Non-stick appliance
The non-stick utensil with a ceramic coating and slow-release particles addresses the short lifespan issue by sustaining non-stick performance through controlled silicone oil release and enhanced substrate bonding.
Patent Information
- Application Number
- CN202310649648.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
Ceramic coatings for non-stick utensils have a short lifespan and fail to meet consumer demands due to rapid degradation of non-stick properties, especially in high-temperature cooking and with metal spatulas.
A non-stick utensil with a ceramic coating containing slow-release particles and silicone oil, where the particles have a disordered porous structure to adsorb and bond silicone oil, combined with a substrate surface roughness of 3 to 15 microns for enhanced bonding, and multiple layers to sustain the non-stick effect.
The ceramic coating maintains a long-lasting non-stick performance by slowly releasing silicone oil, improving the durability and non-stick properties of the utensil.
Smart Images

Figure CN119060567A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of non-stick coatings, and in particular relates to a non-stick utensil. Background Art
[0002] Currently, non-stick technologies mainly include PTFE coatings and ceramic coatings. Ceramic coatings are very limited in use due to their short non-stick lifespan. They are far less widely used than PTFE products and cannot meet consumers' daily demand for non-stick utensils. For example, non-stick pans will stick to the pan after about one month of use in an average household, especially in high-temperature cooking methods such as Chinese cooking, and under the condition of wear and tear of metal spatulas, the non-stick properties decay very quickly.
[0003] Therefore, improving the long-lasting non-stick properties of ceramic coatings has become a very meaningful and urgent technical need. Summary of the invention
[0004] Based on the above-mentioned deficiencies of the prior art, the present invention provides a non-stick utensil, wherein the surface of the substrate of the non-stick utensil is functionalized so that the substrate can be more firmly combined with the ceramic coating.
[0005] According to an aspect of an exemplary embodiment, a non-stick utensil includes: a substrate; a ceramic coating located on the surface of the substrate, the ceramic coating including a ceramic coating precursor and slow-release particles dispersed in the ceramic coating precursor. The slow-release particles include a slow-release material and silicone oil bound to the slow-release material, the slow-release material including at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate, and layered sulfate. The surface of the substrate has a surface roughness of 3 microns to 8 microns.
[0006] The particle size of the sustained-release particles may be less than or equal to 20 microns.
[0007] The particle size of the sustained-release particles may be in the range of 8 microns to 15 microns.
[0008] The sustained-release particles may be included in an amount of 5.15-32.97 parts by weight per 100 parts by weight of the ceramic coating.
[0009] The thickness of the ceramic coating may be in the range of 10 microns to 80 microns.
[0010] The ceramic coating may include at least two sub-layers, and at least an uppermost sub-layer of the at least two sub-layers may include slow-release particles.
[0011] The thickness of each of the sub-layers including the slow-release particles may be not less than 10 micrometers, and the thickness of the ceramic coating layer may be not more than 80 micrometers.
[0012] The content of the sustained-release particles in each sub-layer may increase in a direction away from the substrate.
[0013] The substrate may include two or more layers composed of at least two materials selected from aluminum, aluminum alloy, titanium, titanium alloy, iron, and stainless steel.
[0014] The substrate may include a base layer and a functional layer disposed between the base layer and the ceramic coating layer, and a surface of the functional layer may have a surface roughness of 3 micrometers to 15 micrometers.
[0015] The non-stick utensil may further include a sealing layer, wherein the sealing layer is located on the surface of the ceramic coating.
[0016] The non-stick utensil of the present invention includes a ceramic coating containing slow-release particles. Since the slow-release material in the slow-release particles included in the ceramic coating has a disordered porous structure, silicone oil is adsorbed and bonded on the surface and pores of the slow-release material, so the ceramic coating has a silicone oil slow-release effect, thereby improving the long-lasting non-stick performance. In addition, since the substrate has a surface roughness of 3 microns to 15 microns after treatment, the substrate with such a surface roughness can be more firmly combined with the ceramic coating, thereby improving the service life of the non-stick utensil. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a schematic diagram showing a first embodiment of a ceramic coating according to an exemplary embodiment;
[0018] Figure 2 is a schematic enlarged view showing slow-release particles in a ceramic coating according to an exemplary embodiment;
[0019] Figure 3 is a schematic diagram showing a second embodiment of a ceramic coating according to an exemplary embodiment; DETAILED DESCRIPTION
[0020] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which embodiments are shown. However, the present invention may be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that the disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. The same reference numerals refer to the same elements throughout.
[0021] The non-stick effect of non-stick utensils formed by ceramic coatings is mainly achieved by the silicon methyl group and doped silicone oil in the ceramic coatings. As the product is heated and worn during use, the silicone oil in the coating will gradually be lost, destroying the silicon methyl group on the surface, and the non-stick effect will be lost, and finally the cooking pot will stick. If the ceramic coating can store oil continuously, it can form an effective oil film to isolate the food and the coating surface, thereby achieving long-lasting non-stick properties.
[0022] Therefore, the present invention provides a non-stick utensil having a ceramic coating including slow-release particles containing a slow-release material, wherein the slow-release material of the slow-release particles included in the ceramic coating has a disordered porous and / or layered structure, and silicone oil is combined (e.g., adsorbed, bonded) to the slow-release material. During the cooking process, the slow-release particles in the ceramic coating can slow down the release of silicone oil, so that the ceramic coating can maintain a long-lasting non-stick effect.
[0023] Figure 1 is a schematic diagram showing a first embodiment of a non-stick utensil according to an exemplary embodiment, Figure 2 is a schematic enlarged view showing the sustained-release particles included in the ceramic coating of the first embodiment, Figure 3 is a schematic diagram showing a second embodiment of a non-stick utensil according to an exemplary embodiment. Figures 1 to 3 To describe the non-stick utensil of the present invention.
[0024] Reference Figure 1 and Figure 2 , a non-stick utensil according to a first exemplary embodiment of the present inventive concept includes a base 100 and a ceramic coating disposed on the base.
[0025] According to an exemplary embodiment, the substrate 100 may be a substrate of a cooker known in the art, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, a titanium substrate, etc. In addition, since a substrate of a single material has some defects in terms of thermal conductivity, hardness, etc., preferably, the substrate may include two or more composite layers of at least two of aluminum, aluminum alloy, titanium, titanium alloy, stainless steel, and iron. For example, the substrate may include two or more composite layers of titanium-aluminum, iron-aluminum, or stainless steel-aluminum. However, the present invention does not limit the material, use, and other properties of the substrate. That is, those skilled in the art may use any substrate on which a ceramic coating 300 is to be applied as the substrate 100 as needed, so that the non-stick utensil conceived by the present invention may be applicable to any scene requiring non-stick (such as a non-stick coating of a cooking pot (e.g., a frying spoon, an inner pot of an electric rice cooker), an inner and outer coating of a transport pipeline, etc.).
[0026] In addition, the substrate 100 has an unlimited shape and thickness, for example, the substrate 100 can be a frying spoon substrate, an electric rice cooker liner substrate, etc. However, the surface of the substrate 100 needs to have a surface roughness of 3 microns to 15 microns. With such a surface roughness, the roughness and hardness of the substrate 100 can be increased, so that it can have better bonding force and wear resistance. In the case where the substrate 100 has a single-layer structure, the upper surface of the substrate 100 can have a surface roughness of 3 microns to 15 microns, or, when the substrate has a multi-layer structure (not shown), the surface of the uppermost layer of the multi-layer structure can have a surface roughness of 3 microns to 15 microns.
[0027] In order to achieve the surface roughness of the substrate 100, the substrate 100 may be functionalized. Here, the functionalization may include existing technologies such as hard oxidation, shot peening, embossing, graining, etching, thermal spraying, etc. Figure 1 The substrate 100 after functionalization treatment such as shot peening and etching is shown, and the substrate 100 may have a surface roughness of 3 μm to 15 μm. In addition, when the substrate is subjected to functionalization treatment such as thermal spraying (for example, thermal spraying the substrate surface by arc spraying, flame spraying, plasma spraying) using, for example, molten iron, titanium, aluminum, alloys, metal oxides, carbides, nitrides, etc., as shown in FIG. Figure 3 As shown, the surface of the substrate 100 according to the second embodiment of the present invention may additionally include a hard layer as a functional layer due to partial functionalization. In this case, the substrate 100 may include a base layer 101 and a functional layer 102 formed on the base layer 101. Here, the base layer 101 may be the same as the reference Figure 1 The substrate 100 of the first embodiment described has the same or substantially the same characteristics except that the surface has no roughness, and the functional layer 102 is a layer formed on the surface of the base layer 101 by functionalization treatment, and the base layer 101 and the functional layer 102 serve as the substrate 100 for forming the ceramic coating. Therefore, the surface of the functional layer 102 located on the upper part of the substrate 100 as the surface of the substrate 100 can have a surface roughness of 3 microns to 15 microns.
[0028] The ceramic coating 200 is located on the surface of the substrate 100. The ceramic coating 200 includes a ceramic coating precursor 1 and slow-release particles 2 (such as Figure 2 ).
[0029] Herein, the ceramic coating precursor 1 may be equivalent to the ceramic coating used in the art, and therefore, may have the components of the ceramic coating conventionally used in the art, so that the ceramic coating preparation method known in the art may be used. However, the exemplary embodiment is not limited thereto, as mentioned in the method for manufacturing the ceramic coating precursor 1 according to the inventive concept described below in conjunction with the exemplary embodiment, the ceramic coating precursor 1 may be prepared by the method described below, and the ceramic coating precursor 1 prepared by the method of the inventive concept to be described below may have a more excellent feature of cooperating with the slow-release particles to provide non-stickiness.
[0030] The slow-release particles 2 dispersed in the ceramic coating precursor 1 include a slow-release material 21 and silicone oil 22 bound to the slow-release material.
[0031] According to an exemplary embodiment, the slow-release material 21 may have a layer gap and / or a pore structure, so that the silicone oil 22 may be, for example, bonded to the surface of the slow-release material and / or adsorbed in the pore and / or layer gap structure. According to an example, the slow-release material 21 may include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material 21 has a porous and / or layered structure and is combined with silicone oil, so that the silicone oil 22 combined with the slow-release material 21 can be slowly released during the use of the cookware with the non-stick coating formed by the ceramic coating of the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick coating formed by the ceramic coating.
[0032] According to an exemplary embodiment, the silicone oil 22 is combined (e.g., adsorbed, bonded) to the sustained-release material 21. And provides the main non-stickiness for the ceramic coating. Here, the silicone oil 22 can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil and polyether modified silicone oil. In addition, by weight percentage, the silicone oil 22 can include 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil, wherein the molecular weight of the low molecular weight silicone oil can be between 500-1000, the molecular weight of the medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of the high molecular weight silicone oil can be between 12000-30000. Here, the silicone oil 22 can be prepared by mixing different molecular weights, because: the silicone oil with a large molecular weight is more firmly bonded to the sustained-release material and the release speed is slower; the silicone oil with a small molecular weight has better free mobility, thereby having better non-stickiness; in addition, the silicone oil with a medium molecular weight takes into account both free mobility and bonding firmness. Therefore, by combining low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil, the sustained release and non-stick effects can be better exerted.
[0033] In addition, in order to improve the bonding strength between the silicone oil and the sustained-release material, a coupling agent may be provided between the sustained-release material and the silicone oil. Here, the coupling agent may include a silane coupling agent. However, the exemplary embodiment is not limited thereto, and the coupling agent may be omitted.
[0034] Preferably, the particle size of the slow-release particles according to the exemplary embodiment may be less than or equal to 20 microns. This is because an excessively large particle size (e.g., greater than 20 microns) tends to have a large impact on the appearance of the formed non-stick coating. More preferably, the particle size of the slow-release particles may be in the range of 8 microns to 15 microns.
[0035] According to an exemplary embodiment, in the ceramic coating 200, 5.15-32.97 parts by weight of the slow-release particles may be included per 100 parts by weight of the ceramic coating 200. This is because when there is too much ceramic coating precursor, the content of the slow-release particles is relatively small, so the slow-release effect is poor, while when the content of the slow-release particles is relatively large, the strength and bonding force of the coating are reduced.
[0036] Figure 1 and Figure 3 A case of a single-layer ceramic coating 200 on the substrate 100 is shown, however, exemplary embodiments are not limited thereto, that is, the ceramic coating (not shown) may also include at least two layers (eg, two layers, three layers, etc.) of ceramic coating.
[0037] In addition, when the ceramic coating 200 is a single layer, the single layer of the ceramic coating 200 may have a thickness in the range of 10 micrometers to 80 micrometers. This is because when the thickness of the ceramic coating 200 is less than 10 micrometers, the wear resistance is insufficient and the ceramic coating is easily worn out; on the contrary, when the thickness of the ceramic coating is greater than 80 micrometers, the coating becomes loose, thereby reducing the impact strength.
[0038] In addition, when the ceramic coating includes a plurality of sub-layers (e.g., a first sub-layer, a second sub-layer, etc.), at least one of the plurality of sub-layers may be identical to the reference Figure 1 The ceramic coating 200 described above has the same structure. For example, when the ceramic coating includes a first sublayer and a second sublayer on the first sublayer, at least the second sublayer on the first sublayer may have the same structure as the reference. Figure 1 The structure of the ceramic coating 200 described is the same as or similar to that of the ceramic coating precursor, and may include a ceramic coating precursor and slow-release particles dispersed in the ceramic coating precursor, and the difference between the first sublayer and the second sublayer may be that the first sublayer includes a small amount of slow-release particles or does not include slow-release particles. That is, when multiple (for example, two) sublayers are provided, the content of the slow-release particles included in each sublayer (that is, the number of slow-release particles included in the sublayer, for example, the density of the slow-release particles in the sublayer) may increase in the direction away from the substrate 100, and the content of the slow-release particles in at least the uppermost sublayer may include 5.15-32.97 parts by weight of the slow-release particles per 100 parts by weight of the sublayer, and there is no specific limitation on the content (for example, density) of the slow-release particles included in the sublayer provided thereunder.
[0039] In addition, although not shown, in order to further slow down the release of silicone oil in the ceramic coating 200 , a sealing layer (not shown) may be further disposed on the ceramic coating 200 .
[0040] The closed layer may include a closed ceramic coating. Here, the closed ceramic coating may be the same as or different from the ceramic coating precursor included in the ceramic coating 200. That is, the closed ceramic coating may be a ceramic coating precursor formed during the preparation of the ceramic coating described below or prepared using a method for preparing a ceramic coating precursor, or the closed ceramic coating may be a ceramic coating conventionally used in the prior art or prepared using a conventional formula. For example, according to an example, a silane substance, an alkaline silica sol, and a non-stick additive may be formulated into a closed ceramic coating according to a general ratio formula.
[0041] The sealing layer does not include the slow-release particles, so as to further slow down the release of the silicone oil in the slow-release particles in the ceramic coating 200. Therefore, the sealing layer may have a thickness of 8 micrometers to 20 micrometers.
[0042] In the above, the non-stick utensil according to the present invention is described in detail in conjunction with the exemplary embodiment. According to the present invention, the non-stick utensil may include a substrate 100 having a surface roughness, a ceramic coating 200 having a single-layer or multi-layer structure, and an optional sealing layer. Hereinafter, a method for manufacturing a non-stick utensil will be described in detail.
[0043] The method of manufacturing a non-stick utensil according to the inventive concept may include: providing a substrate and treating the substrate; preparing a ceramic coating; and forming a ceramic coating 200 on a substrate 100 using the ceramic coating by a laying process.
[0044] According to an exemplary embodiment, the substrate 100 may be a substrate known in the art for making cookware, and may include a stainless steel substrate, an iron substrate, an aluminum substrate, a titanium substrate, etc., and may have various required shapes, and the inventive concept does not limit the substrate. That is, those skilled in the art may use any material on which a ceramic coating is to be applied as the substrate 100 as needed, so that the non-stick utensil conceived by the present invention may be applicable to any scene requiring non-stick. In addition, preferably, the substrate may include two or more composite layers of at least two of aluminum, aluminum alloy, titanium, titanium alloy, stainless steel, and iron.
[0045] When the substrate 100 is provided, the substrate 100 may be functionalized so that the substrate has a surface roughness of 3 microns to 15 microns. Here, the process of functionalizing the substrate 100 may include hard oxidation, shot peening, embossing, car graining, etching, thermal spraying, etc. For example, the substrate 100 may be sandblasted with 60# brown corundum to form a surface roughness of 3 microns to 6 microns, and then the substrate is cleaned and preheated to 40°C to 60°C, and then the ceramic coating formation process is performed.
[0046] Before, during or after providing the substrate 100, a ceramic coating may be provided. According to an exemplary embodiment, the ceramic coating may include a ceramic coating precursor and slow-release particles dispersed in the ceramic coating precursor. Therefore, the step of providing the ceramic coating may include the steps of separately preparing the ceramic coating precursor and the slow-release particles and mixing the ceramic coating precursor with the slow-release particles to obtain the ceramic coating. However, the exemplary embodiment is not limited thereto, that is, the step of preparing the ceramic coating precursor may be combined with the step of preparing the slow-release particles. Below, a method for preparing a ceramic coating according to the present invention by separately preparing a ceramic coating precursor and slow-release particles will be mainly described.
[0047] Preparation of ceramic coating precursors
[0048] According to an exemplary embodiment, the step of preparing the ceramic coating precursor may include a step of providing materials and a step of mixing.
[0049] The step of providing materials may include the steps of separately providing A material, B material and C material.
[0050] Here, material A may include a silane substance, material B may include silica sol and filler as essential components, optional pigments, wetting agents, thickeners and emulsifiers as unnecessary components, and a solvent, and material C may include an organic acid as an essential component, and optional pH buffers and catalysts (zirconium acetate) as unnecessary components.
[0051] In the A material, according to an exemplary embodiment, the silane substance is used to form polysiloxane during the formation of the ceramic coating, and therefore, the silane substance here may include a substance known in the art for polycondensation to form polysiloxane. According to an exemplary embodiment, the silane substance may include at least one of methyltrimethoxysilane, methyltriethoxysilane, and dimethyldimethoxysilane, but is not limited thereto. In addition, in addition to the silane substance, the A material may also include tetraethyl orthosilicate that is polycondensed to form polysiloxane, and in this case, in the A material, by weight percentage, the silane substance may account for 80%-97% of the A material, and the tetraethyl orthosilicate may account for 3%-20% of the A material.
[0052] Material B may necessarily include fillers and silica sol. The filler plays a role in increasing the wear resistance of the coating, etc. Therefore, the present invention does not limit the type of filler, and ordinary commonly used fillers can be selected, for example, at least one of mica powder, kaolin, montmorillonite, silicon carbide, alumina and silicon dioxide can be selected. In addition, silica sol is the main film-forming substance of ceramic coatings, which reacts with polysiloxane under acidic conditions to form a ceramic coating. Therefore, commercially available ordinary silica sol can be selected as the silica sol in material B of the present invention. For example, the silica sol can be Akzo Nobel 1050 (silica sol) or American Grace LUDIXAM-50.
[0053] The necessary components in the B material can be dispersed in a solvent. That is, the B material can also include a solvent. Here, the solvent can include deionized water, and in order to adjust the volatilization rate of the solvent during the coating drying process, the solvent can also include isopropanol. In addition, the ratio between isopropanol and water is unlimited, and the ratio between water and isopropanol can be selectively proportioned according to actual needs.
[0054] In the B material, in addition to the above-mentioned necessary components, one or more of a pigment, a wetting agent, a thickener and an emulsifier may be selectively included as an unnecessary component. Here, the pigment is mainly used to give the coating different colors, so ordinary inorganic pigments can be selected. Inorganic pigments have good temperature resistance and good safety, and inorganic pigments are preferably selected in the high temperature resistant field. According to an exemplary embodiment, at least one of carbon black, copper chrome black, titanium dioxide, iron oxide, etc. may be selected as a filler. In addition, during the preparation of the necessary components in the solvent, in order to provide the excellent properties of the material, at least one of a wetting agent, a thickener and an emulsifier may also be added to the material.
[0055] According to a specific example, the B material may include, by weight percent: 30wt%-48wt% of silica sol, 8wt%-13wt% of pigment, 8wt%-25wt% of filler, 0.2wt%-1wt% of wetting agent, 1wt%-3wt% of thickener, 3wt%-5wt% of emulsifier, and the balance is isopropyl alcohol and deionized water. However, exemplary embodiments are not limited thereto, and one or more of the unnecessary components may be omitted.
[0056] The C material is used as a strong acid catalyst, and may include an organic acid as an essential component, and an optional pH buffer and a catalyst (e.g., zirconium acetate) as an unnecessary component. Here, the organic acid is used to adjust the pH value of the silica sol in the subsequent process so that it can react with the A material in an acidic environment, and therefore, an organic acid commonly used in the art for ceramic coatings can be used. According to an exemplary embodiment, at least one of formic acid and acetic acid can be selected as an organic acid, and when both formic acid and acetic acid are included, the weight ratio between formic acid and acetic acid can be between 4:6 and 1:1. In addition, in the C material, a pH buffer and a catalyst may also be selectively included. Here, the pH buffer and the catalyst may be a pH buffer and a catalyst used in the process of preparing a strong acid catalyst for ceramic coatings known in the art, for example, the pH buffer may be a weak acid such as boric acid, and the catalyst is used to accelerate the reaction rate of the sol-gel, and may be zirconium acetate, etc. However, the exemplary embodiment is not limited to the types of pH buffers and catalysts, and suitable pH buffers and catalysts may be omitted or appropriately selected based on the prior art.
[0057] According to an exemplary embodiment, the C material may include 80-97 parts by weight of a mixture of formic acid and acetic acid, 1-2 parts by weight of a boric acid pH buffer, and 0.5 parts by weight of a zirconium acetate catalyst.
[0058] After providing the above-mentioned materials, a mixing step may be performed. Herein, the mixing step may include a first mixing step of mixing the B material with the C material to obtain the first material and a second step of mixing the result of the first mixing step (ie, the first material) with the A material.
[0059] Specifically, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidic (e.g., less than or equal to 4) by using the acidity of the C material to obtain the first material. Since the C material includes a solid filler and an optional pigment, the C material can be added to a grinder and ground for 0.5h-2h before mixing or during the preparation of the C material, so that it is fully dispersed and ground to a particle size of less than or equal to 15 microns to obtain a uniformly dispersed slurry.
[0060] After the B material and the C material are mixed, the mixture may be tumbling dispersed for a predetermined time (eg, 0.5 h) so that the first material has a high degree of dispersion.
[0061] After obtaining the first material, material A may be added to the first material. Here, the weight ratio of the added amount of material A to material B may be in the range of (20-30):(40-60). After adding material A, the mixture may be shaken evenly so that material A and material B undergo a sol-gel reaction in an acidic environment to form a ceramic coating precursor.
[0062] Preparation of sustained-release granules
[0063] The slow-release particles can be prepared during, before, or after the preparation of the ceramic coating precursor. The slow-release particles can be prepared by mixing the slow-release material with silicone oil.
[0064] According to an exemplary embodiment, the sustained-release particles may include the Figure 1 and Figure 2 The described sustained-release material 21 has a pore structure and / or a layer structure and the silicone oil 22 is combined with (eg, adsorbed, bonded to) the sustained-release material.
[0065] A slow-release material precursor of appropriate size (i.e., a slow-release material before grinding, when the grinding step is omitted, the slow-release material precursor can be considered as the slow-release material used in the end) can be selected to prepare slow-release particles. According to an exemplary embodiment, the slow-release material precursor can have a layer gap and / or pore structure. According to the example, the slow-release material precursor can include at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica hollow glass micropowder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate. The slow-release material precursor has a porous and / or layered structure and the slow-release material formed after grinding is combined with silicone oil. The silicone oil combined with the slow-release material can be slowly released during the use of the cookware with a non-stick coating formed by the ceramic coating conceived by the present invention, thereby greatly improving the long-lasting non-stick performance of the non-stick layer formed by the ceramic coating.
[0066] According to an exemplary embodiment, the particle size of the slow-release material precursor may be within the range of 100 mesh sieve to 3000 mesh sieve, and the particle size of the slow-release material within this range may obey a normal distribution. However, when the particle size is too large (e.g., 100 mesh sieve), the excessively large particle size is likely to increase the grinding process or make the particle size of the slow-release material after grinding too large, which ultimately affects the appearance of the non-stick coating made using the ceramic coating; on the contrary, the particle size is too small (e.g., 3000 mesh sieve, and the particle size will be smaller after grinding) It is not easy to effectively adsorb and bond silicone oil, so it is not easy to achieve a good silicone oil slow-release effect.
[0067] When the slow-release material precursor has the above-mentioned particle size distribution, the particle size of the slow-release material finally obtained can be made to be less than 20 microns (preferably 8 microns-15 microns) by using two grinding processes as described below. However, the exemplary embodiment is not limited to this, that is, when the slow-release material precursor is selected to have a smaller value within the range of 100 mesh-3000 mesh, one grinding process can be omitted; in addition, when the particle size of the slow-release material precursor is selected to have a smaller value within the above-mentioned range, two grinding processes can be omitted. When at least one of the grinding processes is omitted, the omitted grinding process can be replaced by a stirring process, or the mixture can be left untreated.
[0068] Silicone oil can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, and polyether modified silicone oil, and can be mixed by silicone oils of different molecular weights in a certain proportion to form a silicone oil composition with a molecular weight normal distribution; wherein, by weight percentage, the content of low molecular weight silicone oil can be 20wt%-30wt%, the content of medium molecular weight silicone oil can be 40wt%-60wt%, and the content of high molecular weight silicone oil can be 20wt%-30wt%. Here, the molecular weight of low molecular weight silicone oil can be between 500-1000, the molecular weight of medium molecular weight silicone oil can be between 3000-6000, and the molecular weight of high molecular weight silicone oil can be between 12000-30000. By utilizing a normally distributed silicone oil composition, the sustained release and non-stick effects can be better exerted. This is because: the large molecular weight silicone oil is more firmly bonded to the sustained release material and the release speed is slower; the free mobility of small molecular weight silicone oil is better, so it has better non-stickiness; in addition, the medium molecular weight silicone oil takes into account both free mobility and bonding firmness. Therefore, low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil can be combined to better exert the sustained release and non-stick effects.
[0069] 35-58 parts by weight of the slow-release material precursor can be mixed with 42-60 parts by weight of silicone oil to obtain a mixture, and 1 part by weight of a coupling agent (e.g., a methoxysilane coupling agent), 0.3 parts by weight of a catalyst (e.g., a titanate catalyst) and 1-1.5 parts by weight of a dispersant can be added to the mixture. However, exemplary embodiments are not limited thereto, and the coupling agent and the catalyst are used to enhance the bonding force between the silicone oil and the slow-release material, and the dispersant is used to improve the dispersion of the slow-release material in the silicone oil. However, exemplary embodiments are not limited thereto, and at least one of the coupling agent, the catalyst and the dispersant can be omitted.
[0070] According to a specific example, silicone oil, a slow-release material precursor of 100 meshes-3000 meshes, and a silane coupling agent can be mixed evenly, and after grinding to a particle size of less than or equal to 30 microns, a catalyst is added, and the particle size is continued to be less than or equal to 20 microns, and then ultrasonic treatment is performed at room temperature for 0.5h-1h, so that slow-release particles can be obtained. Here, firstly, silicone oil is mixed with the slow-release material and then ground to a particle size of less than or equal to 30 microns, so that silicone oil and the slow-release material can be mixed evenly, and thereafter, grinding to a particle size of less than or equal to 20 microns under the condition of a catalyst can make silicone oil fully firmly adsorbed and bonded to its outside by the slow-release material. However, when the particle size of the slow-release material is less than 30 microns, the first grinding can be omitted, and a stirring process can be optionally provided, or a second grinding process can be directly performed. In addition, when the particle size of the slow-release material is less than 20 microns, the second grinding process can be further omitted, and a stirring process can be optionally provided.
[0071] Preparation of ceramic coatings and optional sealer coatings
[0072] After the ceramic coating precursor and the slow-release particles are prepared, the slow-release particles may be mixed with the ceramic coating precursor to prepare a ceramic coating according to an exemplary embodiment.
[0073] For ceramic coatings including slow-release particles of different numbers and / or sizes, slow-release particles of required size and / or number can be selected and added to the ceramic coating, and after the ceramic coating precursor is mixed with the slow-release particles, the mixture can be stirred and reacted at a speed of 120 rpm to 200 rpm for 6 h to 8 h to obtain the required ceramic coating with different particle sizes and / or numbers.
[0074] Although the above describes a method of obtaining a ceramic coating by separately preparing a ceramic coating precursor and slow-release particles and mixing the ceramic coating precursor with the slow-release particles, in a method of combining the step of preparing a ceramic coating precursor with the step of preparing slow-release particles, as described above, after mixing the B material with the C material, the A material and the slow-release particles can be added to the mixture of the B material and the C material at the same time. For example, 40-60 parts by weight of the B material can be mixed with 1-2 parts by weight of the C material, so that the pH of the mixture is adjusted to acidity (for example, less than or equal to 4) by using the acidity of the C material to obtain the first material. Then, the A material and the slow-release particles can be added to the mixture, where the weight ratio of the addition amount between the A material and the B material can be in the range of (20-30): (40-60). And different addition amounts of the slow-release particles can be adaptively selected based on the requirements of the layer. After mixing, the mixture can be stirred at a speed of 120-200 rpm for 6h-8h to obtain various ceramic coatings as required.
[0075] According to an exemplary embodiment, when a single ceramic coating 200 is provided, 5.15-32.97 parts by weight of slow-release particles may be dispersed in every 100 parts by weight of the ceramic coating 200. In addition, when a plurality of sub-layers are provided, the content of slow-release particles included in each sub-layer may gradually (e.g., a gradient) increase in a direction away from the substrate 100 and satisfy that the sub-layer provided at the top has 5.15-32.97 parts by weight of slow-release particles dispersed in every 100 parts by weight of the sub-layer, or that the sub-layers provided below the top sub-layer have the same or different content of slow-release particles that is less than the content of the top sub-layer.
[0076] In order to further improve the sustained release effect of silicone oil in non-stick utensils, a sealing layer can also be formed on the ceramic coating. Therefore, a sealing coating for forming a sealing layer can be prepared before, during or after the preparation of the ceramic coating.
[0077] According to an exemplary embodiment, the sealing coating may be a ceramic coating commonly used in the art, and thus, may be prepared using a conventional formula in the prior art.
[0078] According to the example, a sealing coating can be prepared by the following method: (1) silane and tetraethyl orthosilicate are mixed and stirred to obtain a component E silane composition; (2) silica sol is mixed with isopropyl alcohol and deionized water, and an emulsifier and a thickener are added to obtain a component F slurry; (3) formic acid, acetic acid, a buffer (e.g., boric acid) and a catalyst (e.g., zirconium acetate) are mixed to obtain a component G strong acid catalyst; (4) the above three components are mixed in sequence according to a mass ratio of E:F:G=(20-30):(40-60):(1-2), and rolling and aging are performed to obtain a sealing coating, wherein the mixing order and aging method are as follows: first, components F and G are mixed evenly according to the required number of parts, the pH is adjusted to below 4, rolling and dispersing for 0.5h, and then the required number of parts of E are added and shaken evenly to obtain the required sealing coating.
[0079] Formation of ceramic coating and optional sealing layer
[0080] After obtaining the ceramic coating (or further sealing coating), the ceramic coating (or further sealing coating) can be sprayed on the preheated substrate 100 described above by air spraying. For example, the ceramic coating (or further sealing coating) can be sprayed by air spraying. Here, the spraying of ceramic coating and sealing coating does not limit the air spraying parameters, and the difference between the spraying of ceramic coating and the spraying of sealing coating can only be that ceramic coatings of different thicknesses are formed by different spraying times. Here, the air spraying parameters are as follows: the spraying distance is 160mm; the air pressure is 0.3MPa; the flow rate is 8L / min. However, the exemplary embodiment is not limited to this, and the parameters of air spraying can be adaptively adjusted according to the specific process, and those skilled in the art can also adopt other methods of forming layers to form ceramic coatings and sealing layers using the ceramic coatings and sealing coatings conceived by the present invention.
[0081] After air spraying, the resultant can be cured at a temperature of 230°C-280°C for 10min-15min to form a single ceramic coating 200 with a thickness of 10 microns-80 microns or a ceramic coating including multiple sub-layers, and a sealing layer with a thickness of 8 microns-20 microns can be optionally further formed on the ceramic coating.
[0082] Through the detailed description above in combination with the exemplary embodiments, the ceramic coating of the non-stick utensil conceived by the present invention includes slow-release particles, so that during the cooking process, the release of silicone oil can be slowed down, thereby maintaining a long-lasting non-stick effect. In addition, by treating the surface of the substrate, the bonding force between the substrate and the ceramic coating can be enhanced. In addition, when a sealing layer is further provided, the slow-release effect of silicone oil can be further improved.
[0083] Hereinafter, embodiments of the inventive concept will be described in detail.
[0084] Example 1
[0085] The ceramic coating is formed by the following method.
[0086] S1: 80 wt % of methyltrimethoxysilane and 20 wt % of ethyl orthosilicate are mixed and stirred uniformly to obtain a silane composition of component A;
[0087] S2: 30wt% of Akzo Nobel 1050 (silica sol), 8wt% of titanium dioxide (pigment), 25wt% of kaolin (filler), 3wt% of Tween-80 (emulsifier), 1wt% of water-based modified bentonite (thickener), 0.3wt% of polyoxyethylene ether TRITON X-100 (wetting agent), 20wt% of isopropanol and the balance of deionized water were mixed evenly, then added to a grinder and ground for 2h, fully dispersed and ground to a particle size of not more than 15 microns, to obtain component B slurry;
[0088] S3: 48 parts by weight of formic acid, 48 parts by weight of acetic acid, 1 part by weight of boric acid (buffer), and 0.5 parts by weight of zirconium acetate (catalyst) are uniformly mixed to obtain component C strong acid catalyst;
[0089] S4: 58 parts by weight of hydroxy silicone oil with a molecular weight of 3000 and 42 parts by weight of vermiculite (slow-release material) with a particle size of 100 to 3000 meshes are mixed, and then 3 parts by weight of methoxysilane coupling agent are added and mixed evenly, and the mixture is ground to a particle size of no more than 30 microns, and then 0.3 parts by weight of titanate (catalyst) is added, and the mixture is further ground to a particle size of no more than 20 microns, and then ultrasonically treated at room temperature of 22° C. for 0.5 h to obtain a slow-release particle component D, and the particle size of the slow-release particle component D obeys a normal distribution;
[0090] S5: The above four components are mixed in order according to the weight ratio of A: B: C: D = 22: 40: 1: 20, and rolled to mature to obtain the ceramic coating. The mixing order and the maturation method are as follows: first, 40 parts by weight of component B and 1 part by weight of component C are mixed evenly, and the pH is adjusted to 4 by component C, and the mixture is rolled and dispersed for 0.5 hours, and then 22 parts by weight of component A are added and shaken evenly, and then 20 parts by weight of component D are added, and the reaction is stirred at a speed of 200 rpm for 8 hours to obtain the desired ceramic coating.
[0091] The non-stick frying pan is manufactured by using the ceramic coating as follows.
[0092] S6: Matrix treatment. The stainless steel frying spoon is sandblasted with 60# brown corundum to form a surface roughness of 3 microns;
[0093] S7: Preheating. Clean the sandblasted substrate and preheat it to 60°C;
[0094] S8: Spraying. The ceramic coating is sprayed on the substrate by air spraying, and the spraying film thickness is 70 microns; the air spraying parameters are as follows: the spraying distance is 160mm; the air pressure is 0.3MPa; and the flow rate is 8L / min.
[0095] S9: Sintering: Curing at 250°C for 10 minutes.
[0096] Through the above method, the non-stick cookware of Example 1 is obtained.
[0097] Example 2
[0098] The difference from Example 1 is that the sustained-release material is bentonite.
[0099] Example 3
[0100] The difference from Example 1 is that the sustained-release material is alpha alumina.
[0101] Example 4
[0102] The difference from Example 1 is that the particle size of the sustained-release granular component is in the range of 8 microns to 12 microns.
[0103] Example 5
[0104] The difference from Example 1 is that the particle size of the sustained-release granular component is in the range of 16 microns to 20 microns.
[0105] Example 6
[0106] The difference from Example 1 is that the particle size of the sustained-release granular component is in the range of 6 microns to 10 microns.
[0107] Example 7
[0108] The difference from Example 1 is that the film thickness is 10 microns.
[0109] Example 8
[0110] The difference from Example 1 is that the film thickness is 40 microns.
[0111] Example 9
[0112] The difference from Example 1 is that A, B, C and D are mixed in sequence according to a weight ratio of A:B:C:D=22:40:1:30 to prepare the ceramic coating.
[0113] Example 10
[0114] The difference from Example 1 is that A, B, C and D are mixed in order according to the weight ratio of A:B:C:D=30:60:2:5 to prepare the ceramic coating.
[0115] Embodiment 11
[0116] The difference from Example 1 is:
[0117] (1) preparing ceramic coating 01 by using step S5;
[0118] (2) further comprising step S51, wherein the step S51 differs from step S5 only in that the components A, B, C and D obtained in steps S1 to S4 are sequentially mixed in a weight ratio of A:B:C:D=22:40:1:1 to prepare ceramic coating 02;
[0119] (3) A first sublayer with a thickness of 35 μm was formed on the substrate using ceramic coating 02 by the air spraying method of Example 1, and a second sublayer with a thickness of 35 μm was formed on the first sublayer using ceramic coating 01 by the air spraying method of Example 1.
[0120] Example 12
[0121] The difference from Example 11 is that the thickness of the first sub-layer is 10 microns.
[0122] Embodiment 13
[0123] The difference from Example 11 is that the thickness of the first sub-layer is 20 microns.
[0124] Embodiment 14
[0125] The difference from Example 11 is that the thickness of the second sub-layer is 10 microns.
[0126] Embodiment 15
[0127] The difference from Example 11 is that the thickness of the second sub-layer is 20 microns.
[0128] Example 16
[0129] The difference from Example 11 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=22:40:1:15 to prepare ceramic coating 02.
[0130] Embodiment 17
[0131] The difference from Example 11 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=22:40:1:30 to prepare ceramic coating 01.
[0132] Embodiment 18
[0133] The difference from Example 1 is:
[0134] (1) preparing ceramic coating 01 by using step S5;
[0135] (2) It also includes using step S52, and the difference between step S52 and step S5 is that: the components A, B and C obtained in steps S1-S3 are mixed in order according to a weight ratio of A:B:C=22:40:1 to prepare ceramic coating 03, that is, the difference between step S52 and S5 is that step S4 is omitted;
[0136] (3) A first sublayer with a thickness of 35 μm was formed on the substrate using ceramic coating 03 by the air spraying method of Example 1, and a second sublayer with a thickness of 35 μm was formed on the first sublayer using ceramic coating 01 by the air spraying method of Example 1.
[0137] Embodiment 19
[0138] The difference from Example 18 is that the thickness of the first sub-layer is 10 microns.
[0139] Embodiment 20
[0140] The difference from Example 18 is that the thickness of the first sub-layer is 20 microns.
[0141] Embodiment 21
[0142] The difference from Example 18 is that the thickness of the second sub-layer is 10 microns.
[0143] Embodiment 22
[0144] The difference from Example 18 is that the thickness of the second sub-layer is 20 microns.
[0145] Embodiment 23
[0146] The difference from Example 18 is that A, B, C and D are mixed in sequence according to the weight ratio of A:B:C:D=22:40:1:30 to prepare ceramic coating 01.
[0147] Embodiment 24
[0148] The difference from Example 1 is that the silicone oil is composed of 20 wt % of hydroxy silicone oil with a molecular weight of 800, 60 wt % of hydroxy silicone oil with a molecular weight of 3000 and 20 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0149] Embodiment 25
[0150] The difference from Example 1 is that the silicone oil is composed of 30 wt % of hydroxy silicone oil with a molecular weight of 800, 40 wt % of hydroxy silicone oil with a molecular weight of 3000 and 30 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0151] Embodiment 26
[0152] The difference from Example 1 is that the silicone oil is composed of 25 wt % of hydroxy silicone oil with a molecular weight of 800, 50 wt % of hydroxy silicone oil with a molecular weight of 3000 and 25 wt % of hydroxy silicone oil with a molecular weight of 12000.
[0153] Embodiment 27
[0154] The difference from the first embodiment is that a sealing layer is further included on the ceramic coating, and the sealing layer is formed by using a sealing material.
[0155] The sealing material is formed by the following method.
[0156] W1: 80 wt% of methyltrimethoxysilane and 20 wt% of ethyl orthosilicate are mixed and stirred uniformly to obtain a component E silane composition;
[0157] W2: 30 wt % of Akzo Nobel 1050 (silica sol), 3 wt % of Tween-80 (emulsifier), 1 wt % of water-based modified bentonite (thickener), 20 wt % of isopropanol and the remainder of deionized water were mixed uniformly to obtain component F slurry;
[0158] W3: 48 parts by weight of formic acid, 48 parts by weight of acetic acid, 1 part by weight of boric acid (buffer), and 0.5 parts by weight of zirconium acetate (catalyst) are uniformly mixed to obtain component G strong acid catalyst;
[0159] W4: The above three components are mixed in order according to the weight ratio of E: F: G = 20: 40: 1, and rolled and matured to obtain a closed coating. The mixing order and the aging method are as follows: first, 20 parts by weight of component F and 1 part by weight of component G are mixed evenly, and the pH is adjusted to 4 by component G, and the mixture is rolled and dispersed for 0.5 hours, and then 40 parts by weight of component E are added and shaken evenly to obtain the required closed coating.
[0160] After the sprayed ceramic coating is formed, a sealing layer with a thickness of 8 μm is formed on the ceramic coating using a sealing coating using the same process as the spraying process for forming the ceramic coating.
[0161] Embodiment 28
[0162] The difference from Example 27 is that the thickness of the sealing layer is 12 microns.
[0163] Embodiment 29
[0164] The difference from Example 27 is that the thickness of the sealing layer is 15 microns.
[0165] Embodiment 30
[0166] The difference from Example 1 is that a functional layer having a surface roughness of 8 μm is formed on the surface of the substrate by thermal spraying using molten titanium.
[0167] Embodiment 31
[0168] The difference from Example 30 is that the surface roughness of the substrate is 15 microns.
[0169] Comparative Example 1
[0170] The difference from Example 1 is that the substrate is not subjected to functionalization treatment to have a smooth surface.
[0171] Comparative Example 2
[0172] The difference from Example 30 is that the surface roughness of the substrate is 20 microns.
[0173] Comparative Example 3
[0174] The difference from Example 1 is that step S4 is omitted. That is, in step S5, components A, B and C are mixed in order according to a weight ratio of A:B:C=22:40:1, and the obtained ceramic coating is used to manufacture non-stick cookware.
[0175] Comparative Example 4
[0176] The difference from Example 11 is that the second sublayer is located on the substrate, and the first sublayer is located on the second sublayer.
[0177] The non-stick properties of the non-stick cookware of the above-mentioned Examples 1-31 and Comparative Examples 1-4 were tested, and the test results are shown in the following table.
[0178]
[0179]
[0180] Performance index test
[0181] The above-obtained cookware was subjected to a performance test, and the specific performance test method is as follows:
[0182] (1) Long-lasting non-stick test method: refer to 4.2.1 Fried egg non-stick test in GB_T 32095.2-2015. The unit is the number of times. The higher the number, the longer the life. The non-stick result is evaluated once every 1000 times, and the number of times when the non-stickiness reaches Level III is recorded.
[0183] (2) Plane wear resistance test method: GB_T 32095.2-2015 4.3.1 Plane wear resistance test, use 3M7447 scouring pad, apply a force of 15N, the frequency is 33 times / minute, and the scouring pad is replaced every 500 times.
[0184] By comparing and analyzing the embodiments 1-31 of the present invention and the comparative examples 1-4, it is found that:
[0185] (1) The substrate surface of Comparative Example 1 was not functionalized, so the coating formed thereon was easy to fall off;
[0186] (2) Since the surface roughness of the substrate in Comparative Example 2 is relatively large, although it has good long-lasting non-stick properties, the surface of the formed coating is too rough, thus affecting the product appearance and user experience;
[0187] (3) The conventional ceramic coating in comparative example 3 has a long-lasting non-stickiness of no more than 500 times, while the ceramic coating according to the present invention has a long-lasting non-stickiness of 10,000-25,000 times;
[0188] (4) Although Comparative Example 4 includes two sublayers, the content of sustained-release particles in the uppermost sublayer is lower than the content of sustained-release particles in the lower sublayer. Therefore, the test performance of the ceramic coating with a double-layer structure formed is lower than the test performance of the ceramic coating in the embodiment.
[0189] Although one or more embodiments of the present invention have been described with reference to the drawings, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the claims.
Claims
1. A non-stick utensil, characterized in that: The non-stick utensil comprises: matrix; A ceramic coating is disposed on the surface of a substrate, wherein the ceramic coating comprises a ceramic coating precursor and slow-release particles dispersed in the ceramic coating precursor, wherein: The sustained-release particles include a sustained-release material and silicone oil combined with the sustained-release material. The sustained-release material comprises at least one of vermiculite, zeolite, bentonite, diatomaceous earth, alpha alumina, silica aerogel, fumed silica, amorphous silica, hollow glass powder, porous silicate, layered silicate, porous phosphate, layered phosphate, porous carbonate, layered carbonate, porous sulfate and layered sulfate, and Wherein, the surface of the substrate has a surface roughness of 3 micrometers to 15 micrometers.
2. The non-stick utensil according to claim 1, characterized in that The particle size of the sustained-release particles is less than or equal to 20 microns.
3. The non-stick utensil according to claim 1, characterized in that The sustained-release particles are contained in an amount of 5.15-32.97 parts by weight per 100 parts by weight of the ceramic coating.
4. The non-stick utensil according to claim 1, characterized in that The thickness of the ceramic coating is in the range of 10 microns to 80 microns.
5. The non-stick utensil according to claim 1, characterized in that The ceramic coating includes at least two sub-layers, and at least an uppermost sub-layer of the at least two sub-layers includes slow-release particles.
6. The non-stick utensil according to claim 5, characterized in that The thickness of each of the sub-layers including the sustained-release particles is not less than 10 micrometers, and the thickness of the ceramic coating is not more than 80 micrometers.
7. The non-stick utensil according to claim 5, characterized in that The content of the sustained-release particles in each sub-layer increases in the direction away from the substrate.
8. The non-stick utensil according to claim 1, characterized in that The substrate includes two or more layers composed of at least two materials selected from aluminum, aluminum alloy, titanium, titanium alloy, iron, and stainless steel.
9. The non-stick utensil according to claim 1, characterized in that: The substrate comprises a base layer and a functional layer arranged between the base layer and the ceramic coating layer, and the surface of the functional layer has a surface roughness of 3 micrometers to 15 micrometers.
10. The non-stick utensil according to claim 1, characterized in that The non-stick utensil further comprises a sealing layer, which is located on the surface of the ceramic coating.
Citation Information
Patent Citations
Nano composite ice-covering-proof coating containing phase change silicone oil and preparation method thereof
CN102676056A
Preparation method of slow-release antifouling composite coating with bionic structure
CN113278360A
Modified ceramic coating, composite coating, preparation methods of modified ceramic coating and composite coating, and cooker
CN115820116A
Modified ceramic coating, composite coating, preparation methods of modified ceramic coating and composite coating, and cooker
CN116082956A
Ceramic-paint coatings
US4074010A