Method for evaluating coating effect of pellets
The method of evaluating the coating effect of pellet ore solves the problem of difficult evaluating the coating effect in the prior art by sampling before and after the coating of pellet ore and calculating the coating quality and coating rate, and provides comprehensiveness of the coating effect Indicators help enterprises achieve refined production control.
Patent Information
- Application Number
- CN202411174031.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art lacks a method to evaluate the effect of pellet ore coating, which makes it difficult to refine the coating quality control and lacks qualitative or quantitative judgments.
By taking samples before and after coating, measuring and calculating the coating quality and coating rate, comprehensive indicators of coating effect are calculated and the coating effect is judged. Specific methods include detecting the wet matrix volume density, dry matrix volume density and the covering area of the pellet after coating, calculating the coating quality and coverage rate using a two-dimensional coordinate system, and then evaluating the coating effect.
The accurate evaluation of the coating effect of pellet ore is achieved, which helps enterprises achieve refined production control and ensures optimization of coating effect.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and more specifically discloses a method for evaluating the coating effect of pellets. Background Art
[0002] The function of the shaft furnace coating system is to spray the coating agent solution on the surface of the pellets, and the coated pellets are fed into the shaft furnace. The coating layer will prevent the pellets from sticking together and forming lumps due to the high temperature in the shaft furnace during the reduction process. Reduced iron lumps are produced by two or more iron ore particles sticking together to form lumps, usually in the reduction zone of the shaft furnace, where the pellets are in the highest plastic phase. In order to avoid this aggregation problem, the surface of the iron ore is coated with cement slurry or lime solution. The coating agent forms a micro layer on the surface of the raw material, reducing the possible bonding between the Fe of a particle (lump or granule) and the Fe of another particle. These compounds have a high melting point and they will not form bonds between particles at the temperature at which the reduction process is carried out.
[0003] At present, the coating effect is mainly controlled by setting the ratio of coating agent and water, and setting the unit consumption to control the coating quality. This method has certain limitations and cannot truly reflect the coating effect, which is not conducive to the company's refined production control. There is currently a lack of qualitative or quantitative judgment on the actual coating effect of pellets, and there is a lack of a method to evaluate the coating effect. Summary of the invention
[0004] The present invention mainly provides a method for evaluating the coating effect of pellets, which can solve the problem that the prior art lacks a method for evaluating the actual coating effect of pellets.
[0005] To solve the above technical problems, according to one aspect of the present invention, more specifically, a method for evaluating the coating effect of pellets is provided, wherein the pellets are sampled before and after coating, the coating quality of the obtained samples is measured and calculated, and the coating rate is calculated by sampling, and a comprehensive index for judging the coating effect is calculated by the coating quality and the coating rate; wherein:
[0006] The calculation method of pellet coating quality is:
[0007] The wet basis bulk density of pellets sampled before coating is ρ0 (unit: kg / m 3 ), the dry basis volume density is ρ1 (unit: kg / m 3 ), the dry basis volume density of the pellets after coating is ρ2 (unit: kg / m 3 ), the mass of coating agent per ton of pellets is calculated as (unit: kg):
[0008]
[0009] The calculation method of pellet coverage is:
[0010] After coating, sample n regularly shaped pellets, classify and count them according to the rules by observation; the number of pellets with a coating area greater than 2 / 3 is n1, and the coating area is counted as 5 / 6 of the ball; the number of pellets with a coating area greater than 1 / 3 and less than 2 / 3 is n2, and the coating area is counted as 1 / 2 of the ball; the number of pellets with a coating area greater than 0 and less than 1 / 3 is n3, and the coating area is counted as 1 / 6 of the ball; uncoated pellets are not counted; the pellet coating rate is calculated as follows:
[0011]
[0012] The calculation method of CE, a comprehensive index of coating effect, is as follows:
[0013] Ideal index: The coating mass of pellets is m0, the coating rate is s0, and the comprehensive index coordinates of the coating effect in the two-dimensional coordinate system are (m0, s0);
[0014] Actual measurement indicators: The coating mass of pellets is m, the coating rate is s, and the comprehensive index coordinates of the coating effect in the two-dimensional coordinate system are (m, s). The coating effect CE is calculated as follows:
[0015]
[0016] The calculation result of CE, a comprehensive index of coating effect, may be positive or negative, but the closer the result is to 0, the better the coating effect.
[0017] The beneficial effect of the method for evaluating the coating effect of pellets of the present invention is as follows: compared with the current method of controlling the coating quality by setting the ratio of the coating agent to water and setting the unit consumption to reflect the coating effect, the method for evaluating the coating effect of pellets provided by the present invention performs pellet sampling before coating and after coating, calculates the coating quality and the coating rate of the obtained samples, and calculates a comprehensive index of the coating effect by the coating quality and the coating rate, thereby truly reflecting the coating effect of the pellets, which is beneficial to the enterprise's refined production control. DETAILED DESCRIPTION
[0018] The present invention is described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.
[0019] According to one aspect of the present invention, a method for evaluating the coating effect of pellets is provided, wherein the pellets are sampled before and after coating at the chute before and after coating, respectively, and the obtained samples are dried in a sample drying oven in a laboratory, and then the obtained samples are measured and the coating quality is calculated, and the coating rate is calculated by sampling, and a comprehensive index for judging the coating effect is calculated by the coating quality and the coating rate; wherein:
[0020] The bulk density test is carried out in accordance with the national standard GB / T 34568-2017 "Determination of bulk density of iron ore for blast furnace and direct reduction".
[0021] The calculation method of pellet coating quality is:
[0022] The wet basis bulk density of pellets sampled before coating is ρ0 (unit: kg / m 3 ), the dry basis volume density is ρ1 (unit: kg / m 3 ), the dry basis volume density of the pellets after coating is ρ2 (unit: kg / m 3 ), the mass of coating agent per ton of pellets is calculated as (unit: kg):
[0023]
[0024] The calculation method of pellet coverage is:
[0025] After coating, sample n regularly shaped pellets, classify and count them according to the rules by observation; the number of pellets with a coating area greater than 2 / 3 is n1, and the coating area is counted as 5 / 6 of the ball; the number of pellets with a coating area greater than 1 / 3 and less than 2 / 3 is n2, and the coating area is counted as 1 / 2 of the ball; the number of pellets with a coating area greater than 0 and less than 1 / 3 is n3, and the coating area is counted as 1 / 6 of the ball; uncoated pellets are not counted; the pellet coating rate is calculated as follows:
[0026]
[0027] The calculation method of CE, a comprehensive index of coating effect, is as follows:
[0028] Ideal index: The coating mass of pellets is m0, the coating rate is s0, and the comprehensive index coordinates of the coating effect in the two-dimensional coordinate system are (m0, s0);
[0029] Actual measurement indicators: The coating mass of pellets is m, the coating rate is s, and the comprehensive index coordinates of the coating effect in the two-dimensional coordinate system are (m, s). The coating effect CE is calculated as follows:
[0030]
[0031] The calculation result of CE, a comprehensive index of coating effect, may be positive or negative, but the closer the result is to 0, the better the coating effect.
[0032] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention also fall within the protection scope of the present invention.
Claims
1. A method for evaluating the coating effect of pellets, characterized in that: By sampling the pellets before and after coating, measuring and calculating the coating quality of the samples, and calculating the coating rate by sampling, a comprehensive index for judging the coating effect is calculated by the coating quality and the coating rate; wherein: The calculation method of pellet coating quality is: The wet basis bulk density of pellets sampled before coating is ρ0 (unit: kg / m 3 ), the dry basis volume density is ρ1 (unit: kg / m 3 ), the dry basis volume density of the pellets after coating is ρ2 (unit: kg / m 3 ), the mass of coating agent per ton of pellets is calculated as (unit: kg): The calculation method of pellet coverage is: After coating, sample n regularly shaped pellets, classify and count them according to the rules by observation; the number of pellets with a coating area greater than 2 / 3 is n1, and the coating area is counted as 5 / 6 of the ball; the number of pellets with a coating area greater than 1 / 3 and less than 2 / 3 is n2, and the coating area is counted as 1 / 2 of the ball; the number of pellets with a coating area greater than 0 and less than 1 / 3 is n3, and the coating area is counted as 1 / 6 of the ball; uncoated pellets are not counted; the pellet coating rate is calculated as follows: The calculation method of CE, a comprehensive index of coating effect, is as follows: Ideal index: The coating mass of pellets is m0, the coating rate is s0, and the comprehensive index coordinates of the coating effect in the two-dimensional coordinate system are (m0, s0); Actual measurement indicators: The coating mass of pellets is m, the coating rate is s, and the comprehensive index coordinates of the coating effect in the two-dimensional coordinate system are (m, s). The coating effect CE is calculated as follows: The calculation result of CE, a comprehensive index of coating effect, may be positive or negative, but the closer the result is to 0, the better the coating effect.