more sub-layers, the method for preparing the ceramic coating further includes the steps of preparing corresponding ceramic coatings (e.g., a third ceramic coating, a fourth ceramic coating, etc.) and forming corresponding sub-layers using the corresponding ceramic coatings, and the ceramic coatings used to form different sub-layers may differ only in the content of slow-release particles (or further in particle size). For example, when a third sublayer is further provided between the first sublayer and the second sublayer, a third ceramic coating can be formed first, and then the third sublayer can be provided on the first sublayer using the third ceramic coating, and then the second sublayer can be formed on the third sublayer using the second ceramic coating. Here, the third ceramic coating can include a ceramic coating precursor 1 and slow-release particles 2, and the content of the slow-release particles included in the third ceramic coating can be different from the content of the slow-release particles included in the first sublayer and the content of the slow-release particles included in the second sublayer (for example, the content of the slow-release particles included in the third ceramic coating is greater than the content of the slow-release particles included in the first sublayer and less than the content of the slow-release particles included in the second sublayer). Hereinafter, the description will be mainly based on the case where the ceramic coating includes the first sublayer and the second sublayer, and those skilled in the art can know the case where the third sublayer is formed between the first sublayer and the second sublayer based on the concept of the present invention.
[0033] According to an exemplary embodiment, before, during, or after providing the substrate 100, a first ceramic coating and a second ceramic coating may be prepared. The first ceramic coating is used to form a first sublayer, and the second ceramic coating is used to form a second sublayer. Both the first ceramic coating and the second ceramic coating have a ceramic coating precursor, and the difference is only in the content, particle size, etc. of the slow-release particles. Therefore, the preparation method of the first ceramic coating is mainly described in detail here, and the description of the preparation method of the second ceramic coating is simplified.
[0034] Herein, the ceramic coating precursor 1 may be equivalent to the ceramic coating used in the art, and therefore, may have the components of the ceramic coating conventionally used in the art, so that the ceramic coating preparation method known in the art may be used. However, the exemplary embodiment is not limited thereto, as mentioned in the method for manufacturing the ceramic coating precursor 1 according to the inventive concept described below in conjunction with the exemplary embodiment, the ceramic coating precursor 1 may be prepared by the method described below, and the ceramic coating precursor 1 prepared by the method of the inventive concept to be described below may have a more excellent feature of cooperating with the slow-release particles to provide non-stickiness.
[0035] According to an exemplary embodiment, the first ceramic coating comprises a ceramic coating precursor 1 and optionally slow-release particles 2 dispersed in the ceramic coating precursor. Figure 1 The first embodiment in which the slow-release particles 2 are dispersed in the ceramic coating precursor 1 of the first sub-layer 201 is shown, but the exemplary embodiments are not limited thereto, and as Figure 3 In the second embodiment shown, the first sub-layer 201 is formed only of the ceramic coating precursor 1, and therefore, the ceramic coating precursor 1 used to form the first ceramic coating may not be dispersed with the slow-release particles 2. Therefore, the following will mainly describe the case where the first sub-layer 201 according to the first embodiment includes the slow-release particles 2.
[0036] According to an exemplary embodiment, the step of providing a first ceramic coating may include the steps of preparing a ceramic coating precursor 1 and slow-release particles 2, respectively, and mixing the ceramic coating precursor 1 with the slow-release particles 2 to obtain the first ceramic coating. However, the exemplary embodiment is not limited thereto, that is, those skilled in the art may also adopt the preparation method of ceramic coatings in the prior art to obtain the ceramic coating precursors here, or may combine the steps of preparing the ceramic coating precursors with the steps of preparing the slow-release particles, and the method for manufacturing the ceramic coatings in the prior art will not be redundantly described here. Below, the method for preparing the first ceramic coating according to the present invention by preparing the ceramic coating precursor 1 and the slow-release particles 2, respectively, will be mainly described.
[0037] Preparation of ceramic coating precursors
[0038] According to an exemplary embodiment, the step of preparing the ceramic coating precursor may include a step of providing materials and a step of mixing.
[0039] The step of providing materials may include the steps of separately providing A material, B material and C material.
[0040] Here, material A may include a silane substance, material B may include silica sol and filler as essential components, optional pigments, wetting agents, thickeners and emulsifiers as unnecessary components and a solvent, and material C may include an organic acid as an essential component, and optional pH buffers and catalysts (e.g., zirconium acetate) as unnecessary components.
[0041] In the A material, according to an exemplary embodiment, the silane substance is used to form polysiloxane during the formation of the ceramic coating, and therefore, the silane substance here may include a substance known in the art for polycondensation to form polysiloxane. According to an exemplary embodiment, the silane substance may include at least one of methyltrimethoxysilane, methyltriethoxysilane, and dimethyldimethoxysilane, but is not limited thereto. In addition, in addition to the silane substance, the A material may also include tetraethyl orthosilicate that is polycondensed to form polysiloxane, and in this case, in the A material, by weight percentage, the silane substance may account for 80%-97% of the A material, and the tetraethyl orthosilicate may account for 3%-20% of the A material.
[0042] Material B may necessarily include fillers and silica sol. The filler plays a role in increasing the wear resistance of the coating, etc. Therefore, the present invention does not limit the type of filler, and ordinary commonly used fillers can be selected, for example, at least one of mica powder, kaolin, montmorillonite, silicon carbide, alumina and silicon dioxide can be selected. In addition, silica sol is the main film-forming substance of ceramic coatings, which reacts with polysiloxane under acidic conditions to form a ceramic coating. Therefore, commercially available ordinary silica sol can be selected as the silica sol in material B of the present invention. For example, the silica sol can be Akzo Nobel 1050 (silica sol) or American Grace LUDIXAM-50.
[0043] The necessary components in the B material can be dispersed in a solvent. That is, the B material can also include a solvent. Here, the solvent can include deionized water, and in order to adjust the volatilization rate of the solvent during the coating drying process, the solvent can also include isopropanol. In addition, the ratio between isopropanol and water is unlimited, and the ratio between water and isopropanol can be selectively proportioned according to actual needs.
[0044] In the B material, in addition to the above-mentioned necessary components, one or more of a pigment, a wetting agent, a thickener and an emulsifier may be selectively included as an unnecessary component. Here, the pigment is mainly used to give the coating different colors, so ordinary inorganic pigments can be selected. Inorganic pigments have good temperature resistance and good safety, and inorganic pigments are preferably selected in the high temperature resistant field. According to an exemplary embodiment, at least one of carbon black, copper chrome black, titanium dioxide, iron oxide, etc. may be selected as a filler. In addition, during the preparation of the necessary components in the solvent, in order to provide the excellent properties of the material, at least one of a wetting agent, a thickener and an emulsifier may also be added to the material.
[0045] According to a specific example, the B material may include, by weight percent: 30wt%-48wt% of silica sol, 8wt%-13wt% of pigment, 8wt%-25wt% of filler, 0.2wt%-1wt% of wetting agent, 1wt%-3wt% of thickener, 3wt%-5wt% of emulsifier, and the balance is isopropyl alcohol and deionized water. However, exemplary embodiments are not limited thereto, and one or more of the unnecessary components may be omitted.
[0046] The C material is used as a strong acid catalyst, and may include an organic acid as an essential component, and an optional pH buffer and a catalyst (e.g., zirconium acetate) as an unnecessary component. Here, the organic acid is used to adjust the pH value of the silica sol in the subsequent process so that it can react with the A material in an acidic environment, and therefore, an organic acid commonly used in the art for ceramic coatings can be used. According to an exemplary embodiment, at least one of formic acid and acetic acid can be selected as an organic acid, and when both formic acid and acetic acid are included, the weight ratio between formic acid and acetic acid can be between 4:6 and 1:1. In addition, in the C material, a pH buffer and a catalyst may also be selectively included. Here, the pH buffer and the catalyst may be a pH buffer and a catalyst used in the process of preparing a strong acid catalyst for ceramic coatings known in the art, for example, the pH buffer may be a weak acid such as boric acid, and the catalyst is used to accelerate the reaction speed of the sol-gel, and may be zirconium acetate, etc. However, the exemplary embodiment is not limited to the types of pH buffers and catalysts, and suitable pH buffers and catalysts may be omitted or appropriately selected based on the prior art.
[0047] According to an exemplary embodiment, the C material may include 80-97 parts by weight of a mixture of formic acid and acetic acid, 1-2 parts by weight of a boric acid pH buffer, and 0.5 parts by weight of a zirconium acetate catalyst.
[0048] After providing the above-mentioned materials, a mixing step may be performed. Herein, the mixing step may include a first mixing step of mixing the B material with the C material and a second step of mixing the result of the first mixing step (ie, the first material described below) with the A material.
[0049] Specifically, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidic (e.g., to less than or equal to 4) by utilizing the acidity of the C material to obtain the first material. Since the C material includes a solid filler and an optional pigment, the C material can be added to a grinder and ground for 0.5h-2h before mixing or during the preparation of the C material, so that it is fully dispersed and ground to a particle size of less than or equal to 15 microns to obtain a uniformly dispersed slurry.
[0050] After the B material and the C material are mixed, the mixture may be tumbling dispersed for a predetermined time (eg, 0.5 h) so that the first material has a high degree of dispersion.
[0051] After obtaining the first material, material A may be added to the first material. Here, the weight ratio of the added amount of material A to material B may be in the range of (20-30):(40-60). After adding material A, material A and material B may be shaken evenly so that material A and material B undergo a sol-gel reaction in an acidic environment to form a ceramic coating precursor.
[0052] Preparation of sustained-release granules
[0053] The slow-release particles can be prepared during, before, or after the preparation of the ceramic coating precursor. The slow-release particles can be prepared by mixing the slow-release material with silicone oil.
[0054] According to an exemplary embodiment, the sustained-release particle 2 may include a sustained-release material 21 having a pore structure and / or a layer structure and a silicone oil 22 combined with (eg, adsorbed, bonded to) the sustained-release material.
[0055] A slow-release material precursor of appropriate size (i.e., a slow-release material before grinding, when the grinding step is omitted, the slow-release material precursor can be considered as the slow-release material used in the end) can be selected to prepare slow-release particles. According to an exemplary embodiment, the slow-release material precursor can have a layer gap and / or pore structure. According to the example, the slow-release material precursor can include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material precursor has a porous and / or layered structure and the slow-release material formed after grinding is combined with silicone oil. The silicone oil combined with the slow-release material can be slowly released during the use of the cookware with a non-stick coating formed by the ceramic coating conceived by the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick layer formed by the ceramic coating.
[0056] According to an exemplary embodiment, the particle size of the slow-release material precursor may be in the range of 100 meshes to 3000 meshes, and the particle size of the slow-release material within this range may obey a normal distribution. However, when the particle size is too large (e.g., on a 100 mesh sieve), the excessively large particle size is likely to increase the grinding process or make the particle size of the slow-release material after grinding too large, ultimately affecting the appearance of the non-stick coating made using the ceramic coating; on the contrary, too small a particle size (e.g., under a 3000 mesh sieve, and when the particle size is smaller after grinding) is not easy to effectively adsorb and bond silicone oil, and thus it is not easy to achieve a good silicone oil slow-release effect.
[0057] When the slow-release material precursor has the above-mentioned particle size distribution, the particle size of the slow-release material finally obtained can be made to be less than 20 microns by using two grinding processes as described below. However, the exemplary embodiment is not limited thereto, that is, when the slow-release material precursor is selected to have a smaller value within the range of 100 mesh-3000 mesh, one grinding process can be omitted; in addition, when the particle size of the slow-release material precursor is selected to have a smaller value within the above-mentioned range, two grinding processes can be omitted. When at least one of the grinding processes is omitted, the omitted grinding process can be replaced by a stirring process, or no treatment can be performed on the mixture.
[0058] According to an exemplary embodiment, the silicone oil 22 is combined (e.g., adsorbed, bonded) with the sustained-release material 21 and provides the main non-stickiness for the ceramic coating. The silicone oil can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, and polyether modified silicone oil, and can be mixed by silicone oils of different molecular weights in a certain proportion to form a silicone oil composition with a molecular weight normal distribution; wherein, by weight percentage, the low molecular weight silicone oil content can be 20wt%-30wt%, the medium molecular weight silicone oil content can be 40wt%-60wt%, and the high molecular weight silicone oil content can be 20wt%-30wt%. Here, the molecular weight of the low molecular weight silicone oil can be between 500-1000, the molecular weight of the medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of the high molecular weight silicone oil can be between 12000-30000. By utilizing a normally distributed silicone oil composition, the sustained-release and non-stick effects can be better exerted. This is because: high molecular weight silicone oil is more firmly bonded to the sustained-release material and releases more slowly; low molecular weight silicone oil has better free mobility and thus better non-stick properties; in addition, medium molecular weight silicone oil takes into account both free mobility and strong bonding. Therefore, low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil can be combined to better exert the sustained-release and non-stick effects.
[0059] According to an example, 35-58 parts by weight of a slow-release material precursor can be mixed with 42-60 parts by weight of silicone oil to obtain a mixture, and 1 part by weight of a coupling agent (e.g., a methoxysilane coupling agent), 0.3 parts by weight of a catalyst (e.g., a titanate catalyst) and 1-1.5 parts by weight of a dispersant can be added to the mixture to prepare slow-release particles. Here, the coupling agent and the catalyst are used to enhance the bonding force between the silicone oil and the slow-release material, and the dispersant is used to improve the dispersion of the slow-release material in the silicone oil. Therefore, the exemplary embodiment is not limited to the case of including a coupling agent, a dispersant and a catalyst, and at least one of the coupling agent, the catalyst and the dispersant can be omitted.
[0060] According to a specific example, the silicone oil, the sustained-release material with a particle size of 100 mesh sieve-3000 mesh sieve and the silane coupling agent can be mixed uniformly according to the above ratio, and ground to a particle size of less than or equal to 30 microns, and then the catalyst is added, and the particle size is continued to be less than or equal to 20 microns, and then ultrasonic treatment is performed at room temperature (e.g., 22°C) for 0.5h-1h, so that the sustained-release particles can be obtained. Here, firstly, the silicone oil is mixed with the sustained-release material and then ground to a particle size of less than or equal to 30 microns, so that the silicone oil and the sustained-release material can be mixed uniformly, and then, the silicone oil is ground to a particle size of less than or equal to 20 microns under the condition of the catalyst, so that the silicone oil can be fully firmly adsorbed and bonded to the outside of the sustained-release material. However, when the particle size of the sustained-release material is less than 30 microns, the first grinding can be omitted, and a stirring process can be optionally provided, or a second grinding process can be directly performed. In addition, when the particle size of the sustained-release material is less than 15 microns, the second grinding process can be further omitted, and a stirring process can be optionally provided.
[0061] Preparation of the first ceramic coating
[0062] After the ceramic coating precursor and the slow-release particles are prepared, the slow-release particles can be mixed with the ceramic coating precursor to prepare the first ceramic coating according to the exemplary embodiment. However, the exemplary embodiment is not limited thereto, and when the first ceramic coating does not include the slow-release particles (e.g., Figure 3 ), this step can be omitted and the ceramic coating precursor can be directly used to form the first sub-layer.
[0063] According to an exemplary embodiment, during the preparation of the first ceramic coating, based on the total weight of the first ceramic coating, less than 32.97 wt% of the slow-release particles can be mixed with more than 67.03 wt% of the ceramic coating precursor (i.e., the ceramic coating includes less than 32.97 wt% of the slow-release particles), and after the ceramic coating precursor and the slow-release particles are mixed, the mixture can be stirred at a speed of 120 rpm to 200 rpm for 6 h to 8 h to obtain the desired first ceramic coating.
[0064] In addition, although the above description describes a method of obtaining the first ceramic coating by separately preparing a ceramic coating precursor and slow-release particles and mixing the ceramic coating precursor with the slow-release particles when the first ceramic coating includes slow-release particles, in a method of combining the step of preparing a ceramic coating precursor with the step of preparing slow-release particles, as described above, after mixing the B material with the C material, the A material and the slow-release particles can be simultaneously added to the mixture of the B material and the C material. For example, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, and the pH of the mixture can be adjusted to acidic (e.g., less than or equal to 4) by using the acidity of the C material to obtain the first material. Then, material A and slow-release particles can be added to the mixture, where the weight ratio of material A to material B can be in the range of (20-30): (40-60), and based on the total weight of the mixture (i.e., A, B, C and slow-release particles), the amount of slow-release particles added can be less than 32.97wt% (i.e., the weight ratio of material A, material B and slow-release particles can be (20-30): (40-60): less than 30). After mixing, the mixture can be stirred at a speed of 120 rpm to 200 rpm for 6h to 8h to obtain the desired first ceramic coating.
[0065] In the above, the method for forming the first ceramic coating is described in detail in combination with the exemplary embodiment. Since the first ceramic coating and the second ceramic coating (or, when the ceramic coating includes more than two sublayers, the ceramic coating used to form the remaining sublayers) differ only in the physical parameters of the slow-release particles (for example, content, particle size, etc.), the method for forming the first ceramic coating and the second ceramic coating differs only in the preparation of the slow-release particles and / or the mixing steps of the ceramic coating precursor and the slow-release particles. Therefore, only this difference will be described below.
[0066] According to an exemplary embodiment, the method for forming the second ceramic coating (or, when the ceramic coating includes more than two sub-layers, the ceramic coating for forming the remaining sub-layers) may include the preparation of the ceramic coating precursor, the preparation of the slow-release particles, and the mixing of the ceramic coating precursor and the slow-release particles as described above in conjunction with the method for forming the first ceramic coating. The slow-release particles in the second ceramic coating may have a higher content than the slow-release particles in the first ceramic material (e.g., Figure 1 ), and may further have a size different from that of the sustained-release particles in the first ceramic material ( Figure 4The third embodiment in the figure shows that the size of the slow-release particles 2 of the second sub-layer 202 is larger than the size of the slow-release particles 2 in the first sub-layer 201). Therefore, in the step of preparing the slow-release particles, by controlling the grinding process, the screening process, etc., the size of the slow-release particles suitable for the second ceramic material can be prepared. In addition, in the preparation of the second ceramic coating (i.e., the mixing of the ceramic coating precursor and the slow-release particles), based on the total weight of the second ceramic coating, 5.15wt%-32.97wt% of the slow-release particles can be mixed with 67.03wt%-94.85wt% of the ceramic coating precursor (i.e., the ceramic coating includes less than 32.97wt% of the slow-release particles, for example, the weight ratio of A material, B material and slow-release particles can be (20-30): (40-60): (5-30)) and the content of the slow-release particles included in the second ceramic coating is higher than the content of the slow-release particles included in the first ceramic coating (i.e., the content of the slow-release particles included in each sub-layer increases gradually from the base). In addition, when there are more than two sub-layers, different ceramic coatings including the slow-release particles having a gradient increasing content in the direction away from the substrate 100 can be prepared. After the ceramic coating precursor and the slow-release particles are mixed, the mixture can be stirred at a speed of 120 rpm to 200 rpm for 6 h to 8 h to obtain the desired second ceramic coating.
[0067] Preparation of ceramic coating
[0068] After obtaining ceramic coatings (e.g., first ceramic coatings and second ceramic coatings) for forming at least two sub-layers (e.g., first sub-layers and second sub-layers), different sub-layers may be formed using different ceramic coatings. For example, a first sub-layer 201 may be formed on a substrate 100 using a layer forming process using a first ceramic coating, and then a second sub-layer 202 may be formed on the first sub-layer 201 using a second ceramic coating.
[0069] For example, the first ceramic coating may be sprayed by air spraying to form the first sublayer 201 on the substrate 100. Then, the second ceramic coating may be sprayed by air spraying to form the second sublayer 202 on the first sublayer 201. Here, the type of ceramic coating does not limit the air spraying parameters, and the air spraying parameters are as follows: the spraying distance is 160 mm; the air pressure is 0.3 MPa; the flow rate is 8 L / min. However, the exemplary embodiment is not limited thereto, and those skilled in the art may use other layer forming methods to form the first sublayer 201 and the second sublayer 202 of the ceramic coating 200 using the first ceramic coating and the second ceramic coating of the present invention. In addition, in order to improve the bonding force between the ceramic coating 200 and the substrate 100, the substrate 100 may be treated. For example, the substrate may be sandblasted with 60# brown corundum to form a surface roughness of 3-6 microns, and then the substrate may be cleaned and preheated to 40°C to 60°C, and then the ceramic coating formation process may be performed.
[0070] After air spraying, the resultant may be cured at 230-280° C. for 10-15 min to form a ceramic coating having a total thickness of no more than 80 μm and a thickness of no less than 10 μm including the sublayer of slow-release particles.
[0071] Through the detailed description in combination with the exemplary embodiments above, the ceramic coating of the present invention includes slow-release particles, so that during the cooking process, the release of silicone oil can be slowed down, thereby maintaining a long-lasting non-stick effect. In addition, due to the presence of each sublayer of gradient slow-release particles, the bonding force between the ceramic coating and the substrate can be improved.
[0072] Hereinafter, the beneficial effects of the inventive concept will be described in conjunction with specific examples.
[0073] Example 1
[0074] The ceramic coating is formed by the following method.
[0075] S1: 80 wt % of methyltrimethoxysilane and 20 wt % of ethyl orthosilicate are mixed and stirred uniformly to obtain a silane composition of component A;
[0076] S2: 30wt% of Akzo Nobel 1050 (silica sol), 8wt% of titanium dioxide (pigment), 25wt% of kaolin (filler), 3wt% of Tween-80 (emulsifier), 1wt% of water-based modified bentonite (thickener), 0.3wt% of polyoxyethylene ether TRITON X-100 (wetting agent), 20wt% of isopropanol and the balance of deionized water were mixed evenly, then added to a grinder and ground for 2h, fully dispersed and ground to a particle size of not more than 15 microns, to obtain component B slurry;
[0077] S3: 48 parts by weight of formic acid, 48 parts by weight of acetic acid, 1 part by weight of boric acid (buffer), and 0.5 parts by weight of zirconium acetate (catalyst) are uniformly mixed to obtain component C strong acid catalyst;
[0078] S4: 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 and 42 parts by weight of vermiculite (slow-release material) with a particle size of 100 to 3000 meshes are mixed, and then 3 parts by weight of methoxysilane coupling agent are added and mixed evenly, and the mixture is ground to a particle size of no more than 30 microns, and then 0.3 parts by weight of titanate (catalyst) is added, and the mixture is further ground to a particle size of no more than 20 microns, and then ultrasonically treated at room temperature of 22° C. for 0.5 h to obtain a slow-release particle component D, and the particle size of the slow-release particle component D obeys a normal distribution;
[0079] S5: The above four components are mixed in order according to the weight ratio of A: B: C: D = 20: 40: 1: 2, and rolled to mature to obtain the first ceramic coating. The mixing order and the maturation method are as follows: first, 40 parts by weight of component B and 1 part by weight of component C are mixed evenly, and the pH is adjusted to 4 by component C, and the mixture is rolled and dispersed for 0.5 hours, and then 20 parts by weight of component A are added and shaken evenly, and then 2 parts by weight of component D are added, and the reaction is stirred at a speed of 200 rpm for 8 hours to obtain the desired first ceramic coating;
[0080] S6: The above four components are mixed in order according to the weight ratio of A: B: C: D = 20: 40: 1: 20, and rolled to mature to obtain the second ceramic coating. The mixing order and the maturation method are as follows: first, 40 parts by weight of component B and 1 part by weight of component C are mixed evenly, and the pH is adjusted to 4 by component C, and the mixture is rolled and dispersed for 0.5 hours, and then 20 parts by weight of component A is added and shaken evenly, and then 20 parts by weight of component D is added, and the reaction is stirred at a speed of 200 rpm for 8 hours to obtain the desired second ceramic coating.
[0081] The non-stick cookware is manufactured by using the ceramic coating as follows.
[0082] B1: Substrate treatment. The stainless steel substrate is sandblasted with 60# brown corundum to form a surface roughness of 3 microns;
[0083] B2: Preheating. Clean the sandblasted substrate and preheat it to 60°C;
[0084] B3: Spraying. A first ceramic coating was used to form a first sublayer with a thickness of 10 microns on the substrate by air spraying, and a second ceramic coating was used to form a second sublayer with a thickness of 60 microns on the first sublayer. The air spraying parameters were as follows: spraying distance was 160 mm; air pressure was 0.3 MPa; flow rate was 8 L / min.
[0085] B4: Sintering: Curing at 250°C for 10 minutes.
[0086] Through the above method, the non-stick cookware of Example 1 is obtained.
[0087] Example 2
[0088] The difference from Example 1 is that the sustained-release material is bentonite.
[0089] Example 3
[0090] The difference from Example 1 is that the sustained-release material is alpha alumina.
[0091] Example 4
[0092] The difference from Example 1 is that the particle size of the slow-release particle component is not greater than 15 microns, and the particle size of the slow-release particle component D obeys a normal distribution.
[0093] Example 5
[0094] The difference from Example 1 is that the particle size of the slow-release particle component is not greater than 10 microns, and the particle size of the slow-release particle component D obeys a normal distribution.
[0095] Example 6
[0096] The difference from Example 1 is that the thickness of the first sub-layer is 15 micrometers.
[0097] Example 7
[0098] The difference from Example 1 is that the thickness of the first sub-layer is 20 micrometers.
[0099] Example 8
[0100] The difference from Example 1 is that the thickness of the second sub-layer is 40 micrometers.
[0101] Example 9
[0102] The difference from Example 1 is that the thickness of the second sub-layer is 70 micrometers.
[0103] Example 10
[0104] The difference from Example 1 is that A, B, C and D are mixed in order according to the weight ratio of A:B:C:D=20:40:1:0 to prepare the first ceramic coating. In other words, the first ceramic coating does not include slow-release particles.
[0105] Embodiment 11
[0106] The difference from Example 1 is that A, B, C and D are mixed in order according to a weight ratio of A:B:C:D=20:40:1:8 to prepare the first ceramic coating.
[0107] Example 12
[0108] The difference from Example 1 is that A, B, C and D are mixed in sequence according to a weight ratio of A:B:C:D=20:40:1:15 to prepare the first ceramic coating.
[0109] Embodiment 13
[0110] The difference from Example 1 is that A, B, C and D are mixed in order according to the weight ratio of A:B:C:D=20:40:1:30 to prepare the second ceramic coating.
[0111] Embodiment 14
[0112] The difference from Example 1 is that A, B, C and D are mixed in order according to the weight ratio of A:B:C:D=30:60:2:5 to prepare the second ceramic coating.
[0113] Embodiment 15
[0114] The difference from Example 1 is:
[0115] (1) further comprising step S7, wherein step S7 differs from step S6 in that A, B, C and D are sequentially mixed in a weight ratio of A:B:C:D=20:40:1:10 to prepare a third ceramic coating;
[0116] (2) Step B3 also includes forming a third sub-layer with a thickness of 10 μm on the first sub-layer using a third ceramic material, and forming a second sub-layer with a thickness of 60 μm on the third sub-layer using a second ceramic coating.
[0117] Example 16
[0118] The difference from Example 1 is that the silicone oil is composed of 20 wt % of hydroxy silicone oil with a molecular weight of 800, 60 wt % of hydroxy silicone oil with a molecular weight of 3000 and 20 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0119] Embodiment 17
[0120] The difference from Example 1 is that the silicone oil is composed of 30 wt % of hydroxy silicone oil with a molecular weight of 800, 40 wt % of hydroxy silicone oil with a molecular weight of 3000 and 30 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0121] Embodiment 18
[0122] The difference from Example 1 is that the silicone oil is composed of 25 wt % of hydroxy silicone oil with a molecular weight of 800, 50 wt % of hydroxy silicone oil with a molecular weight of 3000 and 25 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0123] Embodiment 19
[0124] The difference from Example 1 is that 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 49 parts by weight of sustained-release material.
[0125] Embodiment 20
[0126] The difference from Example 1 is that 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 60 parts by weight of sustained-release material.
[0127] Embodiment 21
[0128] The difference from Example 1 is that 35 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 42 parts by weight of sustained-release material.
[0129] Embodiment 22
[0130] The difference from Example 1 is that 46 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 42 parts by weight of sustained-release material.
[0131] Comparative Example 1
[0132] The difference from Example 1 is that in step S5, components A, B, C and D are mixed in sequence according to a weight ratio of A:B:C=22:40:1:0, and the obtained ceramic material is used to manufacture non-stick cookware including a conventional ceramic coating with a thickness of 70 microns, while omitting step S6.
[0133] Comparative Example 2
[0134] The difference from Example 1 is that in step S6, components A, B, C and D are mixed in order according to a weight ratio of 20:40:1:3 to prepare a second ceramic coating.
[0135] Comparative Example 3
[0136] The difference from Example 1 is that the second sub-layer is located on the substrate, and the first sub-layer is located on the second sub-layer.
[0137] Comparative Example 4
[0138] The difference from Example 1 is that 30 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 60 parts by weight of sustained-release material.
[0139] Comparative Example 5
[0140] The difference from Example 1 is that 60 parts by weight of hydroxy silicone oil with a molecular weight of 3000 is mixed with 40 parts by weight of sustained-release material.
[0141] The non-stick properties of the non-stick cookware of the above-mentioned Examples 1-22 and Comparative Examples 1-5 were tested, and the test results are shown in the following table.
[0142]
[0143]
[0144] Performance index test
[0145] The above-obtained cookware was subjected to a performance test, and the specific performance test method is as follows:
[0146] (1) Long-lasting non-stick test method: refer to 4.2.1 Fried egg non-stick test in GB_T 32095.2-2015. The unit is the number of times. The higher the number, the longer the life. The non-stick result is evaluated once every 1000 times, and the number of times when the non-stickiness reaches Level III is recorded.
[0147] (2) Plane wear resistance test method: GB_T 32095.2-2015 4.3.1 Plane wear resistance test, use 3M7447 scouring pad, apply a force of 15N, the frequency is 33 times / minute, and the scouring pad is replaced every 500 times.
[0148] By comparing and analyzing the embodiments 1-22 of the present invention and the comparative examples 1-5, it is found that the long-lasting non-stickiness of the existing conventional ceramic coating in comparative example 1 does not exceed 500 times. In addition, although comparative examples 2 and 3 include two sublayers, the content of the slow-release particles in the uppermost sublayer is low, and therefore, the test performance of the ceramic coating formed with a double-layer structure is lower than the test performance of the ceramic coating in the embodiment. In addition, the silicone oil in comparative example 4 cannot effectively provide a slow-release effect due to its low content, while the content of the slow-release material in comparative example 5 is low, and the combined silicone oil is less, and an effective slow-release effect cannot be formed. In contrast, the long-lasting non-stickiness of the sensible ceramic coating according to the present invention is 8000-25000 times.
[0149] Although one or more embodiments of the present invention have been described with reference to the drawings, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the claims.
Claims
1. A method for preparing a ceramic coating, the ceramic coating comprising a first sublayer and a second sublayer disposed on a substrate, characterized in that: The method comprises: A ceramic coating is prepared, the ceramic coating comprising: a first ceramic coating comprising a ceramic coating precursor and optionally slow-release particles; and a second ceramic coating comprising a ceramic coating precursor and slow-release particles; and A first sublayer is formed on a substrate using a first ceramic coating by using a layer forming process, and a second sublayer is formed on the first sublayer using a second ceramic coating, wherein the content of the slow-release particles included in the first sublayer is different from the content of the slow-release particles included in the second sublayer, Wherein, the sustained-release particles include a sustained-release material and silicone oil bound to the sustained-release material. Wherein, the sustained-release material includes at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate.
2. The method according to claim 1, characterized in that The content of the sustained-release particles included in the first sub-layer is lower than the content of the sustained-release particles included in the second sub-layer.
3. The method according to claim 1, characterized in that The content of the sustained-release particles included in the first sublayer is 0 to less than 32.97 parts by weight per 100 parts by weight of the first sublayer, and the content of the sustained-release particles included in the second sublayer is 5.15-32.97 parts by weight per 100 parts by weight of the second sublayer.
4. The method according to claim 1, characterized in that The sustained-release granules are prepared by mixing 35-58 parts by weight of the sustained-release material precursor with 42-60 parts by weight of silicone oil.
5. The method according to claim 1, characterized in that The ceramic coating further comprises a third sublayer disposed between the first sublayer and the second sublayer, The ceramic coating further comprises a third ceramic coating, wherein the third ceramic coating comprises a ceramic coating precursor and slow-release particles. The method further includes forming a third sub-layer on the first sub-layer using a third ceramic coating, and then forming a second sub-layer on the third sub-layer. The content of the slow-release particles included in the third ceramic coating is different from the content of the slow-release particles included in each of the first sub-layer and the second sub-layer.
6. The method according to claim 1, characterized in that The thickness of the ceramic coating is no more than 80 microns.
7. The method according to claim 6, characterized in that The thickness of each of the sublayers including the sustained-release particles in the first sublayer and the second sublayer is not less than 10 μm.
8. The method according to claim 1, characterized in that The particle size of the sustained-release particles is less than or equal to 20 microns.
9. The method according to claim 1, characterized in that In terms of weight percentage, the silicone oil includes 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil. Among them, the molecular weight of low molecular weight silicone oil is between 500-1000, the molecular weight of medium molecular weight silicone oil is between 3000-6000, and the molecular weight of high molecular weight silicone oil is between 12000-30000.
10. A non-stick utensil, characterized in that: The non-stick utensil comprises a substrate and a ceramic coating formed by the method according to any one of claims 1 to 9.