Synthesis of yttrium-aluminum-containing SiC ceramic fiber precursor and fiber preparation method
By reacting polysilicasilane with aluminum acetylacetone and yttrium to generate yttrium-containing aluminum SiC ceramic fibers, the problem of abnormal grain growth and spinning of SiC fibers during high-temperature sintering is solved, and high strength, densification and high-temperature stability are achieved , improves the mechanical properties and sintering efficiency of the fiber.
Patent Information
- Application Number
- CN202411174678.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-26
AI Technical Summary
During the high-temperature sintering process, existing SiC ceramic fibers have abnormal grain growth and poor grain uniformity, which leads to the impact of mechanical properties. The polycarbosilane pioneers are prone to form cross-linked network polymers and are difficult to spin.
Polysilica silane reacts with acetylacetonate aluminum and yttrium acetylacetonate to form yttrium-containing aluminum polycarbonsilane. Through melt spinning, iodine non-melting and high-temperature sintering, amorphous Si-C-O-(Y/Al) fibers are formed. Reduce the sintering temperature and increase the density.
The high strength, densification and high temperature stability of SiC fibers are achieved, the fiber diameter becomes smaller, the structure is dense, the mechanical properties are improved, the sintering temperature is reduced, the grain size is increased, the fiber surface is smooth, and the tensile strength is improved.
Smart Images

Figure CN119061530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of ceramic fibers, and in particular relates to a synthesis method of a yttrium-aluminum-containing SiC ceramic fiber precursor and a fiber preparation method. Background Art
[0002] Continuous silicon carbide ceramic fibers have the characteristics of high strength, high modulus, high temperature resistance, oxidation resistance, and high temperature molten salt resistance. They have broad application prospects in the fields of thermal structures of ceramic-based composite materials. At present, they are mainly prepared by the precursor conversion method. This method mainly includes the preparation of the precursor, melt spinning, infusible treatment, high temperature firing and sintering. Among them, the composition and structure of the precursor directly affect the performance of the final ceramic fiber. With the development of science and technology, higher requirements are put forward for the performance of SiC ceramic fibers. At present, the main method for preparing high-performance SiC ceramic fibers is to introduce heterogeneous elements into the precursor to improve the comprehensive performance of SiC ceramic fibers. The key to the process lies in the synthesis of SiC ceramic precursors containing heterogeneous elements. At present, a variety of SiC ceramic precursors containing heterogeneous elements have been synthesized at home and abroad, and the comprehensive performance of the prepared SiC ceramic fibers containing heterogeneous elements has been significantly improved.
[0003] High melting point compounds or heterogeneous elements (such as Ta, Hf, Nb, Ti, Mo, Cr, Zr, etc.) are introduced into SiC ceramic precursors to prepare SiC ceramic fibers containing heterogeneous elements. The main purposes are: 1) to improve the performance of the precursor. After the heterogeneous elements are introduced into the precursor, they can play the role of cross-linking aids due to their valence diversity. In addition, the heterogeneous elements are homogenized at the molecular level in the precursor, and the content is controllable and adjustable, which can improve the rheological properties of the precursor, facilitate the reshaping processing of the precursor, and improve the spinning performance of the precursor; 2) to improve the temperature resistance of SiC fibers. Introducing heterogeneous elements into SiC ceramic precursors, the heterogeneous elements form ultra-high temperature silicides with Si in the fiber, and form ultra-high temperature carbides or intermetallic compounds with C, thereby improving the temperature resistance of SiC ceramics; 3) Diversifying the functions of SiC fibers. After introducing heterogeneous elements into SiC ceramic precursors, the functions of the prepared SiC ceramic fibers can be diversified, such as having excellent microwave absorption performance and electrical properties, which have important application value in military and electronic fields; 4) Assisting sintering and densification. SiC fiber densification is one of the keys to preparing high-performance fibers by the precursor conversion method.
[0004] The heterogeneous elements introduced into SiC ceramic fibers can effectively heal the defects such as holes and cracks generated in the high-temperature sintering process of SiC ceramic fibers, improve the densification degree of SiC ceramic fibers, and improve the performance of SiC ceramic fibers. For example, the introduction of iron in the literature "Transactions of Nonferrous Metals Society of China, 2007, 17 (5): 987-991", the introduction of cobalt in the patent (application number: CN201310374328.5), the introduction of nickel in the literature "Ceramics International, 2022, 48 (14): 20495-20505", and the introduction of titanium in the patent (application number: CN201611054103.1) can give silicon carbide ceramic fibers excellent microwave absorption properties. The introduction of aluminum in the patent (application number: CN200510031778.X), zirconium in the patent (application number: CN201711449898.0), and boron in the patent (application number: CN202011383826.2) can give it higher temperature resistance. For example, in China, Cao Feng et al. used aluminum acetylacetonate (AlAcAc)3) and polysilicon carbosilane (PSCS) to obtain a pale yellow resin-like aluminum-containing SiC ceramic precursor, polyaluminum carbosilane (PACS), after several hours of heat preservation reaction under nitrogen atmosphere. The mass fraction of A1 is generally around 0.4%, Mn is about 1500-2000, and M w The temperature is about 1800-2300℃, and the softening point is about 200℃. The study found that there is a Kumada rearrangement phenomenon in the reaction. The reaction mainly involves Si-H reacting with Al(AcAc)3 to form Si-O-Al bonds, and a small amount of Si-Al-Si bonds are formed. SiC(Al) ceramic fiber is made from PACS. The chemical composition of SiC(Al) ceramic fiber is Si 1.15 O 0.026 Al 0.013 Its main structure is β-SiC with an average grain size of 95nm. Auger electron spectroscopy analysis shows that Si, C, O, and Al elements are evenly distributed inside the ceramic fiber, and the temperature resistance is good. After being treated in argon at 1800℃ for 1h, the strength retention rate of SiC(Al) ceramic fiber is 71%. However, the silicon carbide ceramic fiber obtained by polyaluminocarbosilane has problems such as abnormal grain growth and poor grain uniformity, which affects the mechanical properties of the obtained polycrystalline silicon carbide ceramic fiber.
[0005] The preparation of SiC ceramic fibers described in the above literature usually involves reacting polycarbosilane with an organic reagent to synthesize polycarbosilane containing heterogeneous elements. The prepared polymer easily forms a cross-linked network polymer, which makes spinning impossible. Summary of the invention
[0006] In order to solve the problems existing in the background technology, the purpose of the present invention is to provide a synthesis method of yttrium-aluminum-containing SiC ceramic fiber precursor and a fiber preparation method.
[0007] Compared with polycarbosilane, the present invention uses polysilicon carbosilane (PSCS) to polymerize with aluminum acetylacetonate and yttrium acetylacetonate to generate yttrium aluminum-containing polycarbosilane, and the polymer has good melt spinning performance; compared with air infusibility, air infusibility requires a high temperature and has higher requirements for the precursor, mainly carried out at 200-300°C, while iodine infusibility treatment has a short time and low temperature, which can reduce the cross-linking reaction temperature to 80°C and accelerate the reaction rate; yttrium aluminum-doped precursors are conducive to the preparation of sintered densified and high-temperature resistant silicon carbide ceramic fibers.
[0008] Al and Y can form a yttrium aluminum garnet (YAG) liquid phase system as sintering aids for SiC structural ceramics at high temperatures, which is beneficial to reducing the sintering temperature of SiC ceramics and realizing the densification of SiC ceramics. If the fiber can form a YAG phase at high temperatures, it is beneficial to the densification of SiC fibers. The present invention adopts polysilacarbosilane (PSCS) to react with yttrium acetylacetonate and aluminum acetylacetonate to prepare polyyttrium aluminum polycarbosilane (PYACS), and obtains yttrium aluminum SiC ceramic fibers through melt spinning, iodine infusibility, high temperature firing, sintering and other processes. The fiber cross-linking was achieved by iodine infusibility treatment, and amorphous Si-CO-(Y / Al) fiber was obtained by high-temperature cracking at 1000℃, with a ceramic yield of 73.96%. With the increase of sintering temperature, the SiC fiber prepared by high-temperature sintering at 1900℃ has a higher degree of crystallization, larger grain size, smaller fiber diameter, and gradually denser structure, indicating that the doping of Al and Y at high temperature plays a role in sintering densification. Usually, the spinnable polycarbosilane precursor can be obtained by spinning, air infusibility treatment, high-temperature sintering and sintering to obtain polycrystalline silicon carbide ceramic fiber with good temperature resistance. However, the air infusibility treatment requires a high temperature and has high requirements for the precursor, which is mainly carried out at 200-300℃, because PCS starts to react with oxygen above 150℃, and the iodine infusibility treatment has a short time and low temperature, which can reduce the reaction temperature of PCS and oxygen to 80℃ to accelerate the reaction rate to prepare SiC fiber with low softening point, which has a good application prospect in the field of low-temperature cross-linking (80-150℃).
[0009] The technical solution adopted by the present invention is as follows:
[0010] 1. A Yttrium-aluminum-containing SiC ceramic fiber
[0011] The yttrium-aluminum SiC ceramic fiber precursor is prepared by melt spinning, iodine infusibility, pyrolysis and sintering to obtain the yttrium-aluminum SiC ceramic fiber; the yttrium-aluminum SiC ceramic fiber precursor is obtained by polymerizing polysilicon carbosilane, aluminum acetylacetonate and yttrium acetylacetonate, and then dissolving, filtering and distilling under reduced pressure.
[0012] 2. Synthesis of a Yttrium-Aluminum-Containing SiC Ceramic Fiber Precursor and Preparation Method of Yttrium-Aluminum-Containing SiC Ceramic Fiber
[0013] The following steps are involved:
[0014] Step 1) Synthesis of yttrium-aluminum-containing SiC ceramic fiber precursor: polysilicon carbosilane, organometallic aluminum reagent and organometallic yttrium reagent are placed in a three-necked flask according to a certain ratio;
[0015] The principle of the reaction between PSCS and Al(AcAc)3 and Y(AcAc)3 in the spinnable yttrium aluminum polycarbosilane is: Si-H reacts with the organic metal reagent to introduce the metal element into the precursor molecular structure. The reaction diagram is as follows:
[0016]
[0017] Step 2) heating to a target temperature at a certain heating rate under nitrogen protection and keeping the temperature for a certain time to react, and cooling to room temperature after the reaction is completed to obtain a primary product of yttrium aluminum polycarbosilane;
[0018] Step 3) dissolving the initial product yttrium aluminum polycarbosilane obtained in step 2) in an organic solvent, filtering to remove over-crosslinked products and impurities, and performing reduced pressure distillation to obtain the final spinnable yttrium aluminum polycarbosilane;
[0019] Step 4) adding the spinnable yttrium aluminum polycarbosilane obtained in step 3) into a spinning cylinder, heating to a relatively high temperature under the protection of high-purity nitrogen, standing to degas, then lowering to the spinning temperature, pressurizing with high-purity nitrogen, melt-spinning into filaments through a single-hole spinning plate, and winding onto a receiving cylinder to obtain yttrium aluminum polycarbosilane PYACS fibrils;
[0020] Step 5) Iodine infusibility: The yttrium aluminum polycarbosilane PYACS original fibers and iodine in step 4) are placed in a glass container according to a certain mass, and the temperature is slowly increased to obtain yttrium aluminum polycarbosilane PYACS cross-linked fibers. If the temperature is increased too quickly, the fiber may not be sufficiently infusible, and the fiber may be partially melted and wired during high-temperature sintering, resulting in the fiber becoming stiff and brittle, and the strength is reduced.
[0021] Step 6) placing the yttrium aluminum polycarbosilane PYACS cross-linked wire into a TL1200-12001 resistance tube furnace for high temperature pyrolysis to obtain Si-CO-(Y / Al) fiber;
[0022] Step 7) The pyrolyzed Si-CO-(Y / Al) fiber is placed in a crucible, and placed in a ZT-40-21Y high-temperature vacuum hot-pressing sintering furnace for high-temperature sintering to finally obtain the desired yttrium-aluminum-containing SiC ceramic fiber.
[0023] In the step 1):
[0024] Polysilicon carbosilane is liquid polysilicon carbosilane PSCS;
[0025] The organometallic aluminum reagent is aluminum acetylacetonate Al(AcAc)3;
[0026] The organometallic yttrium reagent is yttrium acetylacetonate Y(AcAc)3;
[0027] Aluminum acetylacetonate and yttrium acetylacetonate are uniformly mixed with polysilicon carbosilane, wherein the mass fraction of the added aluminum acetylacetonate is 1% to 3%, and the mass fraction of the added yttrium acetylacetonate is 1% to 3%.
[0028] In the step 2):
[0029] The heating rate is 5-10℃ / min;
[0030] The target temperature is 400°C and the holding time is 9 to 13 hours.
[0031] The organic solvent in step 3) is one of tetrahydrofuran, benzene, toluene, xylene, n-hexane and cyclohexane.
[0032] The reduced pressure distillation temperature in step 3) is 40°C to 90°C.
[0033] In the iodine infusibility process of step 5), the infusibility temperature is 80° C.-150° C., and the heat preservation time is 3 hours.
[0034] In the step 5), the mass ratio of PYACS fibrils to iodine is 3:5.
[0035] During the infusibility process, iodine reacts with the active groups of the original fibers to crosslink and solidify the fibers. If the iodine content is too low, the fibers will be partially crosslinked and solidified; if the iodine content is too high, the oxygen content of the fibers will increase, affecting the fiber properties. Taking all factors into consideration, the mass ratio of original fibers to iodine is 3:5.
[0036] The high temperature pyrolysis process of step 6) is specifically as follows:
[0037] The heating rate from 20°C to 400°C is 2.5°C / min, the heating rate from 400°C to 800°C is 1.7°C / min, and the heating rate from 800°C to 1000°C is 2.5°C / min.
[0038] The high temperature sintering process of step 7) is specifically as follows:
[0039] The heating rate from 1000°C to 1400°C is 2.5°C / min, the heating rate from 1400°C to 1600°C is 2.5°C / min, and the heating rate from 1600°C to 1900°C is 7.5°C / min.
[0040] After sintering at 1900℃, the SiC crystallization degree of Si-CO-(Y / Al) fiber was higher, the β-SiC grain size increased, the structure gradually became denser, and the fiber diameter became smaller. The doping of Al and Y at high temperature played a role in sintering densification.
[0041] The heating rate of heat treatment has a great influence on the microstructure and mechanical properties of the fiber. A slow heating rate will slow down the grain growth rate and affect the growth of grains. The surface of the fiber sintered quickly is rough, loose and uneven, and has defects such as nodular adhesions, cracks, and grooves. The reduction of the sintering rate not only reduces the microcracks on the fiber surface and inside, but also improves the mechanical properties of the fiber. The fiber surface is very smooth and dense, with a small number of small protrusions. Reducing the sintering rate can increase the tensile strength. This is mainly because the density of the fiber is improved after the microcracks on the fiber surface and inside are reduced or eliminated, and the composition and structure of the fiber are more complete.
[0042] Taking into account the influence of firing rate on fiber properties and production efficiency, the heating rate from 20℃ to 400℃ is 2.5℃ / min, the heating rate from 400℃ to 800℃ is 1.7℃ / min, the heating rate from 800℃ to 1000℃ is 2.5℃ / min, the heating rate from 1000℃ to 1400℃ is 2.5℃ / min, the heating rate from 1400℃ to 1600℃ is 2.5℃ / min, and the heating rate from 1600℃ to 1900℃ is 7.5℃ / min, which is more reasonable.
[0043] The present invention selects yttrium acetylacetonate and aluminum acetylacetonate and polysilicon carbosilane to synthesize yttrium aluminum polycarbosilane, and uses iodine infusibility treatment after melt spinning. Al and Y can form yttrium aluminum garnet (YAG) liquid phase system as SiC structural ceramic sintering aids at high temperature, which is beneficial to reduce the sintering temperature of SiC ceramics and realize the densification of SiC ceramics.
[0044] The beneficial effects of the present invention are:
[0045] (1) The present invention uses liquid low molecular weight polysilicon carbosilane to react with aluminum acetylacetonate and yttrium acetylacetonate to synthesize yttrium aluminum polycarbosilane. Compared with the use of larger molecular weight polycarbosilane reported in the literature, polysilicon carbosilane (PSCS) reacts with aluminum acetylacetonate and yttrium acetylacetonate to synthesize yttrium aluminum polycarbosilane. The polymerization process is not easy to crosslink and solidify, and the polymer has good melt spinning performance;
[0046] (2) The iodine infusibility treatment has a short time and low temperature, which can reduce the reaction temperature of PCS and oxygen to 80°C to accelerate the reaction rate to prepare SiC fibers with low softening points, and can achieve crosslinking at a relatively low temperature (80-150°C);
[0047] (3) SiC ceramic fibers doped with Al and Y sintering aids can form a yttrium aluminum garnet (YAG) liquid phase system at high temperature, which is beneficial to reduce the sintering temperature of SiC ceramics and greatly improve the fiber density. The yttrium aluminum-containing fibers prepared by infusibility, high-temperature firing and sintering have high strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 The chemical reaction formula of the spinnable yttrium-aluminum-containing polycarbosilane prepared by the method of the present invention is:
[0049] Figure 2 The figures are of spinnable yttrium-aluminum polycarbosilane with different aluminum-yttrium contents prepared by the method of the present invention; wherein, a is a digital figure of the spinnable yttrium-aluminum polycarbosilane of Example 1; b is a digital figure of the spinnable yttrium-aluminum polycarbosilane of Example 2; c is a digital figure of the spinnable yttrium-aluminum polycarbosilane of Example 3; d is a digital figure of the spinnable yttrium-aluminum polycarbosilane of Example 4; and e is a digital figure of the spinnable yttrium-aluminum polycarbosilane of Example 5;
[0050] Figure 3 is the gel liquid chromatogram of the precursor of Example 3;
[0051] Figure 4 is an optical image of the PYACS fibril of Example 5;
[0052] Figure 5 The molecular weight, molecular weight distribution and spinning performance of PYACS with different aluminum yttrium contents;
[0053] Figure 6 The SEM images of PYACS fibrils with different aluminum yttrium contents;
[0054] Figure 7 Optical images of PYACS fibrils in Example 3 and Example 5 after non-melting and rapid sintering;
[0055] Figure 8 The SEM images of Si-CO-(Y / Al) fibers sintered in air according to different embodiments;
[0056] Fig. 9 The SEM images of Si-CO-(Y / Al) fibers sintered under argon conditions according to different embodiments.
[0057] Fig.10This is the SEM image of Si-CO-(Y / Al) fiber sintered at the first heating rate in Example 6. DETAILED DESCRIPTION
[0058] The present invention is described in detail below in conjunction with specific implementation cases. The following implementation cases will help those skilled in the art to further understand the present invention, but will not limit the present invention in any form.
[0059] The implementation process of the embodiment of the present invention is as follows:
[0060] Example 1
[0061] Weigh 10.000g of polycarbosilane, 0.1g of aluminum acetylacetonate and 0.2g of yttrium acetylacetonate in a three-necked flask, and heat to 400°C at a heating rate of 5-10°C / min for 9h under nitrogen protection, and cool to room temperature after the reaction to obtain the initial product of yttrium aluminum-containing polycarbosilane. Dissolve the initial product of yttrium aluminum-containing polycarbosilane in n-hexane, filter to remove cross-linked products and impurities, and obtain the final spinnable yttrium aluminum-containing polycarbosilane by vacuum distillation, such as Figure 2 As shown in a, PYACS cross-linked fibers are obtained by melt spinning and iodine infusibility treatment. PYACS fibers are subjected to high-temperature pyrolysis to obtain Si-CO-(Y / Al) fibers, and the obtained Si-CO-(Y / Al) fibers are subjected to high-temperature treatment under air and argon conditions, respectively. SEM is shown in Figure 8 a and Fig. 9 As shown in a.
[0062] Example 2
[0063] Weigh 10.000g of polycarbosilane, 0.2g of aluminum acetylacetonate and 0.2g of yttrium acetylacetonate in a three-necked flask, and heat to 400°C at a heating rate of 5-10°C / min for 9h under nitrogen protection, and cool to room temperature after the reaction to obtain the initial product of yttrium aluminum polycarbosilane. Dissolve the initial product of yttrium aluminum polycarbosilane in n-hexane, filter to remove the cross-linked product and impurities, and obtain the final spinnable yttrium aluminum polycarbosilane by vacuum distillation, such as Figure 2 As shown in b, PYACS cross-linked fibers were obtained by melt spinning and iodine infusibility treatment. PYACS fibers were pyrolyzed at high temperature to obtain Si-CO-(Y / Al) fibers. The obtained Si-CO-(Y / Al) fibers were treated at high temperature in air and argon respectively. SEM images were shown in Figure 8 b and Fig. 9 As shown in b.
[0064] Example 3
[0065] Weigh 10.000g of polycarbosilane, 0.3g of aluminum acetylacetonate and 0.2g of yttrium acetylacetonate in a three-necked flask, and heat to 400°C at a heating rate of 5-10°C / min for 10 hours under nitrogen protection. After the reaction, cool to room temperature to obtain the initial product of yttrium aluminum-containing polycarbosilane. Dissolve the initial product of yttrium aluminum-containing polycarbosilane in n-hexane, filter to remove cross-linked products and impurities, and obtain the final spinnable yttrium aluminum-containing polycarbosilane by vacuum distillation, such as Figure 2 c, a gel permeation chromatogram of the gel containing yttrium aluminum polycarbosilane was obtained by gel permeation chromatography, as shown in FIG. Figure 3 As shown. Then, PYACS cross-linked fibers are obtained through melt spinning and iodine infusibility treatment. PYACS fibers are subjected to high temperature pyrolysis to obtain Si-CO-(Y / Al) fibers. The obtained Si-CO-(Y / Al) fibers are subjected to high temperature treatment under air and argon conditions, respectively. Figure 7 As shown in (a), SEM Figure 8 c and Fig. 9 As shown in c.
[0066] Example 4
[0067] Weigh 10.000g of polycarbosilane, 0.2g of aluminum acetylacetonate and 0.3g of yttrium acetylacetonate in a three-necked flask, and heat to 400°C at a heating rate of 5-10°C / min for 12h under nitrogen protection. After the reaction, cool to room temperature to obtain the initial product of yttrium aluminum-containing polycarbosilane. Dissolve the initial product of yttrium aluminum-containing polycarbosilane in n-hexane, filter to remove the cross-linked product and impurities, and obtain the final spinnable yttrium aluminum-containing polycarbosilane by vacuum distillation, such as Figure 2 d, PYACS cross-linked fibers were obtained by melt spinning and iodine infusibility treatment, and PYACS fibers were pyrolyzed at high temperature to obtain Si-CO-(Y / Al) fibers. The obtained Si-CO-(Y / Al) fibers were treated at high temperature in air and argon respectively. SEM images were shown in FIG. Figure 8 d and Fig. 9 As shown in d.
[0068] Example 5
[0069] Weigh 10.000g of polycarbosilane, 0.3g of aluminum acetylacetonate and 0.3g of yttrium acetylacetonate in a three-necked flask, and heat to 400°C at a heating rate of 5-10°C / min under nitrogen protection for 13h for polymerization. After the reaction, cool to room temperature to obtain the initial product of yttrium aluminum-containing polycarbosilane. Dissolve the initial product of yttrium aluminum-containing polycarbosilane in n-hexane, filter to remove cross-linked products and impurities, and obtain the final spinnable yttrium aluminum-containing polycarbosilane by vacuum distillation, such as Figure 2Then, after melt spinning and iodine infusibility treatment, PYACS cross-linked fibers are obtained. PYACS fibers are subjected to high temperature pyrolysis to obtain Si-CO-(Y / Al) fibers. The obtained Si-CO-(Y / Al) fibers are subjected to high temperature treatment under air and argon conditions, respectively. Figure 7 As shown in (b), SEM Figure 8 d and Fig. 9 d. The optical image of the original fiber obtained after spinning the precursor is shown in Figure 4 shown.
[0070] Example 6
[0071] The PYACS crosslinked fiber in Example 3 was subjected to high temperature cracking to obtain Si-CO-(Y / Al) fiber, and the obtained Si-CO-(Y / Al) fiber was divided into two parts and subjected to high temperature treatment under argon conditions at different heating rates: 1) the heating rate from 20°C to 100°C was 4°C / min, the heating rate from 100°C to 1300°C was 15°C / min, the heating rate from 1300°C to 1600°C was 2.5°C / min, and the heating rate from 1600°C to 1900°C was 7.5°C / min. The SEM images of the finally obtained fibers are as follows: Fig.10 2) The heating rate from 20°C to 400°C is 2.5°C / min, the heating rate from 400°C to 800°C is 1.7°C / min, the heating rate from 800°C to 1000°C is 2.5°C / min, the heating rate from 1000°C to 1400°C is 2.5°C / min, the heating rate from 1400°C to 1600°C is 2.5°C / min, and the heating rate from 1600°C to 1900°C is 7.5°C / min. The SEM of the final fiber is as shown Fig. 9 As shown. Comparing the two heating rates, the fibers sintered at the first heating rate present a loose porous structure, the fibers are not dense, and have almost no mechanical properties. Therefore, considering the influence of the sintering rate on the fiber properties and production efficiency, the heating rates from 20℃ to 400℃ are 2.5℃ / min, 400℃ to 800℃ are 1.7℃ / min, 800℃ to 1000℃ are 2.5℃ / min, from 1000℃ to 1400℃ are 2.5℃ / min, from 1400℃ to 1600℃ are 2.5℃ / min, and from 1600℃ to 1900℃ are 7.5℃ / min, which is more reasonable.
[0072] The experimental conditions of each embodiment are compared. Figure 5As shown in the figure, it can be seen that if the content of heterogeneous elements is too low, it cannot play a role in sintering densification. If it is too high, it will destroy the grain boundary to form an impurity phase that is not conducive to the mechanical properties and high-temperature stability of the fiber. The most suitable spinning conditions for yttrium aluminum polycarbosilane are 3% and 2% of the mass fraction of aluminum acetylacetonate and yttrium acetylacetonate, respectively. The present invention uses liquid polysilicon carbosilane to react with organic aluminum reagents and organic yttrium reagents to synthesize yttrium aluminum polycarbosilane, and the prepared fiber has the advantages of high temperature resistance and high strength. Al and Y can form yttrium aluminum garnet (YAG) liquid phase system as sintering aids for SiC structural ceramics at high temperatures, which is conducive to reducing the sintering temperature of SiC ceramics. The prepared yttrium aluminum fiber has high strength after being infusible, high-temperature sintering and sintering. The iodine infusibility treatment has a short time and low temperature, and can reduce the reaction temperature of PCS and oxygen to 80°C to accelerate the reaction rate to prepare SiC fibers with low softening points. It has good application prospects in the field of low-temperature crosslinking (80-150°C).
[0073] Polycarbosilane (PCS) has a high molecular weight. The traditional method uses PCS to prepare ceramic fibers containing heterogeneous elements. When polymerized, it is easy to cause polymer cross-linking and difficult to spin. In response to this problem, the present invention uses liquid PSCS with a smaller molecular weight and Y(AcAc)3 and Al(AcAc)3 to synthesize aluminum- and yttrium-containing PYACS precursors with uniform molecular weight distribution and excellent spinning performance; compared with air infusibility, the present invention uses iodine infusibility treatment with a short time and low temperature, which can reduce the cross-linking reaction temperature to 80°C and accelerate the reaction rate; in response to the problem that the amorphous SiCxOy phase will cause the fiber structure to be loose and the mechanical properties to drop sharply, the present invention introduces heterogeneous elements aluminum and yttrium. After sintering at a high temperature of 1900°C, the SiC fiber has a higher degree of crystallization, an increased grain size, and a further reduced fiber diameter. The doping of Al and Y at high temperature plays a role in sintering densification.
Claims
1. A yttrium-aluminum-containing SiC ceramic fiber, It is characterized in that The yttrium-aluminum-containing SiC ceramic fiber precursor is prepared through melt spinning, iodine infusibility, pyrolysis and sintering processes to obtain the yttrium-aluminum-containing SiC ceramic fiber; The yttrium-aluminum-containing SiC ceramic fiber precursor is obtained by polymerizing polysilicon carbosilane, aluminum acetylacetonate and yttrium acetylacetonate, and then dissolving, filtering and distilling under reduced pressure.
2. A method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber, It is characterized in that The following steps are included Step 1) Synthesis of yttrium-aluminum-containing SiC ceramic fiber precursor: polysilicon carbosilane, organometallic aluminum reagent and organometallic yttrium reagent are placed in a three-necked flask according to a certain ratio; Step 2) heating to a target temperature at a certain heating rate under nitrogen protection and keeping the temperature for a certain time to react, and cooling to room temperature after the reaction is completed to obtain a primary product of yttrium aluminum polycarbosilane; Step 3) dissolving the initial product yttrium aluminum polycarbosilane obtained in step 2) in an organic solvent, filtering to remove over-crosslinked products and impurities, and performing reduced pressure distillation to obtain the final spinnable yttrium aluminum polycarbosilane; Step 4) adding the spinnable yttrium aluminum polycarbosilane obtained in step 3) into a spinning cylinder, heating to a relatively high temperature under the protection of high-purity nitrogen, standing to degas, then lowering to the spinning temperature, pressurizing with high-purity nitrogen, melt-spinning into filaments through a single-hole spinning plate, and winding onto a receiving cylinder to obtain yttrium aluminum polycarbosilane PYACS fibrils; Step 5) Iodine is not melted: the yttrium aluminum polycarbosilane PYACS fibrils in step 4) and iodine are placed in a glass container according to a certain mass, and the yttrium aluminum polycarbosilane PYACS cross-linked fibers are obtained after heating; Step 6) placing the yttrium aluminum-containing polycarbosilane PYACS cross-linked wire into a resistance tube furnace for high-temperature pyrolysis to obtain Si-CO-(Y / Al) fibers; Step 7) The pyrolyzed Si-CO-(Y / Al) fiber is placed in a crucible, placed in a high-temperature vacuum hot-pressing sintering furnace, and sintered at high temperature to finally obtain the desired yttrium-aluminum-containing SiC ceramic fiber.
3. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: In the step (1): Polysilicon carbosilane is liquid polysilicon carbosilane PSCS; The organometallic aluminum reagent is aluminum acetylacetonate Al (AcAc) 3 ; The organometallic yttrium reagent is yttrium acetylacetonate Y (AcAc) 3 ; Aluminum acetylacetonate and yttrium acetylacetonate are uniformly mixed with polysilicon carbosilane, wherein the mass fraction of the added aluminum acetylacetonate is 1% to 3%, and the mass fraction of the added yttrium acetylacetonate is 1% to 3%.
4. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: In the step 2): The heating rate is 5-10℃ / min; The target temperature is 400°C and the holding time is 9 to 13 hours.
5. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: The organic solvent in step 3) is one of tetrahydrofuran, benzene, toluene, xylene, n-hexane and cyclohexane.
6. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: The reduced pressure distillation temperature in step 3) is 40°C to 90°C.
7. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: In the iodine infusibility process of step 5), the infusibility temperature is 80° C.-150° C., and the heat preservation time is 3 hours.
8. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: In the step (5), the mass ratio of PYACS fibrils to iodine is 3:
5.
9. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: The high temperature pyrolysis process of step 6) is specifically as follows: The heating rate from 20°C to 400°C is 2.5°C / min, the heating rate from 400°C to 800°C is 1.7°C / min, and the heating rate from 800°C to 1000°C is 2.5°C / min.
10. The method for synthesizing a yttrium-aluminum-containing SiC ceramic fiber precursor and preparing a yttrium-aluminum-containing SiC ceramic fiber according to claim 1, Features: The high temperature sintering process of step 7) is specifically as follows: The heating rate from 1000°C to 1400°C is 2.5°C / min, the heating rate from 1400°C to 1600°C is 2.5°C / min, and the heating rate from 1600°C to 1900°C is 7.5°C / min.
Citation Information
Patent Citations
Production method of silicon carbide fiber with high temperature tolerance
CN101319414A
Oxygen-free non-melting Polycarbosilane fiber preparation method and device
CN104088034A
Liquid curable metal-based polycarbosilane and preparation method thereof
CN110563955A
Cited By
SiC-ZrC multiphase continuous ceramic fiber and preparation method thereof
CN119663480A