Adhesive as well as preparation method and application thereof
By using a mesh-like adhesive in lithium iron phosphate batteries, combining polyethylene oxide side chains and lithium ions, the problem of poor conductivity of lithium iron phosphate batteries is solved, and the electrochemical and cycling performance of the battery is significantly improved.
Patent Information
- Application Number
- CN202411080307.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-22
- Filing Date
- 2024-08-07
- Publication Date
- 2024-12-03
AI Technical Summary
The organic solvent-based adhesive used in lithium iron phosphate batteries is difficult to process and is easily swelled by the electrolyte, resulting in poor conductivity and lithium conductivity, affecting the electrochemical performance and service life.
Adhesives with a mesh structure are introduced through polyethylene oxide (PEO) side chains and lithium ions to form continuous channels to improve conductivity and stabilize in the electrolyte to avoid adhesive decomposition and chemical gel formation.
It significantly improves the conductivity, energy density and cycling performance of lithium iron phosphate batteries, enhances the cycling stability of the electrodes, and extends the service life of the battery.
Smart Images

Figure BDA0004984791330000021 
Figure BDA0004984791330000121 
Figure FDA0004984791300000011
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of adhesives, and in particular to an adhesive and a preparation method and application thereof. Background Art
[0002] Lithium iron phosphate batteries have excellent cycle performance and safety performance and are widely used in various electronic products and electric vehicles. However, due to the olivine crystal structure of lithium iron phosphate materials, the capacity and rate performance in actual applications are far from the theoretical values, which leads to the deterioration of the conductivity and lithium conductivity of lithium iron phosphate materials. In recent years, with the rapid development of the electric vehicle industry and the energy storage industry, higher requirements have been put forward for the comprehensive performance of lithium iron phosphate batteries.
[0003] As an important component of lithium iron phosphate batteries, although the amount of binder used is very small (about 1%-10% of the electrode mass), it can stabilize the electrode in the battery and enhance the electronic contact between the electrode active material and the conductive agent as well as between the electrode active material and the current collector, thereby overcoming the poor electrical conductivity and lithium conductivity of lithium iron phosphate materials during application, and having a positive impact on the overall performance of lithium batteries.
[0004] The main adhesive used in current lithium iron phosphate batteries is an organic solvent-based adhesive polyvinylidene fluoride (PVDF). However, polyvinylidene fluoride adhesives are difficult to process, are easily swelled by the electrolyte during use, and easily form lithium carbide with metallic lithium, making the electronic and ionic conductivity of the lithium iron phosphate material poor, thereby affecting the electrochemical performance and service life of the lithium iron phosphate battery. Summary of the invention
[0005] In order to improve the conductivity of the adhesive and its stability in the electrolyte, and thus improve the cycle performance of the lithium battery, the present application provides an adhesive and a preparation method and application thereof.
[0006] In a first aspect, the present application provides an adhesive, which adopts the following technical solution:
[0007] An adhesive, wherein the structural formula of the adhesive comprises at least one of Formula I and Formula II:
[0008]
[0009] Wherein, the value of n1 is an integer between 3000 and 10000, the value of n2 is an integer between 3000 and 10000, the value of n3 is an integer between 3000 and 10000, and the value of n4 is an integer between 3000 and 10000;
[0010] The structural formula of the R group includes
[0011] The value of m1 is an integer between 3 and 80, and the value of m2 is an integer between 3 and 80.
[0012] First, the adhesive of the present application has a network structure, which can provide a continuous channel for the deintercalation of lithium ions and the conduction of electrons on the positive electrode sheet, thereby improving the conductivity of the lithium iron phosphate battery; and the polyethylene oxide (PEO) side chain on the adhesive structure can reduce the pairing of lithium ions with hexafluorophosphate ions in the lithium battery electrolyte, thereby increasing the number of free lithium ions in the lithium iron phosphate battery, which helps to improve the energy density and cycle performance of the lithium battery. Second, since lithium ions are introduced into the adhesive, the adhesive can play a certain lithium replenishing role for the positive electrode during the charge and discharge process of the lithium iron phosphate battery, and a large amount of active lithium can pass through the network structure, thereby increasing the lithium ion migration number and significantly improving the conductivity of the lithium battery. The increase in the number of active lithium can also significantly increase the capacity of the lithium battery, thereby improving the electrochemical performance and cycle life of the lithium iron phosphate battery; third, the adhesive with a network structure has excellent stability in the electrolyte, which can prevent the CF bond or CH bond in the adhesive from being decomposed to form double bonds, and the water, amine substances, etc. in the electrolyte have a strong destructive effect on the double bonds, which will have a negative impact on the performance of the adhesive; therefore, using the adhesive of the present application in the electrode preparation process can prevent the electrode from being swollen by the electrolyte during use to produce chemical gel, which causes the lithium iron phosphate active material to have poor adhesion on the current collector, thereby improving the cycle stability of the electrode and contributing to the improvement of the cycle performance of the lithium battery.
[0013] In summary, the adhesive prepared in the present application can significantly improve the electrochemical performance and cycle performance of lithium iron phosphate batteries after being used in lithium iron phosphate batteries.
[0014] In a second aspect, the present application provides a method for preparing an adhesive, using the following technical solution:
[0015] A method for preparing an adhesive comprises the following steps:
[0016] S1, mixing polyethylene glycol with a solvent and heating to obtain a mixed solution;
[0017] S2, heating the mixed solution, adding a polymerization inhibitor thereto and stirring, and continuing to add an organic acid and an inorganic acid to obtain a pretreatment solution;
[0018] S3, adding a lithium source to the pretreatment solution after heating and cooling, and stopping heating after the reaction to obtain a lithium-containing premix;
[0019] S4, mixing the lithium-containing premix, dispersant and deionized water, heating in an inert atmosphere, and continuously adding an initiator and a polymerization monomer to obtain the adhesive.
[0020] By adopting the above steps to prepare the adhesive, the final product has a smaller amount of adsorption of the dispersant, a higher purity and a lower cost; and the lithium-containing premix prepared by the above steps has excellent polymerization properties, which can significantly improve the stability of the molecular structure of the adhesive finally prepared, thereby significantly improving the electrolyte resistance and conductivity of the adhesive.
[0021] Preferably, in S1, the heating temperature is 50-65°C; in S2, the mixed solution is heated to 70-75°C, and the stirring time is 15-30min; in S3, the pretreatment solution is heated to 130-150°C, kept warm for 5-8h, and then cooled to 60-70°C, and the reaction time after adding the lithium source is 0.8-1.2h; in S4, the heating temperature is 50-60°C, the pressure is maintained at 3.4-4.0MPa, and after the initiator and the polymerization monomer are added, the mixture reacts until the pressure drops to 2.5-2.7MPa to obtain the adhesive.
[0022] Preferably, the raw materials used in the preparation process include the following raw materials in parts by weight: 2000-5000 parts of polyethylene glycol, 360-1000 parts of solvent, 5-15 parts of inhibitor, 350-400 parts of organic acid, 50-100 parts of inorganic acid, 20-60 parts of lithium source, 50-115 parts of dispersant, 255-495 parts of initiator, and 51700-82200 parts of polymerization monomer.
[0023] By using polyethylene glycol, an inhibitor, an organic acid and a polymerized monomer, an adhesive with a network structure can be synthesized, thereby accelerating the deintercalation and electron conduction of lithium ions on the positive electrode sheet and improving the electrochemical performance of the lithium iron phosphate battery; and the adhesive has PEO side chains introduced from the polyethylene glycol raw material, which can reduce the pairing of lithium ions with hexafluorophosphate ions in the lithium battery electrolyte, thereby increasing the number of free lithium ions in the lithium iron phosphate battery; further, lithium ions are introduced into the adhesive by adding a lithium source, so that the adhesive can have a lithium replenishing effect on the positive electrode sheet, which helps to significantly improve the cycle performance of the lithium ion battery.
[0024] Preferably, the solvent includes one of an organic solvent and an inorganic solvent; the organic solvent includes at least one of N,N-dimethylformamide and acetone; and the inorganic solvent includes deionized water.
[0025] Preferably, the polymerizable monomer includes vinylidene fluoride monomer.
[0026] Preferably, the molecular weight of the polyethylene glycol is 200-5000 Da.
[0027] By controlling the molecular weight of polyethylene glycol, a network structure channel suitable for the passage of lithium ions can be generated, avoiding poor lithium ion transmission performance or large accumulation of lithium ions at the negative electrode material due to the network structure channel being too narrow or too wide, which is conducive to obtaining an adhesive with excellent conductive properties, thereby improving the electrochemical properties and cycle performance of lithium batteries.
[0028] Preferably, the organic acid includes at least one of maleic acid and itaconic acid.
[0029] Preferably, the inorganic acid includes any one of concentrated sulfuric acid and concentrated nitric acid.
[0030] Preferably, the concentrated sulfuric acid refers to a sulfuric acid aqueous solution with a mass fraction greater than or equal to 70%; and the concentrated nitric acid refers to a nitric acid aqueous solution with a mass fraction greater than or equal to 68%.
[0031] By using concentrated sulfuric acid, the hydroxyl groups in the polyethylene glycol can be protonated to turn it into a good ionic nucleophilic reagent, so that the network cross-linked structure of the finally prepared adhesive is more uniform and dense and the electrolyte resistance of the adhesive is improved.
[0032] Preferably, the lithium source comprises an aqueous solution of lithium hydroxide.
[0033] Preferably, the concentration of the lithium hydroxide aqueous solution is 8wt%-12wt%.
[0034] Preferably, the dispersant includes at least one of hydroxypropyl methyl ether cellulose, polyvinyl alcohol, and cellulose acetate butyrate; and the initiator includes at least one of potassium persulfate and ammonium sulfate.
[0035] In a third aspect, the present application provides a positive electrode sheet, which adopts the following technical solution:
[0036] A positive electrode sheet comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises the binder as described above or the binder prepared by the method as described above.
[0037] In a fourth aspect, the present application provides a lithium-ion battery, which adopts the following technical solution:
[0038] A lithium ion battery comprises a negative electrode sheet, an electrolyte, a separator and the positive electrode sheet as described above. DETAILED DESCRIPTION
[0039] For better understanding and implementation, the technical solution of the present application will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0041] Unless otherwise indicated, all numerical values expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.
[0042] As used herein, "and / or" means one or all of the mentioned elements.
[0043] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.
[0044] All percentages in this application are by weight unless otherwise stated.
[0045] Unless otherwise indicated, "a", "an", "an" and "the" used in this specification are intended to include "at least one" or "one or more". For example, "a component" means one or more components, so more than one component may be considered and may be employed or used in the implementation of the embodiment.
[0046] Example 1
[0047] 1. Preparation of Adhesive
[0048] An adhesive comprising the following raw materials in parts by weight:
[0049] 3500 parts of polyethylene glycol with a molecular weight of 1000-3000Da, 700 parts of N,N-dimethylformamide, 10 parts of benzoquinone, 370 parts of itaconic acid, 75 parts of 80% sulfuric acid aqueous solution, 40 parts of 10wt% lithium hydroxide aqueous solution, 85 parts of hydroxypropyl methyl ether cellulose, 370 parts of potassium persulfate, and 67000 parts of vinylidene fluoride monomer;
[0050] An adhesive is prepared by the following steps:
[0051] Step 1, mixing polyethylene glycol and N,N-dimethylformamide in a light-proof environment, heating to 60° C. and stirring to obtain a mixed solution;
[0052] Step 2, heating the mixed solution to 72° C., adding benzoquinone thereto, stirring for 20 minutes, continuing to add itaconic acid and the above-mentioned aqueous sulfuric acid solution, stirring for 7 minutes to obtain a pretreatment solution;
[0053] Step 3, heating the pretreatment solution to 140° C. and keeping it warm for 6 hours, then cooling it to 65° C., adding the lithium hydroxide aqueous solution thereto, keeping it warm for 1 hour, stopping heating, collecting the material, and obtaining a lithium-containing premix;
[0054] Step 4: Mix the lithium-containing premix obtained in step 3, hydroxypropyl methyl ether cellulose and deionized water, heat at 55° C. in a nitrogen atmosphere and keep the pressure at 3.6 MPa, continue to add potassium persulfate and vinylidene fluoride monomer until the pressure drops to 2.6 MPa, and obtain an adhesive.
[0055] 2. Preparation of positive electrode
[0056] The positive electrode slurry is prepared as follows: the lithium iron phosphate positive electrode active material, the conductive agent acetylene black, and the above-mentioned binder are added to a vacuum mixer in a mass ratio of 97.9:0.9:1.2 for mixing, and then the solvent NMP is added to the mixed slurry, and the mixed slurry is stirred to a uniform state under the action of the vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment. The above-mentioned positive electrode slurry is evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying at room temperature, it is transferred to an oven for further drying, and after drying in the oven, a semi-finished positive electrode sheet is obtained, and then the semi-finished positive electrode sheet is cold pressed and cut to obtain the positive electrode sheet to be assembled.
[0057] 3. Preparation of negative electrode
[0058] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were added into a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4 for mixing, and then deionized water was added as a solvent to the mixture obtained, and the mixed slurry was stirred until it was uniform under the action of the vacuum mixer, thereby obtaining the negative electrode slurry of this embodiment.
[0059] The negative electrode slurry is evenly coated on both surfaces of the negative electrode current collector copper foil, dried at room temperature and then transferred to an oven for further drying. After drying in the oven, a negative electrode sheet semi-finished product is obtained, and then the negative electrode sheet semi-finished product is cold pressed and cut to obtain the negative electrode sheet to be assembled.
[0060] 4. Assembly of lithium batteries
[0061] A commercially available polyethylene film is used as a separator of a lithium-ion battery, and a commercially available electrolyte suitable for a 4.2V (charging upper limit) voltage system battery is used as an electrolyte. The above-mentioned positive electrode sheet, negative electrode sheet and separator are wound together to obtain a bare cell, and the bare cell is packaged, injected, left to stand, formed, and divided to obtain a finished battery.
[0062] Example 2
[0063] 1. Preparation of Adhesive
[0064] An adhesive comprising the following raw materials in parts by weight:
[0065] 2000 parts of polyethylene glycol with a molecular weight of 500-1000Da, 1000 parts of acetone, 5 parts of p-hydroxyanisole, 400 parts of maleic acid, 100 parts of 70% sulfuric acid aqueous solution, 20 parts of 12wt% lithium hydroxide aqueous solution, 115 parts of polyvinyl alcohol, 255 parts of ammonium sulfate, and 82200 parts of vinylidene fluoride monomer;
[0066] An adhesive is prepared by the following steps:
[0067] Step 1, mixing polyethylene glycol and acetone in a light-proof environment, heating to 50° C. and stirring to obtain a mixed solution;
[0068] Step 2, heating the mixed solution to 75° C., adding p-hydroxyanisole thereto, stirring for 15 minutes, continuing to add maleic acid and the above-mentioned sulfuric acid aqueous solution, stirring for 10 minutes to obtain a pretreatment solution;
[0069] Step 3, heating the pretreatment solution to 130° C. and keeping it warm for 8 hours, then cooling it to 60° C., adding the lithium hydroxide aqueous solution thereto, keeping it warm for 1.2 hours, then stopping heating, collecting the material, and obtaining a lithium-containing premix;
[0070] Step 4: Mix the lithium-containing premix in step 3, polyvinyl alcohol and deionized water, heat at 50° C. in a nitrogen atmosphere and keep the pressure at 4.0 MPa, continue to add ammonium sulfate and vinylidene fluoride monomer until the pressure drops to 2.5 MPa, and obtain an adhesive.
[0071] 2. Preparation of positive electrode
[0072] The positive electrode slurry is prepared as follows: the lithium iron phosphate positive electrode active material, the conductive agent acetylene black, and the above-mentioned binder are added to a vacuum mixer in a mass ratio of 97.9:0.9:1.2 for mixing, and then the solvent NMP is added to the mixed slurry, and the mixed slurry is stirred to a uniform state under the action of the vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment. The above-mentioned positive electrode slurry is evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying at room temperature, it is transferred to an oven for further drying, and after drying in the oven, a semi-finished positive electrode sheet is obtained, and then the semi-finished positive electrode sheet is cold pressed and cut to obtain the positive electrode sheet to be assembled.
[0073] 3. Preparation of negative electrode
[0074] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were added into a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4 for mixing, and then deionized water was added as a solvent to the mixture obtained, and the mixed slurry was stirred until it was uniform under the action of the vacuum mixer, thereby obtaining the negative electrode slurry of this embodiment.
[0075] The negative electrode slurry is evenly coated on both surfaces of the negative electrode current collector copper foil, dried at room temperature and then transferred to an oven for further drying. After drying in the oven, a negative electrode sheet semi-finished product is obtained, and then the negative electrode sheet semi-finished product is cold pressed and cut to obtain the negative electrode sheet to be assembled.
[0076] 4. Assembly of lithium batteries
[0077] A commercially available polyethylene film is used as a separator of a lithium-ion battery, and a commercially available electrolyte suitable for a 4.2V (charging upper limit) voltage system battery is used as an electrolyte. The above-mentioned positive electrode sheet, negative electrode sheet and separator are wound together to obtain a bare cell, and the bare cell is packaged, injected, left to stand, formed, and divided to obtain a finished battery.
[0078] Example 3
[0079] 1. Preparation of Adhesive
[0080] An adhesive comprising the following raw materials in parts by weight:
[0081] 5000 parts of polyethylene glycol with a molecular weight of 200-500Da, 360 parts of deionized water, 15 parts of benzoquinone, 350 parts of maleic acid, 50 parts of 90% sulfuric acid aqueous solution, 60 parts of 8wt% lithium hydroxide aqueous solution, 50 parts of cellulose acetate butyrate, 495 parts of potassium persulfate, and 51700 parts of vinylidene fluoride monomer;
[0082] An adhesive is prepared by the following steps:
[0083] Step 1, mixing polyethylene glycol and deionized water in a light-proof environment, heating to 65° C. and stirring until the polyethylene glycol is completely dissolved to obtain a mixed solution;
[0084] Step 2, heating the mixed solution to 70° C., adding benzoquinone thereto, stirring for 30 minutes, continuing to add maleic acid and the above-mentioned sulfuric acid aqueous solution, stirring for 5 minutes to obtain a pretreatment solution;
[0085] Step 3, heating the pretreatment solution to 150° C. and keeping it warm for 5 hours, then cooling it to 70° C., adding the lithium hydroxide aqueous solution thereto, keeping it warm for 0.8 hours, then stopping heating, collecting the material to obtain a lithium-containing premix;
[0086] Step 4: Mix the lithium-containing premix in step 3, cellulose acetate butyrate and deionized water, heat at 60° C. in a nitrogen atmosphere and keep the pressure at 3.4 MPa, continue to add potassium persulfate and vinylidene fluoride monomer until the pressure drops to 2.7 MPa, and obtain an adhesive.
[0087] 2. Preparation of positive electrode
[0088] The positive electrode slurry is prepared as follows: the lithium iron phosphate positive electrode active material, the conductive agent acetylene black, and the above-mentioned binder are added to a vacuum mixer in a mass ratio of 97.9:0.9:1.2 for mixing, and then the solvent NMP is added to the mixed slurry, and the mixed slurry is stirred to a uniform state under the action of the vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment. The above-mentioned positive electrode slurry is evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying at room temperature, it is transferred to an oven for further drying, and after drying in the oven, a semi-finished positive electrode sheet is obtained, and then the semi-finished positive electrode sheet is cold pressed and cut to obtain the positive electrode sheet to be assembled.
[0089] 3. Preparation of negative electrode
[0090] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were added into a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4 for mixing, and then deionized water was added as a solvent to the mixture obtained, and the mixed slurry was stirred until it was uniform under the action of the vacuum mixer, thereby obtaining the negative electrode slurry of this embodiment.
[0091] The negative electrode slurry is evenly coated on both surfaces of the negative electrode current collector copper foil, dried at room temperature and then transferred to an oven for further drying. After drying in the oven, a negative electrode sheet semi-finished product is obtained, and then the negative electrode sheet semi-finished product is cold pressed and cut to obtain the negative electrode sheet to be assembled.
[0092] 4. Assembly of lithium batteries
[0093] A commercially available polyethylene film is used as a separator of a lithium-ion battery, and a commercially available electrolyte suitable for a 4.2V (charging upper limit) voltage system battery is used as an electrolyte. The above-mentioned positive electrode sheet, negative electrode sheet and separator are wound together to obtain a bare cell, and the bare cell is packaged, injected, left to stand, formed, and divided to obtain a finished battery.
[0094] Example 4
[0095] 1. Preparation of Adhesive
[0096] An adhesive comprising the following raw materials in parts by weight:
[0097] 4000 parts of polyethylene glycol with a molecular weight of 3000-5000Da, 800 parts of acetone, 7 parts of benzoquinone, 390 parts of maleic acid, 60 parts of 80% sulfuric acid aqueous solution, 60 parts of 9wt% lithium hydroxide aqueous solution, 90 parts of cellulose acetate butyrate, 300 parts of potassium persulfate, and 70,000 parts of vinylidene fluoride monomer;
[0098] An adhesive is prepared by the following steps:
[0099] Step 1, mixing polyethylene glycol and acetone in a light-proof environment, heating to 55° C. and stirring until the polyethylene glycol is completely dissolved to obtain a mixed solution;
[0100] Step 2, heating the mixed solution to 70° C., adding benzoquinone thereto, stirring for 25 minutes, continuing to add maleic acid and the above-mentioned sulfuric acid aqueous solution, stirring for 7 minutes to obtain a pre-treated solution;
[0101] Step 3, heating the pretreatment solution to 135° C. and keeping it warm for 7 hours, then cooling it to 60° C., adding the lithium hydroxide aqueous solution thereto, keeping it warm for 0.8 hours, then stopping heating, collecting the material to obtain a lithium-containing premix;
[0102] Step 4: Mix the lithium-containing premix in step 3, cellulose acetate butyrate and deionized water, heat at 65° C. in a nitrogen atmosphere and keep the pressure at 3.8 MPa, continue to add potassium persulfate and vinylidene fluoride monomer until the pressure drops to 2.6 MPa, and obtain an adhesive.
[0103] 2. Preparation of positive electrode
[0104] The positive electrode slurry is prepared as follows: the lithium iron phosphate positive electrode active material, the conductive agent acetylene black, and the above-mentioned binder are added to a vacuum mixer in a mass ratio of 97.9:0.9:1.2 for mixing, and then the solvent NMP is added to the mixed slurry, and the mixed slurry is stirred to a uniform state under the action of the vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment. The above-mentioned positive electrode slurry is evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying at room temperature, it is transferred to an oven for further drying, and after drying in the oven, a semi-finished positive electrode sheet is obtained, and then the semi-finished positive electrode sheet is cold pressed and cut to obtain the positive electrode sheet to be assembled.
[0105] 3. Preparation of negative electrode
[0106] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were added into a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4 for mixing, and then deionized water was added as a solvent to the mixture obtained, and the mixed slurry was stirred until it was uniform under the action of the vacuum mixer, thereby obtaining the negative electrode slurry of this embodiment.
[0107] The negative electrode slurry is evenly coated on both surfaces of the negative electrode current collector copper foil, dried at room temperature and then transferred to an oven for further drying. After drying in the oven, a negative electrode sheet semi-finished product is obtained, and then the negative electrode sheet semi-finished product is cold pressed and cut to obtain the negative electrode sheet to be assembled.
[0108] 4. Assembly of lithium batteries
[0109] A commercially available polyethylene film is used as a separator of a lithium-ion battery, and a commercially available electrolyte suitable for a 4.2V (charging upper limit) voltage system battery is used as an electrolyte. The above-mentioned positive electrode sheet, negative electrode sheet and separator are wound together to obtain a bare cell, and the bare cell is packaged, injected, left to stand, formed, and divided to obtain a finished battery.
[0110] Example 5
[0111] An adhesive, which is different from Example 1 in that the molecular weight of the polyethylene glycol is 10000-12000Da; the remaining steps and process parameters are consistent with Example 1.
[0112] Example 6
[0113] An adhesive, which is different from Example 1 in that an aqueous nitric acid solution with a mass fraction of 68% is used instead of the aqueous sulfuric acid solution in Example 1; and the remaining steps and process parameters are consistent with those in Example 1.
[0114] Example 7
[0115] An adhesive, which is different from Example 1 in that the weight portion of the lithium source is 10 parts; the remaining steps and process parameters are consistent with Example 1.
[0116] Example 8
[0117] An adhesive, which is different from Example 1 in that the weight portion of the lithium source is 70 parts; the remaining steps and process parameters are consistent with Example 1.
[0118] Comparative Example 1
[0119] An adhesive, which is different from Example 1 in that the adhesive in this comparative example is commercially available PVDF.
[0120] Test Method
[0121] 1. Electrolyte resistance performance test
[0122] The electrolyte tolerance performance test was performed on the adhesive prepared in the above embodiments and comparative examples. The specific steps are as follows: 70g of the adhesive diluted to 20wt% by the products of each embodiment and comparative example was poured into a mold and transferred to an oven, and baked at 60°C for 8h, 90°C for 4h, 120°C for 2h, and 140°C for 15min to obtain an adhesive film; then the adhesive film was punched into a dumbbell shape, its weight was weighed using a micrometer, its thickness was measured using a micrometer, and the relevant data was recorded as a first adhesive film for standby use. ; Place the first adhesive film in an aluminum-plastic bag, inject 40 times the weight of the electrolyte into the film and seal it; move the packaged aluminum-plastic bag into a 40°C oven and bake it for 15 days; take out the adhesive film in the aluminum-plastic bag, use absorbent paper to absorb the electrolyte on the surface of the film, use a micrometer to weigh its weight, use a micrometer to measure its thickness, record the relevant data, and use it as a second adhesive film; calculate the weight change rate and thickness change rate respectively, and record the calculation results in Table 1; Among them, the smaller the weight change rate and thickness change rate, the better the electrolyte resistance of the adhesive.
[0123] 2. Conductive performance test
[0124] The conductive properties of the adhesives prepared in the above embodiments and comparative examples were tested, and the specific steps are as follows: (1) 70 g of the adhesive diluted to 20 wt % from the products of each embodiment and comparative example was poured into a mold and transferred to an oven, and baked at 60°C for 8 h, 90°C for 4 h, 120°C for 2 h, and 140°C for 15 min to obtain an adhesive film; (2) 5 cm × 5 cm adhesive film was cut, and the conductivity of the film was tested using a conductivity tester. The conductivity of the film is recorded in Table 1.
[0125] 3. Cycle performance test
[0126] The lithium batteries prepared in the above embodiments and comparative examples were subjected to a cycle performance test, and the specific steps are as follows: 1C / 1C cycle test: At 25°C, the prepared battery was charged at a 1C rate and discharged at a 1C rate, and a full charge and discharge cycle test was performed for 1000 cycles, and the capacity retention rate was recorded in Table 1.
[0127] Table 1
[0128]
[0129] In combination with Examples 1-4, Comparative Examples 1-2 and Table 1, it can be seen that by adding polyethylene glycol and introducing a lithium source, not only can a network molecular structure with channels that are conducive to the insertion and extraction of lithium ions be formed in the active material layer of the positive electrode of the lithium battery, but also the content of active lithium in the lithium battery can be significantly increased. Due to the presence of the above-mentioned network structure, the improvement of the conductivity of the lithium battery and the improvement of the capacity and cycle performance of the lithium battery can be further promoted; and the adhesive with a network structure has the lowest weight change rate and thickness change rate, which means that the adhesive prepared in the present application has excellent electrolyte resistance and improves its structural stability in the electrolyte during the cycle of the lithium battery.
[0130] In combination with Example 1, Example 5 and Table 1, it can be seen that when the molecular weight of polyethylene glycol is too high, the weight change rate and thickness change rate of the adhesive increase slightly, and the cycle performance decreases slightly. This is because the change in the molecular weight of polyethylene glycol will cause the ions in the network structure of the adhesive to pass through the pores unevenly, which will have a negative impact on the conductive properties of the adhesive.
[0131] In combination with Example 1, Example 6 and Table 1, it can be seen that when concentrated nitric acid is used in the process of synthesizing the adhesive, the weight change rate and thickness change rate of the adhesive are slightly increased relative to Example 1, and the cycle performance is slightly decreased, but the overall performance is still maintained at a high level; this is because concentrated nitric acid can also increase the protonation degree of hydroxyl groups in polyethylene glycol, which is conducive to the formation of a uniform and stable network structure, improve the conductivity of the adhesive, and have a positive effect on the electrolyte resistance of the adhesive.
[0132] In combination with Example 1, Examples 7-8 and Table 1, it can be seen that by introducing a certain concentration of lithium ions into the binder, the amount of active lithium in the lithium battery can be increased while avoiding the generation of lithium dendrites at the negative electrode of the lithium battery due to the increase in the amount of active lithium; when the amount of lithium source introduced is too small, the amount of -COOLi generated decreases, which may affect the ionic conductivity of the lithium ion battery to a certain extent. In addition, the lithium replenishment effect of the binder on the positive electrode is reduced, which is not conducive to the improvement of the cycle performance of the lithium battery; and when the amount of lithium source introduced is too much, it is easy to cause unbalanced transfer of lithium ions between the positive and negative electrodes of the lithium battery, significantly reducing the overall performance of the lithium battery.
[0133] The above embodiments are only used to illustrate the technical solution of the present application rather than to limit the protection scope of the present application. Although the present application is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solution of the present application can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present application.
Claims
1. An adhesive, Features: The structural formula of the adhesive includes at least one of Formula I and Formula II: Wherein, the value of n1 is an integer between 3000 and 10000, the value of n2 is an integer between 3000 and 10000, the value of n3 is an integer between 3000 and 10000, and the value of n4 is an integer between 3000 and 10000; The structural formula of the R group includes The value of m1 is an integer between 3 and 80, and the value of m2 is an integer between 3 and 80.
2. The method for preparing the adhesive according to claim 1, Features: The steps include: S1, mixing polyethylene glycol with a solvent and heating to obtain a mixed solution; S2, heating the mixed solution, adding a polymerization inhibitor thereto and stirring, and continuing to add an organic acid and an inorganic acid to obtain a pretreatment solution; S3, adding a lithium source to the pretreated solution after heating and cooling, and stopping heating after the reaction to obtain a lithium-containing premix; S4, mixing the lithium-containing premix, dispersant and deionized water, heating in an inert atmosphere, and continuously adding an initiator and a polymerization monomer to obtain the adhesive.
3. The method for preparing the adhesive according to claim 2, Features: In S1, the heating temperature is 50-65°C; In S2, the mixed solution is heated to 70-75° C. and stirred for 15-30 min; In S3, the pretreatment solution is heated to 130-150° C., kept warm for 5-8 hours, and then cooled to 60-70° C., and the reaction time after adding the lithium source is 0.8-1.2 hours; In the S4, the heating temperature is 50-60°C, the pressure is maintained at 3.4-4.0 MPa, and after the initiator and the polymerization monomer are added, the reaction is carried out until the pressure drops to 2.5-2.7 MPa to obtain the adhesive.
4. The method for preparing the adhesive according to claim 2, Features: The raw materials used in the preparation process are calculated by weight and include the following raw materials in parts by weight: 2000-5000 parts of polyethylene glycol, 360-1000 parts of solvent, 5-15 parts of inhibitor, 350-400 parts of organic acid, 50-100 parts of inorganic acid, 20-60 parts of lithium source, 50-115 parts of dispersant, 255-495 parts of initiator, and 51700-82200 parts of polymerization monomer.
5. The method for preparing the adhesive according to claim 4, Features: The molecular weight of the polyethylene glycol is 200-5000Da.
6. The method for preparing the adhesive according to claim 4, Features: The organic acid includes at least one of maleic acid and itaconic acid.
7. The method for preparing the adhesive according to claim 4, Features: The inorganic acid includes any one of concentrated sulfuric acid and concentrated nitric acid.
8. The method for preparing the adhesive according to claim 4, Features: The lithium source includes an aqueous solution of lithium hydroxide.
9. The method for preparing the adhesive according to claim 4, Features: The dispersant includes at least one of hydroxypropyl methyl ether cellulose, polyvinyl alcohol, and cellulose acetate butyrate; the initiator includes at least one of potassium persulfate and ammonium sulfate.
10. A positive electrode sheet, Features: The invention comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises the binder as described in claim 1 or the binder prepared by the method as described in any one of claims 2 to 9.
11. A lithium ion battery, Features: The invention comprises a negative electrode sheet, an electrolyte, a separator and the positive electrode sheet as claimed in claim 10.