Photosensitive film

A photosensitive film with controlled absorbance layers addresses the low resolution and undercut resistance issues in negative resin compositions, achieving improved hole formation and adhesion in semiconductor devices.

CN119065200APending Publication Date: 2024-12-03AJINOMOTO CO INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410677861.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Negative photosensitive resin compositions used in semiconductor devices exhibit low resolution and poor undercut resistance, particularly when forming through holes in thick insulating layers, resulting in an inverted cone shape and reduced adhesion to copper foil.

Method used

A photosensitive film comprising a support with two layers of photosensitive resin composition, where the difference in absorbance between the layers is controlled between 0.05 and 0.5, utilizing specific resins, photoradical generators, and photocrosslinking agents to enhance undercut resistance and adhesion.

Benefits of technology

The solution provides a cured product with excellent undercut resistance and improved adhesion to copper foil, enabling the formation of small-diameter holes with enhanced resolution and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004864734390000031
    Figure BDA0004864734390000031
  • Figure BDA0004864734390000032
    Figure BDA0004864734390000032
  • Figure BDA0004864734390000091
    Figure BDA0004864734390000091
Patent Text Reader

Abstract

Provided is a photosensitive film or the like having excellent undercut resistance. The photosensitive film is provided with a supporting body and a photosensitive resin composition layer arranged on the supporting body. The photosensitive resin composition layer has, in order from the support body side, a first photosensitive resin composition layer containing a first photosensitive resin composition, and a second photosensitive resin composition layer containing a second photosensitive resin composition provided on the first photosensitive resin composition layer. The first photosensitive resin composition and the second photosensitive resin composition each contain: (A) one or more resins selected from among polyimides and polyimide precursors; (B) a photoradical generator; and (C) a photo-crosslinking agent. The difference between the absorbance of the second photosensitive resin composition layer and the absorbance of the first photosensitive resin composition layer is 0.05-0.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photosensitive film, a method for manufacturing a semiconductor package substrate using the same, a semiconductor package substrate, and a semiconductor device. Background Art

[0002] In the past, a negative photosensitive resin composition containing a photosensitive polyimide resin or a precursor thereof having excellent heat resistance and insulation properties was sometimes used in the insulating layer of a semiconductor device (see, for example, Patent Document 1). In addition, in recent years, with the increase in communication speed and capacity of communication equipment, excellent resolution is sought in the photosensitive resin composition used for forming an insulating layer of a semiconductor package substrate or the like of a wafer-level package (WLP) or the like of the communication equipment. Prior art literature Patent Literature

[0003] Patent Document 1: Japanese Patent Application Publication No. 2003-084435 Summary of the invention Problems to be solved by the invention

[0004] On the other hand, sometimes it is desirable to form the insulating layer containing polyimide resin thicker. However, it is known that negative photosensitive resin compositions generally have low resolution, and in particular, when a hole (through hole) is formed in a thick insulating layer, the resolution of the lower layer portion is reduced, and therefore, the problem of the cross section of the through hole presenting an inverted cone shape becomes more obvious.

[0005] Specifically, regarding exposure, crosslinking using free radicals is usually performed from the exposure surface of the photosensitive resin composition layer, and as the position moves away from the exposure surface of the photosensitive resin composition layer, the crosslinking using free radicals decreases. If the crosslinking is not much, the solubility relative to the developer is poor. Therefore, in the cross section obtained by cutting the photosensitive resin composition layer using a plane in the thickness direction, the cross-sectional shape of the hole presents an inverted cone shape in which the diameter of the bottom formed at the deepest part is larger than the diameter of the opening formed on the exposure surface, which may become obvious especially when the film thickness of the photosensitive resin composition layer is thick. At this time, the difference between the radius of the opening corresponding to the top of the hole and the radius of the bottom corresponding to the deepest part of the hole (radius of the bottom - radius of the top) is sometimes called "undercut", and the property that the opening shape is not easy to present an inverted cone is called "undercut resistance".

[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a photosensitive film capable of obtaining a cured product having excellent undercut resistance; a method for manufacturing a semiconductor package substrate using the photosensitive film; and a semiconductor package substrate and a semiconductor device. Means for solving problems

[0007] The present inventors have conducted intensive research to solve the above-mentioned problems. As a result, the present inventors have found that by having a first photosensitive resin composition layer and a second photosensitive resin composition layer as the photosensitive resin composition layer, adjusting the (A) one or more resins selected from polyimide and polyimide precursor, (B) a photo radical generator, and (C) a photocrosslinking agent contained in the first photosensitive resin composition and the second photosensitive resin composition constituting the first photosensitive resin composition layer so that the difference in absorbance between the first photosensitive resin composition layer and the second photosensitive resin composition layer is 0.05 or more and 0.5 or less, the above-mentioned problems can be solved, and the present invention has been completed. That is, the present invention includes the following technical solutions.

[0008] [1] A photosensitive film comprising a support and a photosensitive resin composition layer provided on the support, The photosensitive resin composition layer includes, in order from the support side, a first photosensitive resin composition layer including a first photosensitive resin composition and a second photosensitive resin composition layer provided on the first photosensitive resin composition layer including a second photosensitive resin composition. The first photosensitive resin composition and the second photosensitive resin composition respectively include: (A) one or more resins selected from polyimide and polyimide precursors; (B) a photoradical generator; and (C) a photocrosslinking agent, The difference between the absorbance of the second photosensitive resin composition layer and the absorbance of the first photosensitive resin composition layer (absorbance of the second photosensitive resin composition layer−absorbance of the first photosensitive resin composition layer) is 0.05 or more and 0.5 or less. [2] The photosensitive film according to [1], wherein the component (A) contains a structural unit represented by the following formula (A-1). [Chemistry 1] (wherein A each independently represents a tetravalent organic group, B represents a divalent organic group, and R 1 and R 2 Each independently represents a hydrogen atom or a monovalent organic group. ) [3] The photosensitive film according to [2], wherein R in formula (A-1) 1 and R 2 Each independently, and at least one is a free radical reactive group. [4] The photosensitive film according to [3], wherein the radical reactive groups are each independently represented by the following formula (A-2). [Chemistry 2] (In formula (A-2), R 4a , R 5a and R 6a Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and X represents a divalent organic group. * represents a bond. ) [5] The photosensitive film according to any one of [1] to [4], wherein the component (B) comprises (B-1) a highly reactive photoradical generator and (B-2) a photoradical generator having excellent deep curability. [6] The photosensitive film according to any one of [1] to [5], wherein the content of the component (B) contained in the first photosensitive resin composition is smaller than the content of the component (B) contained in the second photosensitive resin composition. [7] The photosensitive film according to any one of [1] to [6], wherein the content of the component (B) in the first photosensitive resin composition is 0.03 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the component (A) in the first photosensitive resin composition. [8] The photosensitive film according to any one of [1] to [7], wherein the content of the component (B) in the second photosensitive resin composition is 0.05 parts by mass or more and 8 parts by mass or less relative to 100 parts by mass of the component (A) in the second photosensitive resin composition. [9] The photosensitive film according to any one of [1] to [8], wherein the absorbance of the first photosensitive resin composition layer is 0.2 or more and 1.5 or less.

[10] The photosensitive film according to any one of [1] to [9], wherein the absorbance of the second photosensitive resin composition layer is 0.3 or more and 1.5 or less.

[11] The photosensitive film according to any one of [1] to

[10] , wherein the nonvolatile component of the first photosensitive resin composition is 100% by mass, and the content of the component (B-1) in the first photosensitive resin composition is b-1. 1-1 , the content of the component (B-1) in the second photosensitive resin composition is set to b 2-1 When b 1-1 / b 2-1 It is 0.1 or more and 3 or less.

[12] A semiconductor package substrate comprising an insulating layer, wherein the insulating layer comprises a cured product of the photosensitive resin composition layer of the photosensitive film according to any one of [1] to

[11] .

[13] A semiconductor device comprising the semiconductor package substrate described in

[12] .

[14] A method for manufacturing a semiconductor package substrate, comprising: A step of laminating the photosensitive resin composition layer of the photosensitive film described in any one of [1] to

[11] on a circuit board; a step of irradiating the photosensitive resin composition layer with active light; and A step of developing the photosensitive resin composition layer.

[15] A method for manufacturing a semiconductor package substrate, comprising: A step of coating a second photosensitive resin composition on a circuit substrate to form a second photosensitive resin composition layer; A step of coating the first photosensitive resin composition on the second photosensitive resin composition layer to form the first photosensitive resin composition layer; a step of irradiating the first photosensitive resin composition layer and the second photosensitive resin composition layer with active light; and a step of developing the first photosensitive resin composition layer and the second photosensitive resin composition layer, The first photosensitive resin composition and the second photosensitive resin composition respectively include: (A) one or more resins selected from polyimide and polyimide precursors; (B) a photoradical generator; and (C) a photocrosslinking agent, The difference in absorbance between the first photosensitive resin composition layer and the second photosensitive resin composition layer is 0.05 or more and 0.5 or less. Effects of the Invention

[0009] According to the present invention, a photosensitive film capable of obtaining a cured product having excellent undercut resistance, a method for producing a semiconductor package substrate using the photosensitive film, and a semiconductor package substrate and a semiconductor device can be provided. DETAILED DESCRIPTION

[0010] Hereinafter, the present invention will be described in detail by showing embodiments and examples. However, the present invention is not limited to the embodiments and examples listed below, and can be implemented with any changes within the scope of the claims and their equivalents.

[0011] [Photosensitive film] The photosensitive film of the present invention is a photosensitive film having a support and a photosensitive resin composition layer disposed on the support, wherein the photosensitive resin composition layer has, from the support side, a first photosensitive resin composition layer comprising a first photosensitive resin composition and a second photosensitive resin composition layer disposed on the first photosensitive resin composition layer, comprising a second photosensitive resin composition, wherein the first photosensitive resin composition and the second photosensitive resin composition respectively comprise: (A) one or more resins selected from polyimide and polyimide precursor, (B) a photoradical generator, and (C) a photocrosslinking agent, and the difference between the absorbance of the second photosensitive resin composition layer and the absorbance of the first photosensitive resin composition layer is 0.05 or more and 0.5 or less. By using such a photosensitive film, a cured product having excellent undercut resistance can be obtained. In addition, a cured product having excellent limiting resolution and excellent adhesion to copper foil can also be obtained.

[0012] The photosensitive film of the present invention has a support, a first photosensitive resin composition layer, and a second photosensitive resin composition layer in sequence. Therefore, when the photosensitive resin composition layer is stacked on a stacking object member such as a circuit substrate, the second photosensitive resin composition layer is bonded to the stacking object member. Therefore, when a hole is formed in the photosensitive resin composition layer, the second photosensitive resin composition layer is located in the deepest part of the hole. In the present invention, since the difference between the absorbance of the second photosensitive resin composition layer and the absorbance of the first photosensitive resin composition layer is 0.05 or more and 0.5 or less, the absorbance of the second photosensitive resin composition layer is greater than the absorbance of the first photosensitive resin composition layer. Therefore, the second photosensitive resin composition layer is cross-linked by free radicals in the same manner as the first photosensitive resin composition layer, and even if the film thickness of the photosensitive resin composition layer is thick, the undercut resistance is excellent.

[0013] The photosensitive resin composition layer of the photosensitive film can be used as a positive photosensitive resin composition or a negative photosensitive resin composition layer, but is preferably a negative photosensitive resin composition from the viewpoint of undercut resistance. Therefore, the first photosensitive resin composition and the second photosensitive resin composition constituting the photosensitive resin composition layer can be used as negative photosensitive resin compositions.

[0014] <Support> The photosensitive film includes a support, and a first photosensitive resin composition layer is formed on the support.

[0015] Examples of the support include polyethylene terephthalate films (PET films), polyethylene naphthalate films, polypropylene films, polyethylene films, polyvinyl alcohol films, triacetyl acetate films, and the like. Polyethylene terephthalate films are particularly preferred.

[0016] Examples of commercially available supports include polypropylene films such as "Alfan MA-410" and "E-200C" manufactured by Oji Paper Co., Ltd., "GF-1" and "GF-8" manufactured by Tamapore Co., Ltd., and polypropylene films manufactured by Shin-Etsu Film Co., Ltd.; and PS series polyethylene terephthalate films such as "PS-25" manufactured by Teijin Co., Ltd., but are not limited to these. For easy removal, these supports are preferably coated with a release agent such as a silicone coating agent or a non-silicone coating agent on the surface. Examples of supports whose surfaces are treated with such a release agent include "AL-5" manufactured by Lintech Co., Ltd.

[0017] The thickness of the support is preferably in the range of 5 μm to 100 μm, more preferably in the range of 10 μm to 50 μm.

[0018] <Photosensitive resin composition layer> The photosensitive film includes a photosensitive resin composition layer. The photosensitive resin composition layer includes a first photosensitive resin composition layer and a second photosensitive resin composition layer in order from the support side. The first photosensitive resin composition layer includes a first photosensitive resin composition, and the second photosensitive resin composition layer includes a second photosensitive resin composition, and the types of components and / or their blending ratios are different so that the difference in absorbance between the first photosensitive resin composition layer and the second photosensitive resin composition layer is 0.01 or more and 0.5 or less.

[0018] The absorbance of the first photosensitive resin composition layer is preferably 0.2 or more, more preferably 0.3 or more, further preferably 0.33 or more or 0.35 or more, and is preferably 1.5 or less, more preferably 1.3 or less, further preferably 1.2 or less. The absorbance is the absorbance at 365 nm, and the absorbance can be measured by the method described in the examples described later.

[0019] The absorbance of the second photosensitive resin composition layer is preferably 0.3 or more, more preferably 0.33 or more, and even more preferably 0.35 or more, and is preferably 1.5 or less, more preferably 1.3 or less, and even more preferably 1.2 or less. The absorbance is the absorbance at 365 nm, and the absorbance can be measured by the method described in the examples below.

[0020] The difference between the absorbance of the second photosensitive resin composition layer and the absorbance of the first photosensitive resin composition layer (absorbance of the second photosensitive resin composition layer - absorbance of the first photosensitive resin composition layer) is 0.05 or more, preferably 0.06 or more, and more preferably 0.07 or more. The upper limit is 0.5 or less, preferably 0.45 or less, and more preferably 0.4 or less. The difference between the absorbance of the second photosensitive resin composition layer and the absorbance of the first photosensitive resin composition layer can be adjusted to the range by, for example, adjusting any one of the types and contents of (A) one or more resins selected from polyimide and polyimide precursor contained in the first photosensitive resin composition layer and the second photosensitive resin composition layer, and (B) any one of the types and contents of the photoradical generator. In particular, it is easy to adjust to the range by adjusting any one of the types and contents of the photoradical generator (B) contained in the first photosensitive resin composition layer and the second photosensitive resin composition layer.

[0021] The thickness of the first photosensitive resin composition layer is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, and is preferably 100 μm or less, more preferably 75 μm or less, and even more preferably 50 μm or less.

[0022] The thickness of the second photosensitive resin composition layer is preferably 10 μm or more, more preferably 15 μm or more, and further preferably 20 μm or more, and is preferably 100 μm or less, more preferably 75 μm or less, and further preferably 50 μm or less.

[0023] The thickness of the photosensitive resin composition layer (the total thickness of the first photosensitive resin composition layer and the second photosensitive resin composition layer. Hereinafter, it is sometimes referred to as "film thickness") is preferably 20 μm or more, more preferably 30 μm or more, further preferably 40 μm or more, and particularly preferably 50 μm or more, and is preferably 150 μm or less, more preferably 120 μm or less, further preferably 100 μm or less, and particularly preferably 80 μm or less.

[0024] The first photosensitive resin composition layer includes a first photosensitive resin composition, and the second photosensitive resin composition layer includes a second photosensitive resin composition. The first photosensitive resin composition and the second photosensitive resin composition respectively include (A) one or more resins selected from polyimide and polyimide precursors, (B) a photoradical generator, and (C) a photocrosslinking agent. Hereinafter, (A) one or more resins selected from polyimide and polyimide precursors are sometimes referred to as "polyimide-based resins".

[0025] The first photosensitive resin composition and the second photosensitive resin composition may further contain (D) other additives and (E) a solvent as needed. Hereinafter, each component that can be contained in the first photosensitive resin composition and the second photosensitive resin composition will be described.

[0026] In the following description, the term "optionally having a substituent" with respect to a compound or a group means both the case where hydrogen atoms of the compound or group are not substituted by a substituent and the case where a part or all of the hydrogen atoms of the compound or group are substituted by a substituent, unless otherwise stated.

[0027] In the following description, the term "organic group" means a group containing at least carbon atoms as backbone atoms unless otherwise specified, and may be linear, branched or cyclic.

[0028] -(A) Polyimide-based resin- The first photosensitive resin composition and the second photosensitive resin composition contain, as component (A), one or more resins (polyimide resins) selected from polyimide and polyimide precursors. The polyimide in component (A) is a resin containing multiple imide structures in the molecule. In addition, the polyimide precursor in component (A) is a resin that can form a polyimide by ring closure by heating. By using component (A), the limiting resolution of the photosensitive film can be improved.

[0029] (A) component can be used alone or in combination of two or more. Thus, (A) component can contain only polyimide, only polyimide precursor, or a combination of polyimide and polyimide precursor. Among them, as (A) component, from the viewpoint of limiting resolution, it is preferred to contain a polyimide precursor.

[0030] As a polyimide precursor, a resin containing more than one structural unit selected from amic acid structural units and amic acid ester structural units can be used. The amic acid structural unit refers to a structural unit having a structure obtained by reacting a carboxylic acid dianhydride with a diamine compound. The amic acid structural unit usually contains a carboxyl group. The amic acid ester structural unit refers to a structural unit having a structure obtained by esterifying a part or all of the carboxyl group, or a structural unit having a structure obtained by reacting a part or all of the carboxyl group with an epoxy group of an epoxy compound containing an ethylenically unsaturated bond. An ethylenically unsaturated bond refers to a non-aromatic carbon-carbon unsaturated bond, for example, a non-aromatic carbon-carbon double bond and a carbon-carbon triple bond.

[0031] From the viewpoint of improving the limiting resolution, the polyimide precursor preferably contains an indane skeleton in the polyamic acid ester structural unit. The indane skeleton represents the skeleton shown in the following formula (a1-1). When the polyamic acid ester structural unit contains the indane skeleton, the solubility of the non-exposed portion of the photosensitive resin composition layer relative to the developer can be improved. Thus, the development time can be shortened, and it is further preferred that the resolution can be improved. "Resolution" means the property of being able to form small-diameter holes in the photosensitive resin composition by exposure and development unless otherwise stated. Generally speaking, the smaller the diameter of the hole that can be formed, the better the resolution. Among them, the polyimide precursor preferably contains a trimethyl indane skeleton shown in the following formula (a1-2). The polyamic acid ester structural unit preferably contains an indane skeleton in the structural portion derived from the diamine compound. [Chemistry 3]

[0032] Carboxylic acid dianhydride represents a dianhydride of a carboxylic acid containing two anhydride groups (i.e., -CO-O-CO-) and an aliphatic carbon or aromatic carbon bonded to the anhydride group. As specific examples of carboxylic acid dianhydride, aliphatic acid dianhydride and aromatic acid dianhydride can be listed. Aliphatic acid dianhydride represents a dianhydride of a carboxylic acid containing two anhydride groups and an aliphatic carbon bonded to the anhydride group. Aromatic acid dianhydride represents a dianhydride of a carboxylic acid containing two anhydride groups and an aromatic carbon bonded to the anhydride group. As a specific example of aliphatic acid dianhydride, aliphatic tetracarboxylic dianhydride can be listed. As a specific example of aromatic acid dianhydride, aromatic tetracarboxylic dianhydride can be listed. These tetracarboxylic dianhydrides can be used alone or in combination of two or more.

[0033] The aliphatic carbon in the aliphatic acid dianhydride is usually a saturated aliphatic carbon. Preferably, the anhydride group is bonded to the saturated aliphatic chain, and a ring structure is formed by the anhydride groups and saturated aliphatic chains bonded together. The ring structure is usually a heterocycle containing oxygen atoms and carbon atoms, preferably a 5-membered ring or a 6-membered ring, and more preferably a 5-membered ring. In addition, the aliphatic acid dianhydride may contain unsaturated aliphatic chains and aromatic chains at positions other than the position directly bonded to the anhydride group.

[0034] The molecular weight of the aliphatic acid dianhydride is preferably not more than 400. By setting the molecular weight within the above range, swelling of the first photosensitive resin composition layer during development can be suppressed or the residual film ratio can be effectively increased.

[0035] Examples of the aliphatic acid dianhydride include 1,2,4,5-cyclohexanetetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.1]heptane-2-endo-3-endo-5-exo-6-exo-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.1]heptane-2-exo-3-exo-5-exo-6-exo-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride, 2-(3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthyl)succinic dianhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, and 1,2,3,4-butanetetracarboxylic dianhydride. Among them, 2-(3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthyl)succinic dianhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, 1,2,3,4-butanetetracarboxylic dianhydride, etc. are mentioned.

[0036] Specific examples of the aromatic acid dianhydride include 4,4'-oxydiphthalic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, pyromellitic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-p-terphenyltetracarboxylic dianhydride, 3,3',4,4'-m-terphenyltetracarboxylic dianhydride, and decahydro-dimethylnaphthalenetetracarboxylic dianhydride.

[0037] As the diamine compound, for example, bis[2-(3-aminopropoxy)ethyl]ether, 1,4-butanediol-bis(3-aminopropyl)ether, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraspiro-5,5-undecane, 1,2-bis(2-aminoethoxy)ethane, 1,2-bis(3-aminopropoxy)ethane, triethylene glycol-bis(3-aminopropyl)ether, polyethylene glycol-bis(3-aminopropyl)ether, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraspiro-5,5-undecane, 1,4-butanediol-bis(3-aminopropyl)ether, etc. can be listed. One diamine compound can be used alone or two or more can be used in combination. In addition, as the diamine compound, a diamine compound containing an aromatic ring can be used. Among them, the diamine compound preferably contains an indane skeleton. Examples of the diamine compound containing an indane skeleton include diamine compounds represented by the following formulae (a2-1) to (a2-10). Among them, diamine compounds represented by formulae (a2-4) to (a2-7) are preferred, and diamine compounds represented by formula (a2-4) are more preferred. [Chemistry 4]

[0038] As the epoxy compound containing an ethylenically unsaturated bond, a compound containing an ethylenically unsaturated bond and an epoxy group can be used. The epoxy group can be contained in the form of a glycidyl group. If examples of epoxy compounds containing ethylenically unsaturated bonds are listed, for example, glycidyl acrylate, glycidyl methacrylate, 4-hydroxybutyl acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl methacrylate, etc. can be listed. The epoxy compound containing an ethylenically unsaturated bond can be used alone or in combination of two or more.

[0039] The polyimide precursor preferably contains a radical reactive group in the molecule of the polyimide precursor. The radical reactive group refers to a reactive group that can be polymerized by means of free radicals generated by heat or light, and examples thereof include groups containing non-aromatic carbon-carbon unsaturated bonds. When a polyimide precursor containing a radical reactive group is used, the polyimide precursor is cross-linked by exposure, which can effectively reduce the solubility of the photosensitive resin composition layer relative to the developer. The radical reactive group may be contained in, for example, the esterified portion of the amic acid ester structural unit.

[0040] In addition, when the polyamic acid ester structural unit is a structural unit having a structure obtained by reacting a part or all of the carboxyl groups with the epoxy group of the epoxy compound containing an ethylenically unsaturated bond, since the epoxy compound contains an ethylenically unsaturated bond, the epoxy compound residue may contain an ethylenically unsaturated bond. Therefore, the epoxy compound residue can function as a radical reactive group.

[0041] As one embodiment of the polyimide precursor, it is preferred that the polyimide precursor includes a structural unit represented by the following formula (A-1). [Chemistry 5] (In formula (A-1), A represents a tetravalent organic group, B represents a divalent organic group, and R 1 and R 2 Each independently represents a hydrogen atom or a monovalent organic group. )

[0042] In formula (A-1), A represents a tetravalent organic group. The number of carbon atoms of A is preferably 6 to 40. Examples of the tetravalent organic group include a tetravalent organic group containing an aliphatic hydrocarbon group and a tetravalent organic group containing an aromatic hydrocarbon group.

[0043] The aliphatic hydrocarbon group contained in the tetravalent organic group contains an aliphatic carbon, and the carbonyl group shown in the aforementioned formula (A-1) is bonded to the aliphatic carbon. The aforementioned aliphatic carbon is usually a saturated aliphatic carbon. Preferably, the tetravalent organic group contains a saturated aliphatic chain, and the carbonyl group shown in the aforementioned formula (A-1) is bonded to the saturated aliphatic chain. The saturated aliphatic chain preferably contains a carbon chain with 2 or 3 carbon atoms connecting the two carbonyl groups shown in the aforementioned formula (A-1), and preferably contains a carbon chain with 2 carbon atoms. The saturated aliphatic chain containing a carbon chain with 2 carbon atoms connecting the two carbonyl groups shown in the aforementioned formula (A-1) can be obtained by reacting an aliphatic acid dianhydride containing an acid anhydride group forming a 5-membered ring with a diamine compound. The saturated aliphatic chain having 3 carbon atoms connecting two carbonyl groups represented by the above formula (A-1) can be obtained by reacting an aliphatic acid dianhydride having an acid anhydride group forming a 6-membered ring with a diamine compound.

[0044] The aromatic hydrocarbon group contains an aromatic group to which the carbonyl group shown in the above formula (A-1) is bonded. Specifically, -COOR 1 Base and-COOR 2 The aromatic group or alicyclic aliphatic group (R 1 and R 2 With R in formula (A-1) 1 and R 2 Same) etc.

[0045] As one embodiment of A, for example, a tetravalent aliphatic hydrocarbon group optionally having a substituent can be listed. The tetravalent aliphatic hydrocarbon group can be a saturated aliphatic hydrocarbon group or an unsaturated aliphatic hydrocarbon group. In addition, the tetravalent aliphatic hydrocarbon group can be a chain hydrocarbon group, a cyclic hydrocarbon group (i.e., an alicyclic hydrocarbon group), or a combination thereof. Furthermore, the chain hydrocarbon group can be either a straight chain or a branched chain. Among them, from the viewpoint of particularly improving the developability, the tetravalent aliphatic hydrocarbon group preferably contains an aliphatic carbocyclic ring, and more preferably, the carbonyl group shown in the aforementioned formula (A-1) is bonded to the aliphatic carbocyclic ring. The number of carbonyl groups bonded to the aliphatic carbocyclic ring is preferably 2 or more.

[0046] For A, as a substituent that the tetravalent organic group may optionally have, there can be listed, for example, a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, n-butyl; alkenyl groups such as vinyl, allyl, propenyl, butenyl; halogen atoms such as fluorine atoms, chlorine atoms, bromine atoms; alkoxy groups having 1 to 10 carbon atoms, such as methoxy, ethoxy, propoxy; hydroxyl groups; halogen atom-substituted alkyl groups such as trifluoromethyl, etc. These substituents may be optionally bonded to form a ring. The above-mentioned substituents may optionally further have a substituent (hereinafter sometimes referred to as a "secondary substituent"). The substituent may be one or more.

[0047] The range of the formula weight of A is preferably not more than 328. When the formula weight of A is within the above range, swelling of the photosensitive resin composition during development can usually be suppressed or the residual film rate can be effectively increased.

[0048] Examples of A include groups represented by the following formulae (a3-1) to (a3-12): In the formulae, * represents a bond. [Chemistry 6]

[0049] In formula (A-1), B represents a divalent organic group. The divalent organic group may contain an aromatic ring. In addition, the divalent organic group preferably contains an aromatic ring. In addition, the divalent organic group may contain an indane skeleton. The divalent organic group may contain an aromatic ring in addition to the indane skeleton.

[0050] As the divalent organic group represented by B, for example, the groups (a4-1) to (a4-30) exemplified below can be cited. In addition, a group formed by combining two or more of the groups (a4-1) to (a4-30) can be used as the divalent organic group. Among them, as B, preferably, the groups (a4-2), (a4-21) to (a4-30) are groups, more preferably, (a4-2), (a4-24) to (a4-27) are groups, and further preferably, the groups (a4-2) or (a4-24) are groups. In the formula, * represents a bond. [Chemistry 7] [Chemistry 8] [Chemistry 9] [Chemistry 10]

[0051] The above-mentioned divalent organic group may have a substituent. As the substituent, for example, the same examples as those for the tetravalent organic group may have are given. The substituent may be one or two or more.

[0052] In formula (A-1), R 1 and R 2Each independently represents a hydrogen atom or a monovalent organic group. Examples of the monovalent organic group include free radical reactive groups and saturated aliphatic groups having 1 to 4 carbon atoms, preferably free radical reactive groups. Examples of free radical reactive groups include groups containing ethylenically unsaturated bonds. Specific examples of free radical reactive groups include vinyl, allyl, propargyl, ethynyl, phenylethynyl, butenyl, maleimide, nadicimide, (meth)acryloyl, and groups represented by formula (A-2) described below. "(Meth)acryloyl" includes methacryloyl, acryloyl, and combinations thereof. Preferably, R of formula (A-1) 1 and R 2 Each independently, at least one is a radical reactive group, and more preferably both are radical reactive groups.

[0053] As the radical reactive group, a group represented by the following formula (A-2) is preferred. 1 and R 2 Each is independently a group represented by the following formula (A-2). [Chemistry 11] (In formula (A-2), R 4a , R 5a and R 6a Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and X represents a divalent organic group. * represents a bond. )

[0054] In formula (A-2), R 4a ~R 6a Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms. Examples of the aliphatic hydrocarbon group having 1 to 3 carbon atoms include an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, a n-propyl group, and a 2-propyl group, among which a methyl group is preferred.

[0055] In formula (A-2), X represents a divalent organic group. The divalent organic group optionally contains heteroatoms such as oxygen atoms and nitrogen atoms. It is preferred to have a heteroatom as a substituent. As the divalent organic group, there can be listed: a divalent aliphatic hydrocarbon group optionally having a substituent, a divalent aromatic hydrocarbon group optionally having a substituent, etc. Among them, as the divalent organic group, it is preferably a divalent aliphatic hydrocarbon group optionally having a substituent.

[0056] The divalent aliphatic hydrocarbon group optionally having a substituent may be linear, branched or cyclic. In addition, the divalent aliphatic hydrocarbon group may be saturated or unsaturated. The number of carbon atoms in the divalent aliphatic hydrocarbon group is preferably 1 to 10, more preferably 1 to 5. Examples of the divalent aliphatic hydrocarbon group include alkylene, alkenylene, alkynylene, etc.

[0057] Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group.

[0058] Examples of the alkenylene group include vinylene, propenylene, butenylene, pentenylene, and hexenylene.

[0059] Examples of the alkynylene group include an ethynylene group and a propynylene group.

[0060] Among them, the divalent aliphatic hydrocarbon group which may have a substituent is preferably an alkylene group having 1 to 10 carbon atoms which may have a substituent, more preferably an alkylene group having 1 to 5 carbon atoms which may have a substituent, further preferably an alkylene group having 1 to 3 carbon atoms which may have a substituent, and particularly preferably an ethylene group, a propylene group or a 2-hydroxypropylene group.

[0061] The number of carbon atoms of the divalent aromatic hydrocarbon group which may have a substituent is preferably 6 to 20, more preferably 6 to 15. Examples of the divalent aromatic hydrocarbon group which may have a substituent include an arylene group, and examples of the arylene group include 1,2-phenylene, 1,3-phenylene, 1,4-phenylene, naphthylene, anthrylene, biphenylene, and 9,9-diphenyl-9H-fluorenylene.

[0062] The divalent aliphatic hydrocarbon group and the divalent aromatic hydrocarbon group may have a substituent. As the substituent, the same examples as the substituents that the tetravalent organic group in A may have are given, among which a hydroxyl group is preferred. The substituent may be one or more.

[0063] As formula (A-2), for example, the groups (a5-1) to (a5-6) shown below can be cited. Among them, as formula (A-2), the group (a5-1), the group (a5-3) or the group (a5-4) is preferred, and the group (a5-1) is more preferred. In the formula, * represents a bond. [Chemistry 12]

[0064] The component (A) preferably has a structural unit represented by the following formula (A-3). [Chemistry 13] (In formula (A-3), A 1arepresents a tetravalent organic group containing an aliphatic hydrocarbon group, B a Represents a divalent organic group, R 1a and R 2a Each independently represents a monovalent organic group containing an ethylenically unsaturated bond.

[0065] In formula (A-3), A 1a A represents a tetravalent organic group containing an aliphatic hydrocarbon group. 1a The same as the tetravalent organic group containing an aliphatic hydrocarbon group represented by A in formula (A-1).

[0066] In formula (A-3), B a represents a divalent organic group and is the same as B in the formula (A-1).

[0067] In formula (A-3), R 1a and R 2a Each independently represents a monovalent organic group containing an ethylenically unsaturated bond. Examples of the monovalent organic group containing an ethylenically unsaturated bond include vinyl, allyl, propargyl, ethynyl, phenylethynyl, butenyl, maleimide, nadicimide, (meth)acryloyl, and the group represented by formula (A-3a). Preferably R 1a and R 2a Each is independently represented by the following formula (A-3a). [Chemistry 14] (In formula (A-3a), R 4b , R 5b and R 6b Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms; a represents an integer from 0 to 10; * represents a bond. )

[0068] In formula (A-3a), R 4b ~R 6b Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and R in formula (A-2) 4a ~R 6a same.

[0069] In formula (A-2), p a It represents an integer of 0 to 10, preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and further preferably 0.

[0070] The component (A) preferably has a structural unit represented by the following formula (A-4a) or the following formula (A-4b). [Chemistry 15] (In formula (A-4a) and formula (A-4b), A 2a Each independently represents a tetravalent organic group, R 11 and R 12 Each independently represents a hydrogen atom or a monovalent organic group, R 13 Each independently represents a hydrogen atom or a methyl group, Xa each independently represents a single bond, a group represented by the following formula (a6-1) or a group represented by the formula (a6-2), and Xb each independently represents a single bond, a group represented by the formula (a6-3) or a group represented by the formula (a6-4). m1 represents an integer of 1 to 5. [Chemistry 16] (In formulas (a6-1) to (a6-4), * represents a bonding bond.)

[0071] In formula (A-4a) and formula (A-4b), A 2a Each independently represents a tetravalent organic group. 2a The same as A in formula (A-1).

[0072] In formula (A-4a) and formula (A-4b), R 11 and R 12 Each independently represents a hydrogen atom or a monovalent organic group. 11 and R 12 With R in formula (A-1) 1 and R 2 same.

[0073] In formula (A-4a) and formula (A-4b), Xa each independently represents a single bond, a group represented by formula (a6-1) or a group represented by formula (a6-2). Examples of the group represented by formula (a6-1) include 1,2-phenylene, 1,3-phenylene, 1,4-phenylene and the like. Examples of the group represented by formula (a6-2) include the following groups (a6-2-1) to (a6-2-6). Among them, Xa is preferably a group represented by formula (a6-1), more preferably 1,4-phenylene. In the following formula, * represents a bond. [Chemistry 17]

[0074] In formula (A-4a) and formula (A-4b), Xb each independently represents a single bond, a group represented by formula (a6-3) or a group represented by formula (a6-4). As the group represented by formula (a6-3), for example, 1,2-phenylene, 1,3-phenylene, 1,4-phenylene, etc. can be listed. As the group represented by formula (a6-4), for example, the following groups (a6-4-1) to (a6-4-3) can be listed. Among them, as Xb, a single bond is preferred. In the following formula, * represents a bonding bond. [Chemistry 18]

[0075] In formula (A-4a) and formula (A-4b), R 13 Each independently represents a hydrogen atom or a methyl group, preferably a methyl group.

[0076] In formula (A-4a) and formula (A-4b), m1 each independently represents an integer of 1 to 5, preferably an integer of 1 to 3, more preferably 2 or 3, and even more preferably 3.

[0077] The component (A) preferably has a structural unit represented by the following formula (A-5a) or the following formula (A-5b). [Chemistry 19] (In formula (A-5a) and formula (A-5b), A 3a Each independently represents a tetravalent organic group containing an aliphatic hydrocarbon group, R 1b and R 2b Each independently represents a monovalent organic group containing an ethylenically unsaturated bond, R 13a Each independently represents a hydrogen atom or a methyl group, Xa 1 Each independently represents a single bond, a group represented by the following formula (a7-1) or a group represented by the following formula (a7-2), Xb 1 Each independently represents a single bond, a group represented by formula (a7-3) or a group represented by formula (a7-4). m2 represents an integer of 1 to 5. [Chemistry 20] (In formulas (a7-1) to (a7-4), * represents a bonding bond.)

[0078] In formula (A-5a) and formula (A-5b), A 3a Each independently represents a tetravalent organic group. 3a The same as A in formula (A-1).

[0079] In formula (A-5a) and formula (A-5b), R 1a and R 1bEach independently represents a monovalent organic group containing an ethylenically unsaturated bond. 1a and R 1b and R in formula (A-3) 1a and R 2a same.

[0080] In formula (A-5a) and formula (A-5b), Xa 1 Each independently represents a single bond, a group represented by formula (a6-1) or a group represented by formula (a6-2). 1 The same as Xa in formula (A-4a) and formula (A-4b).

[0081] In formula (A-5a) and formula (A-5b), Xb 1 Each independently represents a single bond, a group represented by the formula (a6-3) or a group represented by the formula (a6-4). 1 The same as Xb in formula (A-4a) and formula (A-4b).

[0082] In formula (A-5a) and formula (A-5b), R 13a Each independently represents a hydrogen atom or a methyl group, preferably a methyl group.

[0083] In the formula (A-5a) and the formula (A-5b), m2 each independently represents an integer of 1 to 5, and m2 is the same as m1 in the formula (A-4a) and the formula (A-4b).

[0084] The component (A) preferably has a structural unit represented by the following formula (A-6a) or the following formula (A-6b). [Chemistry 21] (In formula (A-6a) and formula (A-6b), A 4a Each independently represents a tetravalent organic group containing an aliphatic hydrocarbon group, R 1c and R 2c Each independently represents a monovalent organic group containing an ethylenically unsaturated bond. )

[0085] In formula (A-6a) and formula (A-6b), A 4a Each independently represents a tetravalent organic group. 4a The same as A in formula (A-1).

[0086] In formula (A-6a) and formula (A-6b), R 1c and R 1c Each independently represents a monovalent organic group containing an ethylenically unsaturated bond. 1c and R 1c and R in formula (A-3) 1a and R 2asame.

[0087] The polyimide precursor may be a copolymer containing a structural unit having an indane skeleton and a structural unit not containing an indane skeleton. For example, in addition to the structural unit containing an indane skeleton shown in formula (A-1), the structural unit not containing an indane skeleton shown in formula (A-1) may also be included. In addition, the polyimide precursor may be a copolymer having a plurality of different structural units shown in formula (A-1).

[0088] The polyimide precursor may contain any structural unit other than the above-mentioned amic acid structural unit and amic acid ester structural unit. Thus, the polyimide precursor may be a copolymer containing a structural unit shown in formula (A-1) and an optional structural unit. Wherein, the polyimide precursor preferably contains a large amount of amic acid structural units and amic acid ester structural units, and thus, the optional structural unit is preferably less. For example, relative to the total mass 100% of the polyimide precursor, the mass of the amic acid structural unit and the amic acid ester structural unit is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more. In the polyimide precursor, as a repeating unit, it may only contain the above-mentioned amic acid structural unit and / or amic acid ester structural unit, or it may not contain an optional structural unit. In addition, the amic acid structural unit and / or amic acid ester structural unit contained in the polyimide precursor may be one kind, or may be two or more kinds.

[0089] The structural unit represented by formula (A-1) is particularly preferably represented by any one of the following formulas (a-1) to (a-31). Therefore, the polyimide precursor preferably contains one or more structural units selected from the structural units represented by the following formulas (a-1) to (a-31), and more preferably contains any one of the structural units represented by the following formula (a-6) and the structural units represented by the following formula (a-26). [Chemistry 22] [Chemistry 23] [Chemistry 24] [Chemistry 25] [Chemistry 26] [Chemistry 27] [Chemistry 28] [Chemistry 29]

[0090] The number of repetitions of the structural unit represented by the formula (A-1) is usually 2 or more, preferably 5 to 200, more preferably 5 to 150, further preferably 5 to 100, particularly preferably 5 to 70.

[0091] Specific examples of the polyimide precursor having the structural unit represented by formula (A-1) include compounds containing the following repeating units (Aa-1) to (Aa-31). However, the polyimide precursor having the amic acid ester structural unit represented by formula (A-1) is not limited to these specific examples. In the formula, n represents an integer of 5 to 200. [Chemistry 30] [Chemistry 31] [Chemistry 32] [Chemistry 33] [Chemistry 34] [Chemistry 35] [Chemistry 36] [Chemistry 37]

[0092] The polyimide precursor can transmit ultraviolet light with high transmittance. In one example, the total transmittance of a layer of a polyimide precursor having a thickness of 60 μm at a wavelength of 365 nm is preferably 80% or more, more preferably 90% or more, and further preferably 95% or more. The total transmittance can be measured by the method described in Synthesis Example 1 of the Examples described later.

[0093] The manufacturing method of polyimide precursor is not particularly limited. Polyimide precursor can be manufactured by, for example, including reacting aliphatic acid dianhydride with diamine compound to obtain polyamic acid and reacting polyamic acid with epoxy compound containing ethylenically unsaturated bond. As aliphatic acid dianhydride, diamine compound and epoxy compound containing ethylenically unsaturated bond, for example, the above-mentioned substances can be used. About the manufacturing method of polyimide precursor, it can be referred to the method described in Japanese Patent No. 3921734, Japanese Patent Laid-Open No. 11-15152, Japanese Patent Laid-Open No. 2015-209461, Japanese Patent Laid-Open No. 2015-214680, Japanese Patent Laid-Open No. 2017-219850 or Japanese Patent Laid-Open No. 2018-146964.

[0094] As polyimide, a resin containing a structure that forms an imide structure by ring-closing the above-mentioned polyimide precursor can be used. In addition, the polyimide can contain a free radical reactive group in the molecule of the polyimide. When using a polyimide containing a free radical reactive group, the polyimide is cross-linked by exposure, which can effectively reduce the solubility of the first photosensitive resin composition and the second photosensitive resin composition relative to the developer. As a preferred polyimide, a compound containing a structure shown in the following formula (A-7) can be listed. One polyimide can be used alone, or two or more can be used in combination. [Chemistry 38]

[0095] (In formula (A-7), A ai1 The same as A in formula (A-1), B ai1 Same as B in formula (A-1), n ai1 Indicates an integer from 5 to 200. )

[0096] Specific examples of polyimide include compounds including the following repeating structures. However, polyimide is not limited to these specific examples. [Chemistry 39]

[0097] From the viewpoint of limiting resolution, the weight average molecular weight of component (A) is preferably 5000 or more, more preferably 10000 or more, and further preferably 30000 or more, and is preferably 1 million or less, more preferably 500,000 or less, and further preferably 200,000 or less. The weight average molecular weight of the resin can be measured as a polystyrene conversion value by gel permeation chromatography (GPC).

[0098] From the viewpoint of effectively forming holes in a thick photosensitive resin composition layer by exposure and development, the content of the component (A) in the first photosensitive resin composition is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more, and is preferably 98% by mass or less, more preferably 97% by mass or less, and further preferably 95% by mass or less, relative to 100% by mass of the non-volatile component of the first photosensitive resin composition.

[0099] From the viewpoint of effectively forming holes in a thick photosensitive resin composition layer by exposure and development, the content of the component (A) in the second photosensitive resin composition is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more, and is preferably 98% by mass or less, more preferably 97% by mass or less, and further preferably 95% by mass or less, relative to 100% by mass of the non-volatile component of the second photosensitive resin composition.

[0100] From the viewpoint of effectively forming holes in a thick photosensitive resin composition layer by exposure and development, the content of the component (A) in the entire photosensitive resin composition layer is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more, and is preferably 98% by mass or less, more preferably 97% by mass or less, and further preferably 95% by mass or less, relative to 100% by mass of the non-volatile components of the photosensitive resin composition layer.

[0101] It should be noted that in the present invention, the content of each component in the first photosensitive resin composition is the value when the non-volatile component in the first photosensitive resin composition is set to 100% by mass unless otherwise expressly stated, and the non-volatile component refers to the non-volatile component of the first photosensitive resin composition as a whole except the solvent. The content of each component in the second photosensitive resin composition is the value when the non-volatile component in the second photosensitive resin composition is set to 100% by mass unless otherwise expressly stated, and the non-volatile component refers to the non-volatile component of the second photosensitive resin composition as a whole except the solvent. In addition, the content of each component in the entire photosensitive resin composition layer is the value when the non-volatile component in the photosensitive resin composition layer (the first photosensitive resin composition layer and the second photosensitive resin composition layer) is set to 100% by mass unless otherwise expressly stated, and the non-volatile component refers to the non-volatile component of the photosensitive resin composition layer as a whole except the solvent.

[0102] <(B) Photoradical Generator> The first photosensitive resin composition and the second photosensitive resin composition contain a (B) light free radical generator as a (B) component. Substances that correspond to the (A) component are excluded from the (B) component. The (B) component generates free radicals when irradiated with active light, and a crosslinking reaction can be performed using the free radicals. The (B) component can be used alone or in combination of two or more.

[0103] The (B) component can generally be classified into (B-1) a highly reactive photoradical generator and (B-2) a photoradical generator with excellent deep curing property. When a semiconductor package substrate is produced by laminating a photosensitive film on a laminated object member, the second photosensitive resin composition layer of the photosensitive resin composition layer is usually laminated in such a way that it is bonded to a circuit substrate, so that the second photosensitive resin composition layer is located at the bottom layer of the photosensitive resin composition layer when laminated. Regarding the total thickness of the photosensitive resin composition layer, the thickness is usually thick, so it is difficult for light to reach the second photosensitive resin composition layer as the bottom layer. Therefore, there is a tendency for the shape of the through hole generated by exposure to be inverted cone-shaped. The (B) component contained in the first photosensitive resin composition and the second photosensitive resin composition may contain only the (B-1) component or only the (B-2) component. From the viewpoint of improving undercut resistance and improving limiting resolution, it is preferred to contain the (B-1) component and the (B-2) component.

[0104] (B-1) As the highly reactive photoradical generator, a photoradical generator containing an oxime ester structure can be mentioned. As the (B-1) component, for example, an oxime ester-based photoradical generator can be mentioned.

[0105] Examples of oxime ester photoradical generators include 2-(benzoyloxyimino)-1-[4-(phenylthio)phenyl]octan-1-one (OXE01), [1-[9-ethyl-6-(2-methylbenzoyl)carbazole-3-yl]ethylideneamino]acetate (OXE02), ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyl oxime), and the like.

[0106] (B-1) A commercially available photoradical generator with high reactivity may be used. Specific examples of commercially available photoradical generators with high reactivity include "Irgacure TPO", "Irgacure OXE-01", and "Irgacure OXE-02" manufactured by BASF, and "N-1919" manufactured by ADEKA.

[0107] In the present invention, as (B-2) a photoradical generator having excellent deep curing property, it has an absorption maximum in the wavelength region of 340 nm to 420 nm or an absorption coefficient of 4000 ml / gcm or less at 365 nm. Examples of the component (B-2) include acylphosphine-based photoradical generators, aminoketone-based photoradical generators, α-hydroxyketone-based photoradical generators, benzoin-based photoradical generators, and benzylketal-based photoradical generators.

[0108] Examples of the acylphosphine-based photoradical generator include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, and polyoxyethylene glycerol ether tris[phenyl(2,4,6-trimethylbenzoyl)phosphinate] (Polymeric TPO-L).

[0109] Examples of the aminoketone photoradical generator include α-aminoketone photoradical generators such as 2-methyl-1-phenyl-2-morpholinopropane-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-methyl-1-(4-hexylphenyl)-2-morpholinopropane-1-one, 2-ethyl-2-(dimethylamino)-1-(4-morpholinophenyl)butane-1-one, 2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)butane-1-one, 2-(dimethylamino)-2-(4-methylphenylmethyl)-1-(4-morpholinophenyl)butane-1-one, and 2-methyl-1-(9,9-dibutylfluoren-2-yl)-2-morpholinopropane-1-one.

[0110] Examples of the α-hydroxyketone-based photoradical generator include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methylpropanone, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropanoyl)benzyl]phenyl}-2-methylpropane-1-one.

[0111] Examples of the benzoin-based photoradical generator include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.

[0112] Examples of the benzyl ketal-based photoradical generator include 2,2-dimethoxy-2-phenylacetophenone.

[0113] (B-2) A commercially available photoradical generator having excellent deep curing property can be used. Specific examples of commercially available photoradical generators having excellent deep curing property include "Omnirad907", "Omnirad369", "Omnirad379", "Omnirad379EG", "Omnirad819", "OmniradTPO" and the like manufactured by IGM.

[0114] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B) in the first photosensitive resin composition is preferably 0.03 parts by mass or more, more preferably 0.1 parts by mass or more, and further preferably 0.5 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and further preferably 3 parts by mass or less, relative to 100 parts by mass of the component (A) in the first photosensitive resin composition.

[0115] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B-1) in the first photosensitive resin composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, and is preferably 2 parts by mass or less, more preferably 1.5 parts by mass or less, and even more preferably 1 part by mass or less, relative to 100 parts by mass of the component (A) in the first photosensitive resin composition.

[0116] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B-2) in the first photosensitive resin composition is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, and is preferably 1 part by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the component (A) in the first photosensitive resin composition.

[0117] The content of the component (B) in the first photosensitive resin composition is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, and is preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less, when the non-volatile component of the first photosensitive resin composition is 100% by mass, from the viewpoint of improving undercut resistance and limiting resolution.

[0118] From the viewpoint of improving undercut resistance and limiting resolution, when the non-volatile component of the first photosensitive resin composition is set to 100 mass %, the content of the component (B-1) in the first photosensitive resin composition is preferably 0.1 mass % or more, more preferably 0.3 mass % or more, further preferably 0.5 mass % or more, and is preferably 5 mass % or less, more preferably 4 mass % or less, further preferably 3 mass % or less.

[0119] From the viewpoint of improving undercut resistance and limiting resolution, when the non-volatile component of the first photosensitive resin composition is set to 100 mass %, the content of the component (B-2) in the first photosensitive resin composition is preferably 0.1 mass % or more, more preferably 0.3 mass % or more, further preferably 0.5 mass % or more, and is preferably 5 mass % or less, more preferably 4 mass % or less, further preferably 3 mass % or less.

[0120] The nonvolatile component of the first photosensitive resin composition is 100 mass %, and the content of the component (B-1) in the first photosensitive resin composition is b 1-1 , the content of the component (B-2) in the first photosensitive resin composition is set to b 2-1 When b 1-1 / b 2-1 It is preferably 0.5 or more, more preferably 1 or more, further preferably 1.5 or more, 2 or more, and is preferably 15 or less, more preferably 12 or less, and further preferably 10 or less. By adjusting the amounts of the components (B-1) and (B-2) contained in the first photosensitive resin composition so that the amount ratio thereof is within the above range, a cured product having excellent undercut resistance can be obtained.

[0121] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B) in the second photosensitive resin composition is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and further preferably 0.5 parts by mass or more, and is preferably 8 parts by mass or less, more preferably 5 parts by mass or less, and further preferably 4 parts by mass or less, relative to 100 parts by mass of the component (A) in the second photosensitive resin composition.

[0122] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B-1) in the second photosensitive resin composition is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the component (A) in the second photosensitive resin composition.

[0123] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B-2) in the second photosensitive resin composition is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, and is preferably 1 part by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the component (A) in the second photosensitive resin composition.

[0124] The content of the component (B) in the second photosensitive resin composition is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more, and is preferably 5% by mass or less, more preferably 4% by mass or less, and further preferably 3% by mass or less, when the non-volatile component of the second photosensitive resin composition is 100% by mass, from the viewpoint of improving undercut resistance and limiting resolution.

[0125] The nonvolatile component of the first photosensitive resin composition is 100 mass %, and the content of the component (B) in the first photosensitive resin composition is b 1-0 , the content of the component (B) in the second photosensitive resin composition is set to b 2-0 When b 1-0 / b 2-0 It is preferably 0.1 or more, more preferably 0.3 or more, further preferably 0.5 or more, 0.6 or more, and preferably 3 or less, more preferably 2 or less, further preferably 1.5 or less, 1 or less, 0.9 or less. By adjusting the amount of the component (B) so that the amount ratio of the component (B) contained in the first photosensitive resin composition and the second photosensitive resin composition is within the above range, a cured product having excellent undercut resistance can be obtained.

[0126] From the viewpoint of improving undercut resistance and limiting resolution, when the non-volatile component of the second photosensitive resin composition is set to 100 mass %, the content of the component (B-1) in the second photosensitive resin composition is preferably 0.05 mass % or more, more preferably 0.1 mass % or more, further preferably 0.5 mass % or more, and is preferably 5 mass % or less, more preferably 4 mass % or less, further preferably 3 mass % or less.

[0127] From the viewpoint of improving undercut resistance and limiting resolution, when the non-volatile component of the second photosensitive resin composition is set to 100 mass %, the content of the component (B-2) in the second photosensitive resin composition is preferably 0.05 mass % or more, more preferably 0.03 mass % or more, further preferably 0.1 mass % or more, and is preferably 1.5 mass % or less, more preferably 1 mass % or less, further preferably 0.5 mass % or less.

[0128] The nonvolatile component of the second photosensitive resin composition is 100 mass %, and the content of the component (B-1) in the second photosensitive resin composition is b 2-1 , the content of the component (B-2) in the second photosensitive resin composition is set to b 2-2 When b 2-1 / b 2-2It is preferably 1 or more, more preferably 2 or more, further preferably 2.5 or more, 3 or more, and is preferably 20 or less, more preferably 15 or less, further preferably 13 or less, 10 or less. By adjusting the amounts of the components (B-1) and (B-2) contained in the second photosensitive resin composition so that the amount ratio thereof is within the above range, a cured product having excellent undercut resistance can be obtained.

[0129] The nonvolatile component of the first photosensitive resin composition is 100 mass %, and the content of the component (B-1) in the first photosensitive resin composition is b 1-1 , the content of the component (B-1) in the second photosensitive resin composition is set to b 2-1 When b 1-1 / b 2-1 It is preferably 0.1 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and is preferably 3 or less, more preferably 1.5 or less, and even more preferably 1 or less. By adjusting the amount ratio of the component (B-1) contained in the first photosensitive resin composition and the second photosensitive resin composition so as to be within the above range, the difference in absorbance between the first photosensitive resin composition layer and the second photosensitive resin composition layer can be easily adjusted to be within a predetermined range, and a cured product having excellent undercut resistance can be obtained.

[0130] The nonvolatile component of the first photosensitive resin composition is 100 mass %, and the content of the component (B-2) in the first photosensitive resin composition is b 1-2 , the content of the component (B-2) in the second photosensitive resin composition is set to b 2-2 When b 1-2 / b 2-2 It is preferably 0.1 or more, more preferably 0.5 or more, and even more preferably 0.8 or more, and is preferably 3 or less, more preferably 1.5 or less, and even more preferably 1.3 or less. By adjusting the amount ratio of the component (B-2) contained in the first photosensitive resin composition and the second photosensitive resin composition so as to be within the above range, the difference in absorbance between the first photosensitive resin composition layer and the second photosensitive resin composition layer can be easily adjusted to within a specified range, and a cured product with excellent undercut resistance can be obtained.

[0131] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B) in the photosensitive resin composition layer is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, and is preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less, when the non-volatile component of the photosensitive resin composition layer is set to 100% by mass.

[0132] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B) in the photosensitive resin composition layer is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and further preferably 0.5 parts by mass or more, and is preferably 8 parts by mass or less, more preferably 5 parts by mass or less, and further preferably 3 parts by mass or less, relative to 100 parts by mass of the component (A) in the photosensitive resin composition layer.

[0133] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B-1) in the photosensitive resin composition layer is preferably 0.03 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.5 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the component (A) in the photosensitive resin composition layer.

[0134] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (B-2) in the photosensitive resin composition layer is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, and is preferably 3 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the component (A) in the photosensitive resin composition layer.

[0135] From the viewpoint of improving undercut resistance, the content of the component (B) contained in the first photosensitive resin composition is preferably less than the content of the component (B) contained in the second photosensitive resin composition. Specifically, when the content of the component (B) contained in the first photosensitive resin composition relative to 100 parts by mass of the component (A) is b1 and the content of the component (B) contained in the second photosensitive resin composition relative to 100 parts by mass of the component (A) is b2, b2-b1 is preferably 0.1 or more, more preferably 0.15 or more, and further preferably 0.2 or more, and is preferably 2 or less, more preferably 1.5 or less, and further preferably 1 or less.

[0136] -(C) Photocrosslinking agent- The first photosensitive resin composition and the second photosensitive resin composition contain a (C) photocrosslinking agent as a (C) component. The (B) crosslinking agent does not include a substance that meets the requirements of the (A) component and the (B) component. If the first photosensitive resin composition and the second photosensitive resin composition are irradiated with active light and free radicals are generated from the (B) photoradical generator, a crosslinking reaction of the (C) photocrosslinking agent occurs, which can effectively reduce the solubility in the developer. Therefore, the difference in solubility between the exposed part and the non-exposed part of the first photosensitive resin composition and the second photosensitive resin composition relative to the developer can be effectively increased. Therefore, during development, the first photosensitive resin composition and the second photosensitive resin composition can be selectively removed except for the part where the crosslinking reaction has been carried out, and a negative pattern can be advantageously formed. In addition, as a result, the film thickness and resolution after development can be ensured. The (C) photocrosslinking agent can be used alone or in combination of two or more.

[0137] As the (C) photocrosslinking agent, a compound capable of undergoing a crosslinking reaction when exposed to light can be used. The (C) photocrosslinking agent contains an ethylenically unsaturated bond, and therefore, the ethylenically unsaturated bond is generally capable of undergoing a crosslinking reaction. As the (C) photocrosslinking agent, a compound containing an ethylenically unsaturated bond and at least one α-carbon atom of the ethylenically unsaturated bond is more preferably bonded to a carbonyl group or an aromatic group. The α-carbon atom of the ethylenically unsaturated bond represents the first carbon atom adjacent to the carbon atom bonded by a carbon-carbon unsaturated bond.

[0138] (C) The photocrosslinking agent usually contains a group containing an ethylenically unsaturated bond. Hereinafter, the "group containing an ethylenically unsaturated bond" is sometimes referred to as an "ethylenically unsaturated group". The ethylenically unsaturated group is usually a monovalent group, and examples thereof include vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimide, nadicimide, and (meth)acryloyl. From the viewpoint of the reactivity of photoradical polymerization, (meth)acryloyl and phenylethynyl are preferred, and (meth)acryloyl is particularly preferred. (B) The crosslinking agent contains an ethylenically unsaturated bond and is therefore capable of photoradical polymerization. When photoradical polymerization is carried out under normal conditions, it is preferably a compound having a carbonyl group or an aromatic group at at least one α position of the ethylenically unsaturated bond.

[0139] The number of ethylenically unsaturated bonds in each molecule of the (C) photocrosslinking agent is usually 1 or more. From the viewpoint of limiting resolution, the number of ethylenically unsaturated bonds in each molecule of the (C) photocrosslinking agent is preferably 2 or more, more preferably 3 or more. The upper limit is not particularly limited and can be set to 20 or less. When each molecule of the (C) photocrosslinking agent contains 2 or more ethylenically unsaturated groups, these ethylenically unsaturated groups may be the same or different.

[0140] (C) The photocrosslinking agent is preferably a compound represented by the following formula (C-1). [Chemistry 40] In the formula, R 1c Each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, each Z independently represents a linear or branched alkylene group having 1 to 20 carbon atoms which may contain an oxygen atom, an arylene group which may contain an oxygen atom, or a linear or branched alkenylene group which may contain an oxygen atom and has 2 to 20 carbon atoms, A 1c It represents a linear, cyclic or branched organic group having a valence of nc and having a carbon number of 1 to 10. nc represents a positive integer of 2 to 20.

[0141] R 1c Each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms. Examples of the linear or branched alkyl group having 1 to 4 carbon atoms include methyl, ethyl, propyl, isopropyl, 1-butyl, sec-butyl, tert-butyl, and the like. 1c , preferably a hydrogen atom or a methyl group.

[0142] Z each independently represents a linear or branched alkylene group having 1 to 20 carbon atoms, optionally containing an oxygen atom, an arylene group optionally containing an oxygen atom, or a linear or branched alkenylene group having 2 to 20 carbon atoms, optionally containing an oxygen atom. As a linear or branched alkylene group having 1 to 20 carbon atoms, a linear or branched alkylene group having 1 to 10 carbon atoms is preferred, and a linear or branched alkylene group having 1 to 6 carbon atoms is more preferred. As such an alkylene group, for example, methylene, ethylene, propylene, butylene, pentylene, hexylene, etc. can be listed, preferably methylene. In addition, the alkylene group can be an oxyalkylene group containing an oxygen atom, and as a specific example of such a group, for example, the groups shown below can be listed. In the formula, "*" represents a bond, c1 represents an integer of 1 to 20, c2 represents an integer of 1 to 10, c3 represents an integer of 1 to 19, and c4 represents an integer of 1 to 9. [Chemistry 41]

[0143] As the arylene group optionally containing an oxygen atom, an arylene group having 6 to 20 carbon atoms is preferred, an arylene group having 6 to 15 carbon atoms is more preferred, and an arylene group having 6 to 10 carbon atoms is further preferred. Examples of such arylene groups include phenylene and naphthylene. In addition, the arylene group may contain an oxygen atom, and specific examples of such groups include the following groups. In the formula, "*" represents a bond, and c5 represents an integer of 1 to 3. [Chemistry 42]

[0144] As a straight-chain or branched alkenylene group having 2 to 20 carbon atoms and optionally containing an oxygen atom, a straight-chain or branched alkenylene group having 2 to 10 carbon atoms is preferred, and a straight-chain or branched alkenylene group having 2 to 6 carbon atoms is more preferred. As such an alkenylene group, for example, vinylene, propenylene, butenylene, pentenylene, hexenylene, etc. can be listed. In addition, the alkenylene group can be an oxyalkenylene group containing an oxygen atom, and as a specific example of such a group, for example, the groups shown below can be listed. In the formula, "*" represents a bond, and c6 represents an integer of 1 to 10. As an alkenylene group, a propenylene group is preferred. [Chemistry 43]

[0145] Among them, Z is preferably a linear or branched alkylene group having 1 to 20 carbon atoms which may contain an oxygen atom, and more preferably an oxyalkylene group and a methylene group.

[0146] A 1c It represents a linear, cyclic or branched nc-valent organic group having 1 to 10 carbon atoms. Examples of the nc-valent organic group include, for example, an nc-valent hydrocarbon group optionally containing an oxygen atom, an nc-valent group derived from bisphenol, an nc-valent group derived from fluorene, an nc-valent group derived from tricyclodecane, or an nc-valent group derived from an isocyanuric acid group. Examples of the nc-valent hydrocarbon group optionally containing an oxygen atom include an nc-valent aliphatic hydrocarbon group optionally containing an oxygen atom, and an nc-valent aromatic hydrocarbon group optionally containing an oxygen atom. An nc-valent aliphatic hydrocarbon group optionally containing an oxygen atom is preferred. For example, when nc is 2, an alkylene group is preferred. As A 1c Specific examples of the group shown include the following groups. In the formula, "*" represents a bond. [Chemistry 44]

[0147] nc represents a positive integer of 2 to 20, preferably a positive integer of 2 to 8, more preferably a positive integer of 2 to 6, further preferably a positive integer of 2 to 5, further preferably 3 or 4, or 2 or 3.

[0148] (C) The photocrosslinking agent may be a compound represented by the following formula (C-2). [Chemistry 45] In formula (C-2), R 2c Each independently represents a hydrogen atom or a methyl group.

[0149] R 2cEach independently represents a hydrogen atom or a methyl group, and is preferably a methyl group.

[0150] Specific examples of the photocrosslinking agent (C) include dipentaerythritol hexaacrylate, dipentaerythritol tetraacrylate, and the following compounds (CL-1) to (CL-11). However, the component (C) is not limited to these. [Chemistry 46] [Chemistry 47]

[0151] (C) A commercially available photocrosslinking agent may be used. Examples of commercially available products include NKester-D-TMP, 4G, 9G, 14G, 23G, DCP, TMPT, and A-TMPT manufactured by Shin-Nakamura Chemical Co., Ltd.; SR209 manufactured by Tomoe Industries; M-940 and M-933 manufactured by Toagosei Co., Ltd.; DPHA (dipentaerythritol hexaacrylate) manufactured by Nippon Kayaku Co., Ltd.; and CN2301 and CN2304 manufactured by Subaru Corporation.

[0152] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (C) in the first photosensitive resin composition is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and further preferably 5 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and further preferably 8 parts by mass or less, relative to 100 parts by mass of the component (A) in the first photosensitive resin composition.

[0153] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (C) in the first photosensitive resin composition is preferably 1% by mass or more, more preferably 2% by mass or more, and further preferably 3% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, and further preferably 8% by mass or less, relative to 100% by mass of the non-volatile components of the first photosensitive resin composition.

[0154] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (C) in the second photosensitive resin composition is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and further preferably 5 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and further preferably 8 parts by mass or less, relative to 100 parts by mass of the component (A) in the second photosensitive resin composition.

[0155] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (C) in the second photosensitive resin composition is preferably 1% by mass or more, more preferably 2% by mass or more, and further preferably 3% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, and further preferably 8% by mass or less, relative to 100% by mass of the non-volatile component of the second photosensitive resin composition.

[0156] From the viewpoint of improving undercut resistance and limiting resolution, when the non-volatile component of the photosensitive resin composition layer is set to 100 mass %, the content of the component (C) in the photosensitive resin composition layer is preferably 1 mass % or more, more preferably 2 mass % or more, further preferably 3 mass % or more, and is preferably 15 mass % or less, more preferably 10 mass % or less, further preferably 8 mass % or less.

[0157] From the viewpoint of improving undercut resistance and limiting resolution, the content of the component (C) in the photosensitive resin composition layer is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and further preferably 5 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and further preferably 8 parts by mass or less, relative to 100 parts by mass of the component (A) in the photosensitive resin composition layer.

[0158] -(D) Optional Additives- The first photosensitive resin composition and the second photosensitive resin composition may contain (D) optional additives as optional components in addition to the above-mentioned (A) to (C) components. The (D) optional additives as the (D) component may be used alone or in combination of two or more.

[0159] As (D) optional additives, for example, sensitizers; photopolymerization initiation aids; adhesion aids; surfactants such as fluorine-based surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, and silicone-based surfactants; thermoplastic resins; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black; polymerization inhibitors such as hydroquinone, phenothiazine, methyl hydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol; thickeners such as BENTON and montmorillonite; silicone-based, fluorine-based, and vinyl resin-based defoamers; flame retardants such as epoxy resins, antimony compounds, phosphorus compounds, aromatic condensed phosphates, and halogen-containing condensed phosphates; thermosetting resins such as phenolic resins and cyanate ester resins, etc.

[0160] -(E)Solvent- The first photosensitive resin composition and the second photosensitive resin composition may contain a solvent (E) as an optional component in combination with non-volatile components such as the above-mentioned components (A) to (D). The solvent (E) is a volatile component, and it is preferred to use a substance that can uniformly dissolve at least any of the components (A) to (D).

[0161] Examples of the (E) solvent include ether compound solvents having 2 to 9 carbon atoms, such as dimethyl ether, diethyl ether, methyl ethyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and triethylene glycol dimethyl ether; ketone compound solvents having 2 to 6 carbon atoms, such as acetone and methyl ethyl ketone; saturated hydrocarbon compound solvents having 5 to 10 carbon atoms, such as n-pentane, cyclopentane, n-hexane, cyclohexane, methylcyclohexane, and decahydronaphthalene; benzene, toluene, xylene, mesitylene, and tetrahydronaphthalene; Aromatic hydrocarbon compound solvents having 6 to 10 carbon atoms; ester compound solvents having 3 to 9 carbon atoms, such as methyl acetate, ethyl acetate, γ-butyrolactone and methyl benzoate; halogen-containing compound solvents having 1 to 10 carbon atoms, such as chloroform, dichloromethane and 1,2-dichloroethane; nitrogen-containing compound solvents having 2 to 10 carbon atoms, such as acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and sulfur-containing compound solvents, such as dimethyl sulfoxide.

[0162] In addition, examples of the (E) solvent include N-ethyl-2-pyrrolidone, tetrahydrofuran, N,N-dimethylacetamide, dimethyl sulfoxide, hexamethylphosphoramide, pyridine, cyclopentanone, α-acetyl-γ-butyrolactone, tetramethyl urea, 1,3-dimethyl-2-imidazolidinone, N-cyclohexyl-2-pyrrolidone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, anisole, ethyl acetate, ethyl lactate, and butyl lactate.

[0163] (E) The solvent may be used alone or in combination of two or more.

[0164] When the entire first photosensitive resin composition including the (E) solvent is set to 100 mass %, the amount of the (E) solvent in the first photosensitive resin composition is preferably 1 mass % or more, more preferably 2 mass % or more, and further preferably 3 mass % or more, and is preferably 40 mass % or less, more preferably 35 mass % or less, and further preferably 30 mass % or less.

[0165] When the entire second photosensitive resin composition including the (E) solvent is set to 100 mass %, the amount of the (E) solvent in the second photosensitive resin composition is preferably 1 mass % or more, more preferably 2 mass % or more, and further preferably 3 mass % or more, and is preferably 40 mass % or less, more preferably 35 mass % or less, and further preferably 30 mass % or less.

[0166] <Other layers> The photosensitive film may include other layers as needed. As the other layers, there can be cited: a photosensitive resin composition layer that is arranged between the first photosensitive resin composition layer and the second photosensitive resin composition layer and is different from the first photosensitive resin composition layer and the second photosensitive resin composition layer. The photosensitive resin composition layer can be formed into multiple layers. The photosensitive resin composition layer that is different from the first photosensitive resin composition layer and the second photosensitive resin composition layer only needs to contain any one of the components (A) to (E). Even if the photosensitive film has a photosensitive resin composition layer that is different from the aforementioned first photosensitive resin composition layer and the second photosensitive resin composition layer, as long as the difference in absorbance between the first photosensitive resin composition layer adjacent to the support and the second photosensitive resin composition layer as the outermost layer of the photosensitive resin composition layer is 0.05 or more and 0.5 or less. In addition, the total thickness of these photosensitive resin composition layers is preferably within the thickness range of the photosensitive resin composition layer.

[0167] In addition, the photosensitive film may have, as another layer, a protective film, for example, provided on the surface of the second photosensitive resin composition layer that is not bonded to the first photosensitive resin composition layer (i.e., the surface opposite to the first photosensitive resin composition layer). By laminating the protective film, adhesion of dirt and the like on the surface of the second photosensitive resin composition layer and damage can be suppressed.

[0168] As the protective film, for example, a film formed of the same material as the support can be used. The thickness of the protective film is not particularly limited, but is preferably in the range of 1 μm to 40 μm, more preferably in the range of 5 μm to 30 μm, and further preferably in the range of 10 μm to 30 μm.

[0169] <Method for producing photosensitive film> As described above, the photosensitive film of the present invention includes a support, a first photosensitive resin composition layer, and a second photosensitive resin composition layer in this order, and optionally includes a protective film and the like. The method for manufacturing the photosensitive film comprises: (1) a step of applying a first resin varnish in which a first photosensitive resin composition is dissolved on a support and drying the varnish to form a first resin sheet having a first photosensitive resin composition layer on the support; (2) a step of applying a second resin varnish in which a second photosensitive resin composition is dissolved on the protective film and drying the varnish to form a second resin sheet having a second photosensitive resin composition layer on the protective film; and (3) A step of laminating the first resin sheet and the second resin sheet so that the first photosensitive resin composition layer and the second photosensitive resin composition layer are bonded to each other.

[0170] -Process (1)- In step (1), a first resin varnish is prepared by dissolving a first photosensitive resin composition in a solvent, and the first resin varnish is applied onto a support and then dried to form a first photosensitive resin composition layer. The solvent is as described above.

[0171] Examples of the coating method of the first resin varnish include gravure coating, micro gravure coating, reverse coating, kiss reverse coating, die coating, slot die, lip coating, comma coating, blade coating, roll coating, knife coating, curtain coating, chamber gravure coating, slot coating, spin coating, slit coating, spray coating, dip coating, hot melt coating, rod coating, applicator coating, air knife coating, curtain coating, offset printing, brush coating, and full-surface printing by screen printing. Among them, the coating method of the resin varnish is preferably spin coating.

[0172] The first resin varnish may be applied in multiple times or once, or may be applied in a combination of different methods. Among them, die coating is preferred due to its excellent uniform coating properties. In addition, in order to avoid the mixing of foreign matter, the coating process is preferably carried out in an environment where less foreign matter is generated, such as a clean room.

[0173] Drying can be carried out by known methods such as heating and blowing hot air. The drying conditions are not particularly limited, and the first photosensitive resin composition layer is dried in such a manner that the solvent content is 10% by mass or less, preferably 5% by mass or less. It also varies depending on the boiling point of the solvent in the first resin varnish. For example, when a first resin varnish containing 30% to 60% by mass of a solvent is used, the first photosensitive resin composition layer can be formed by drying it at 50°C to 150°C for 3 minutes to 10 minutes.

[0174] -Process (2)- In step (2), a second resin varnish is prepared by dissolving a second photosensitive resin composition in a solvent, and the second resin varnish is applied to the protective film and then dried to form a second photosensitive resin composition layer. The solvent is as described above. Step (2) can be carried out in the same manner as step (1).

[0175] -Process (3)- In step (3), the first resin sheet and the second resin sheet are laminated in such a manner that the first photosensitive resin composition layer and the second photosensitive resin composition layer are bonded. Thus, a photosensitive film is formed in the order of a support, a first photosensitive resin composition layer, a second photosensitive resin composition layer, and a protective film. When the photosensitive film is laminated on a laminated object member, the protective film can be peeled off before use.

[0176] Lamination can be performed by vacuum lamination. In vacuum lamination, the lamination temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the lamination pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the lamination time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. Lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.

[0177] Lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho, a vacuum applicator manufactured by Nike Materials, and an intermittent vacuum pressure laminator.

[0178] As a method for producing a photosensitive film, in addition to the above-mentioned production method, for example, a second varnish is applied on the first photosensitive resin composition layer formed on a support and dried to form a second photosensitive resin composition layer on the first photosensitive resin composition layer. The coating and drying are as described above.

[0179] <Photosensitive Film Characteristics, etc.> The photosensitive resin composition layer of the photosensitive film of the present invention exhibits excellent undercut resistance even when the film thickness is relatively thick. A photosensitive resin composition layer is produced on a silicon wafer. A mask having circular holes (through holes) with opening diameters of 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, and 70 μm in the exposure pattern is used for the photosensitive resin composition layer, and the exposure amount is set to 200 mJ / cm 2 、300mJ / cm 2 、400mJ / cm 2 and 500mJ / cm 2 , developing is performed to form each circular hole. In addition, the undercut of the limit opening through hole is determined (the difference between the radius of the bottom and the radius of the top (radius of the bottom - radius of the top)). At this time, the undercut is preferably less than 4 μm, more preferably less than 2 μm, and it is particularly preferred to be able to eliminate the undercut. The evaluation of undercut resistance can be measured according to the method described in the examples described below.

[0180] The photosensitive resin composition layer of the photosensitive film of the present invention generally shows excellent limiting resolution even when the film thickness is relatively thick. Therefore, by using the photosensitive film of the present invention, it is possible to form holes with small diameters by exposure and development. The degree of limiting resolution can be evaluated based on the aspect ratio of the opening diameter of the limiting opening through-hole and the film thickness of the photosensitive resin composition layer. For example, a photosensitive resin composition layer is prepared on a silicon wafer. A mask with circular holes (through-holes) with opening diameters of 20 μm, 30 μm, 40 μm, 50 μm, 60 μm and 70 μm in the exposure pattern is used for the photosensitive resin composition layer, and the exposure amount is set to 200 mJ / cm 2 、300mJ / cm 2 、400mJ / cm 2 and 500mJ / cm 2 , developing is performed to form each circular hole. In addition, the diameter of the bottom of the circular hole is observed to determine the circular hole (limit opening through hole) with the minimum opening diameter that can be opened without residue and peeling. The aspect ratio of the diameter of the limit opening through hole (film thickness (μm) / through hole diameter (μm)) is preferably greater than 0.5, more preferably greater than 0.7, more preferably greater than 0.8, further preferably greater than 0.9, and particularly preferably greater than 1.0. The upper limit is not particularly limited, but is preferably less than 1.5. The evaluation of the limiting resolution can be determined according to the method described in the embodiments described later.

[0181] The cured product of the photosensitive resin composition layer of the photosensitive film of the present invention generally exhibits excellent adhesion to metals such as copper foil. For example, a photosensitive resin composition layer is prepared on a silicon wafer laminated with copper foil. The photosensitive resin composition layer is exposed to light at 200 mJ / cm using a mask having a circular hole with an opening diameter of 70 μm and an exposure pattern. 2 The exposure amount is 0.01, and the development is performed to form a circular hole, and the cross-section of the circular hole is observed. The presence or absence of peeling between the copper foil and the end of the bottom of the circular hole (the bottom of the through hole) and the peeling length are measured. At this time, the peeling length is preferably 4 μm or less, more preferably 2 μm or less, further preferably less than 2 μm, and particularly preferably can eliminate peeling. Adhesion can be measured by the method described in the examples described later.

[0182] The use of the photosensitive film of the present invention is not particularly limited. For example, the photosensitive film has a photosensitive resin composition layer, and therefore, is useful as a PID (Photo Imaginable Dielectric). In addition, the photosensitive film can be used for a wide range of uses using a photosensitive resin composition layer, such as an insulating resin sheet (prepreg, etc.), a silicon wafer, a circuit substrate (laminated board use, multilayer printed circuit board use, etc.), a solder resist, a buffer coating, an underfill material, a chip bonding material, a semiconductor sealing material, a hole filling resin, a component embedding resin, etc.

[0183] As a preferred example, the photosensitive film can be used for forming an insulating layer. As a specific example, the photosensitive film can be used for forming an insulating layer of a printed wiring board (a printed wiring board having a cured product of a photosensitive resin composition layer as an insulating layer).

[0184] For example, the photosensitive film can be used for forming an interlayer insulating layer. Specifically, the photosensitive film can be used for forming the interlayer insulating layer of a printed wiring board having a cured product of a photosensitive resin composition layer as the interlayer insulating layer.

[0185] For example, the photosensitive film can be used for forming a plating layer. Specifically, the photosensitive film can be used for forming the insulating layer of a printed wiring board having an insulating layer composed of a cured product of a photosensitive resin composition layer and a plating layer formed on the insulating layer.

[0186] For example, the photosensitive film can be used for forming a solder resist layer. Specifically, the photosensitive film can be used for forming the solder resist layer of a printed wiring board having a cured product of a photosensitive resin composition layer as the solder resist layer.

[0187] For example, the photosensitive film can be used to form a redistribution formation layer of a wafer-level package. Specifically, the photosensitive film can be used to form the redistribution formation layer of a wafer-level package having a cured product of a photosensitive resin composition layer as the redistribution formation layer.

[0188] For example, the photosensitive film can be used to form a redistribution formation layer of a fan-out wafer level package. Specifically, the photosensitive film can be used to form the redistribution formation layer of a fan-out wafer level package having a cured product of a photosensitive resin composition layer as the redistribution formation layer.

[0189] For example, the photosensitive film can be used to form a redistribution formation layer of a fan-out panel level package. Specifically, the photosensitive film can be used to form the redistribution formation layer of a fan-out panel level package having a cured product of a photosensitive resin composition layer as the redistribution formation layer.

[0190] For example, the photosensitive film can be used for buffer coating applications. Specifically, the photosensitive film can be used for forming the buffer coating of a semiconductor device having a cured product of a photosensitive resin composition layer as the buffer coating.

[0191] For example, the photosensitive film can be used to form an insulating layer of a display. Specifically, the photosensitive film can be used to form the insulating layer of a display including a cured product of a photosensitive resin composition layer as the insulating layer.

[0192] [Laminated body] The laminate of the present invention comprises a first photosensitive resin composition layer comprising a first photosensitive resin composition, and a second photosensitive resin composition layer comprising a second photosensitive resin composition provided on the first photosensitive resin composition layer. The first photosensitive resin composition and the second photosensitive resin composition in the laminate, and the first photosensitive resin composition layer and the second photosensitive resin composition layer are as described above.

[0193] The laminate is obtained by peeling off the support and the protective film after completing steps (1) to (3) in the above-mentioned method for producing a photosensitive film. The support and the like can be peeled off by a known method.

[0194] [Semiconductor package substrate] The semiconductor package substrate has an insulating layer formed by a cured product of the above-mentioned photosensitive resin composition layer (a cured product of the first photosensitive resin composition and the second photosensitive resin composition). Thus, the insulating layer includes a cured product of the photosensitive resin composition layer, preferably only includes a cured product of the photosensitive resin composition layer. When the above-mentioned photosensitive film is used, the insulating layer can be formed thicker. The specific thickness range of the insulating layer can be the same as the thickness range of the photosensitive resin composition layer. The insulating layer is preferably used as a redistribution forming layer, an interlayer insulating layer, a buffer coating or a solder resist layer.

[0195] In the first example, the semiconductor package substrate can be manufactured using the above-mentioned photosensitive film, and the cured product of the photosensitive resin composition layer can be used as an insulating layer. Specifically, the method for manufacturing the semiconductor package substrate described in the first example includes: (I) a step of laminating a photosensitive resin composition layer of a photosensitive film on a circuit board; (II) a step of irradiating the photosensitive resin composition layer with active light; and (III) A step of developing the photosensitive resin composition layer.

[0196] <Step (I)> In the step (I), the circuit board and the second photosensitive resin composition layer in the photosensitive resin composition layer are laminated so as to be bonded to each other.

[0197] As the circuit substrate, there can be cited substrates having supporting substrates such as glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. Here, the circuit substrate refers to a substrate having a patterned conductor layer (circuit) formed on one or both sides of the supporting substrate as described above. In addition, in a multilayer printed circuit board formed by alternately stacking a conductor layer and an insulating layer, a substrate having a patterned conductor layer (circuit) on one or both sides of the outermost layer of the multilayer printed circuit board is also included in the circuit substrate mentioned here. The surface of the conductor layer can be roughened in advance by blackening, copper etching, etc.

[0198] The lamination of the photosensitive film and the circuit substrate is carried out in a manner that the second photosensitive resin composition layer is bonded to the circuit substrate. In the case where the photosensitive film has a protective film, the lamination is carried out after removing the protective film. In addition, the photosensitive film can be laminated on a single side of the circuit substrate, or it can be laminated on both sides. For example, as required, the photosensitive film and the circuit substrate are preheated, and the photosensitive film is pressed and heated while being bonded to the circuit substrate, so that lamination can be carried out. For the photosensitive film, a method of laminating it on the circuit substrate under reduced pressure by vacuum lamination is suitable.

[0199] The lamination conditions are not particularly limited. For example, it is preferred that the pressure bonding temperature (lamination temperature) is preferably 50° C. to 120° C., and the pressure bonding pressure is preferably 1 kgf / cm 2 ~11kgf / cm 2 (9.8×10 4 N / m 2 ~107.9×10 4 N / m 2 ), the pressing time is preferably set to 5 seconds to 300 seconds, and the lamination is performed under reduced pressure with the air pressure being set to 20 mmHg (26.7 hPa) or less. In addition, the lamination process can be intermittent or continuous using a roller. The vacuum lamination method can be performed using a commercially available vacuum laminator. As commercially available vacuum laminators, for example, vacuum applicators manufactured by Nicol Materials, vacuum pressurized laminators manufactured by Namki Manufacturing, roller drying coaters manufactured by Hitachi Instruments, vacuum laminators manufactured by Hitachi Airship, etc. can be cited.

[0200] <Step (II)> After the photosensitive resin composition layer is provided on the circuit substrate, an exposure step is then performed to irradiate a predetermined portion of the photosensitive resin composition layer with active light through a mask pattern. Examples of active light include ultraviolet rays, visible rays, electron beams, and X-rays, and ultraviolet rays are particularly preferred. The irradiation amount of ultraviolet rays is generally 10 mJ / cm 2 ~1000mJ / cm2 The exposure method includes a contact exposure method in which a mask pattern is brought into close contact with a circuit board and a non-contact exposure method in which exposure is performed using parallel light without bringing the mask pattern into close contact. Both methods can be used.

[0201] In step (II), as the mask pattern, a through hole pattern such as a circular hole pattern can be used. For example, a mask pattern capable of forming a latent image of a through hole having a desired through hole diameter (opening diameter) can be used. The through hole diameter (opening diameter) is preferably 100 μm or less, more preferably 90 μm or less, and further preferably 80 μm or less. The lower limit is not particularly limited, and may be 0.1 μm or more, 0.5 μm or more, etc.

[0202] After exposure, a heat treatment may be performed as necessary. The heat treatment can rapidly reduce the solubility of the exposed portion (exposed area) of the photosensitive resin composition layer in the developer.

[0203] <Step (III)> After the exposure step, a development step is performed to remove the unexposed portion (non-exposed portion) of the photosensitive resin composition layer using a developer, thereby forming holes in the photosensitive resin composition layer and obtaining a desired pattern. Development is usually performed by wet development.

[0204] In the case of the wet development, a safe, stable and easy-to-operate developer such as an alkaline solution, an aqueous developer or an organic solvent is generally used as the developer. In addition, a known method such as spraying, shaking immersion, brushing or scrubbing is appropriately used as the developing method.

[0205] As the alkaline aqueous solution used as the developer, there can be listed, for example, an aqueous solution of an alkali metal hydroxide such as lithium hydroxide, sodium hydroxide, potassium hydroxide, a carbonate or bicarbonate such as sodium carbonate, sodium bicarbonate, an alkali metal phosphate such as sodium phosphate, potassium phosphate, an alkali metal pyrophosphate such as sodium pyrophosphate, potassium pyrophosphate, and an aqueous solution of an organic base that does not contain metal ions such as tetraalkylammonium hydroxide. From the viewpoint of not containing metal ions and not affecting the semiconductor chip, an aqueous solution of tetramethylammonium hydroxide (TMAH) is preferred.

[0206] In order to improve the development effect, these alkaline aqueous solutions may contain additives such as surfactants and defoamers. The pH of the alkaline aqueous solution is preferably in the range of 8 to 12, and more preferably in the range of 9 to 11. In addition, the alkali concentration of the alkaline aqueous solution is preferably set to 0.1% by mass to 10% by mass. The temperature of the alkaline aqueous solution can be appropriately selected according to the developability of the photosensitive resin composition layer, and is preferably set to 20°C to 50°C.

[0207] Examples of organic solvents used as the developer include acetone, ethyl acetate, alkoxyethanol having an alkoxy group having 1 to 4 carbon atoms, ethanol, isopropanol, butanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, cyclopentanone, and cyclohexanone.

[0208] The concentration of such an organic solvent is preferably 2% to 90% by mass relative to the total amount of the developer. In addition, the temperature of such an organic solvent can be adjusted according to the developability. Furthermore, such an organic solvent can be used alone or in combination of two or more. As an organic solvent-based developer used alone, for example, 1,1,1-trichloroethane, N-methylpyrrolidone, N,N-dimethylformamide, cyclopentanone, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone can be listed.

[0209] In pattern formation, two or more developing methods may be used in combination as needed. The developing methods include immersion, puddle, spray, high-pressure spray, brushing, scrubbing, etc. In order to improve the resolution, the high-pressure spray is suitable. When the spray method is used, the spray pressure is preferably 0.05 MPa to 0.3 MPa.

[0210] <Thermal Curing (Post-baking) Process> After the above step (III) is completed, a thermal curing (post-baking) step is performed as needed. In the above steps (I) to (III), the photosensitive resin composition layer may sometimes be cured, but by further curing the photosensitive resin composition layer through a thermal curing step, an insulating layer with better mechanical strength can be obtained. As a thermal curing step, a heating step using a clean oven and the like can be listed. The atmosphere during thermal curing can be in air or in an inert gas atmosphere such as nitrogen. In addition, the heating conditions can be appropriately selected according to factors such as the type and content of the resin components in the first photosensitive resin composition layer and the second photosensitive resin composition layer. The specific heating conditions are preferably selected in the range of 150°C to 300°C and 20 minutes to 300 minutes, and more preferably in the range of 170°C to 250°C and 30 minutes to 240 minutes.

[0211] <Optional Process> The method for manufacturing a semiconductor package substrate may further include a hole-forming step and a desmearing step after forming an insulating layer in the form of a cured photosensitive resin composition layer. These steps may be performed according to various methods known to those skilled in the art for manufacturing semiconductor package substrates.

[0212] After forming the insulating layer, the insulating layer formed on the circuit substrate is subjected to a hole-opening process as desired to form through holes and via holes. The hole-opening process can be performed by known methods such as drilling, laser, plasma, or a combination of these methods as required. Among them, the hole-opening process based on lasers such as carbon dioxide lasers and YAG lasers is preferred.

[0213] The decontamination process is a process of performing a decontamination treatment on the insulating layer. Resin residue (dirt) is usually attached to the inside of the openings such as through holes and via holes formed in the hole opening process. The dirt may cause poor electrical connection, so it is preferred to perform a process (decontamination treatment) to remove the dirt in this process.

[0214] The decontamination treatment may be performed by dry decontamination treatment, wet decontamination treatment, or a combination thereof.

[0215] As dry decontamination treatment, for example, decontamination treatment using plasma can be cited. Decontamination treatment using plasma can be performed using a commercially available plasma decontamination treatment device. Among the commercially available plasma decontamination treatment devices, examples suitable for use in manufacturing semiconductor package substrates include a microwave plasma device manufactured by Nissin Corporation and a normal pressure plasma etching device manufactured by Sekisui Chemical Co., Ltd.

[0216] As wet decontamination treatment, for example, decontamination treatment using an oxidant solution can be listed. When using an oxidant solution for decontamination treatment, it is preferred to sequentially perform swelling treatment using a swelling solution, oxidation treatment using an oxidant solution, and neutralization treatment using a neutralizing solution. As swelling solution, for example, “Suwering Design Sealing P” and “Suwering Design Sealing SBU” manufactured by Attech Japan can be listed. The swelling treatment is preferably performed by immersing a substrate having openings such as through holes in a swelling solution heated to 60°C to 80°C for 5 to 10 minutes. As the oxidant solution, an alkaline permanganate aqueous solution is preferred, and examples thereof include a solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The oxidation treatment based on the oxidant solution is preferably carried out by immersing the substrate after the swelling treatment in an oxidant solution heated to 60°C to 80°C for 10 minutes to 30 minutes. Commercially available products of alkaline permanganate aqueous solutions include, for example, "Concentrator Conpack CP" and "Document Soluble Sonic Sciugane P" manufactured by Attech Japan. The neutralization treatment based on a neutralizing solution is preferably carried out by immersing the substrate after the oxidation treatment in a neutralizing solution at 30°C to 50°C for 3 minutes to 10 minutes. As a neutralizing liquid, an acidic aqueous solution is preferable, and an example of a commercially available product is "Lytronic P" manufactured by Atotron Co., Ltd.

[0217] When the dry decontamination treatment and the wet decontamination treatment are performed in combination, the dry decontamination treatment may be performed first, or the wet decontamination treatment may be performed first.

[0218] When the insulating layer is formed as any one of the redistribution forming layer, the interlayer insulating layer and the solder resist layer, the hole opening step and the desmearing step may be performed after the thermal curing step. In addition, in the method for manufacturing a semiconductor package substrate, a conductor layer forming step may be further performed.

[0219] The conductor layer forming step is a step of forming a conductor layer on the insulating layer. The conductor layer can be formed by sputtering after the insulating layer is formed. In addition, the conductor layer can be formed by combining electroless plating with electrolytic plating. Furthermore, a plating resist layer opposite to the pattern of the conductor layer can be formed, and the conductor layer can be formed only by electroless plating. As a subsequent pattern forming method, for example, a subtractive method, a semi-additive method, etc. known to those skilled in the art can be used.

[0220] The semiconductor package substrate described in the second example can be manufactured using the first photosensitive resin composition and the second photosensitive resin composition, and the cured product of the first photosensitive resin composition and the second photosensitive resin composition can be used as an insulating layer. The first photosensitive resin composition and the second photosensitive resin composition are as described above. Specifically, the method for manufacturing the semiconductor package substrate described in the second example includes: (a) a step of applying a second photosensitive resin composition on a circuit substrate and drying the composition to form a second photosensitive resin composition layer; (b) a step of coating the first photosensitive resin composition on the second photosensitive resin composition layer and drying the first photosensitive resin composition to form the first photosensitive resin composition layer; (c) irradiating the first photosensitive resin composition layer and the second photosensitive resin composition layer with active light; and (d) A step of developing the first photosensitive resin composition layer and the second photosensitive resin composition layer.

[0221] In step (a), the second resin varnish containing the second photosensitive resin composition is directly applied on the circuit board and dried to form a second photosensitive resin composition layer on the circuit board. The second resin varnish is as described above.

[0222] The coating method of the second resin varnish is the same as the coating method of the second resin varnish in the method for producing a photosensitive film.

[0223] In step (b), a first resin varnish containing a first photosensitive resin composition is applied on the first photosensitive resin composition layer and dried to form the first photosensitive resin composition layer on the second photosensitive resin composition layer. The first resin varnish is as described above.

[0224] The coating method of the first resin varnish is the same as the coating method of the first resin varnish in the method for producing a photosensitive film.

[0225] Step (c) is the same as step (II). Step (d) is the same as step (III).

[0226] The semiconductor package substrate described in the third example can be manufactured using the above-mentioned photosensitive film or the first photosensitive resin composition and the second photosensitive resin composition, and the cured product of the photosensitive resin composition layer is used as a redistribution forming layer. Specifically, the method for manufacturing the semiconductor package substrate described in the third example includes: (A) a step of laminating a temporary fixing film on a substrate; (B) a step of temporarily fixing the semiconductor chip on a temporary fixing film; (C) forming a sealing layer on the semiconductor chip; (D) a step of peeling the substrate and the temporary fixing film from the semiconductor chip; (E) forming a redistribution forming layer as an insulating layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled off; (F) forming a redistribution layer as a conductor layer on the redistribution formation layer; and (G) A step of forming a solder resist layer on the redistribution layer. In addition, the manufacturing method of the semiconductor package substrate may include: (H) A step of cutting a plurality of semiconductor package substrates into individual semiconductor package substrates to separate them into pieces.

[0227] <Step (A)> Step (A) is a step of laminating a temporary fixing film on a substrate. The lamination conditions of the substrate and the temporary fixing film are not particularly limited, and for example, it is preferred that the pressing temperature (lamination temperature) is preferably set to 70°C to 140°C, and the pressing pressure is preferably set to 1 kgf / cm 2 ~11kgf / cm 2 , the pressing time is preferably set to 5 seconds to 300 seconds, and the air pressure is set to a reduced pressure of less than 20 mmHg for lamination. In addition, the lamination process can be intermittent or continuous using a roller. The vacuum lamination method can be carried out using a commercially available vacuum laminator. As commercially available vacuum laminators, for example, vacuum applicators made by Nicol Materials, vacuum pressurized laminators made by Namki Manufacturing, roller drying coaters made by Hitachi Instruments, vacuum laminators made by Hitachi Airship, etc. can be listed.

[0228] As the substrate, for example, there can be listed silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, cold-rolled steel sheets (SPCC); FR-4 substrates and other substrates in which epoxy resins or the like are impregnated into glass fibers and then heat-cured; substrates containing bismaleimide triazine resins such as BT resins, etc.

[0229] Any material that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip can be used as the temporary fixing film. Examples of commercially available products include "LIVA ALFA" manufactured by Nitto Denko Corporation.

[0230] <Process (B)> Step (B) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using a device such as a flip chip bonding machine or a chip bonding machine. The configuration design and the number of semiconductor chips can be appropriately set according to the shape and size of the temporary fixing film, the number of semiconductor package substrates to be produced as the target, etc. For example, the semiconductor chips can be arranged in a matrix of several rows and columns and temporarily fixed.

[0231] <Process (C)> Step (C) is a step of forming a sealing layer on a semiconductor chip. The sealing layer can be made of any insulating material, and the first and / or second photosensitive resin composition can be used. The sealing layer is usually formed by a method including a step of forming a sealing resin composition layer on a semiconductor chip and a step of thermally curing the resin composition layer to form the sealing layer.

[0232] The formation of the sealing resin composition layer is preferably carried out by compression molding. In the compression molding method, the semiconductor chip and the sealing resin composition are usually arranged in a mold, and pressure and heat are applied to the sealing resin composition in the mold as needed to form a sealing resin composition layer covering the semiconductor chip.

[0233] The specific operation of the compression molding method can be operated as follows. As a compression molding mold, an upper mold and a lower mold are prepared. In addition, as described above, the semiconductor chip temporarily fixed to the temporary fixing film is coated with a sealing resin composition. The semiconductor chip coated with the sealing resin composition is installed in the lower mold together with the substrate and the temporary fixing film. Thereafter, the upper mold and the lower mold are matched, and heat and pressure are applied to the sealing resin composition for compression molding.

[0234] In addition, the specific operation of the compression molding method can be operated as follows. As a compression molding mold, an upper mold and a lower mold are prepared. The lower mold is made to carry a sealing resin composition. In addition, the semiconductor chip is installed in the upper mold together with the substrate and the temporary fixing film. Thereafter, the upper mold and the lower mold are matched, and heat and pressure are applied to carry out compression molding in a way that the sealing resin composition carried on the lower mold contacts the semiconductor chip installed in the upper mold.

[0235] The molding conditions vary depending on the composition of the sealing resin composition. In order to achieve good sealing, appropriate conditions can be adopted. For example, the mold temperature during molding is preferably a temperature at which the sealing resin composition can exert excellent compression moldability, preferably 80°C or more, more preferably 100°C or more, particularly preferably 120°C or more, and preferably 200°C or less, more preferably 170°C or less, and particularly preferably 150°C or less. In addition, the pressure applied during molding is preferably 1MPa or more, more preferably 3MPa or more, particularly preferably 5MPa or more, and preferably 50MPa or less, more preferably 30MPa or less, and particularly preferably 20MPa or less. The curing time is preferably 1 minute or more, more preferably 2 minutes or more, particularly preferably 5 minutes or more, and preferably 60 minutes or less, more preferably 30 minutes or less, and particularly preferably 20 minutes or less. Usually, after forming the sealing resin composition layer, the mold is removed. The removal of the mold can be performed before the thermal curing of the sealing resin composition layer, or after the thermal curing.

[0236] The compression molding method can be performed by spraying the sealing resin composition filled in the case into the lower mold.

[0237] <Process (D)> Step (D) is a step of peeling the substrate and the temporary fixing film from the semiconductor chip. The peeling method is expected to adopt an appropriate method that is consistent with the material of the temporary fixing film. As a peeling method, for example, a method of heating the temporary fixing film to make it foam or expand and peel it off can be cited. In addition, as a peeling method, for example, a method of irradiating the temporary fixing film with ultraviolet rays through the substrate to reduce the adhesive force of the temporary fixing film and peeling it off can be cited.

[0238] In the method of heating the temporary fixing film to make it foam or expand and then peel it off, the heating conditions are usually 100°C to 250°C for 1 second to 90 seconds or 5 minutes to 15 minutes. In the method of irradiating ultraviolet rays to reduce the adhesive force of the temporary fixing film and then peel it off, the irradiation amount of ultraviolet rays is usually 10mJ / cm 2 ~1000mJ / cm 2 .

[0239] <Step (E)> Step (E) is a step of forming a redistribution forming layer as an insulating layer on the surface of the semiconductor chip after the substrate and the temporary fixing film are peeled off. The redistribution forming layer can be formed using the above-mentioned photosensitive film or the first photosensitive resin composition and the second photosensitive resin composition. The method for forming the redistribution forming layer can form a photosensitive resin composition layer by the same method as step (I) in the first example, and may include an operation of forming a photosensitive resin composition layer by the same method as steps (a) and (b) in the second example.

[0240] When forming the redistribution forming layer, a through hole may be formed in the redistribution forming layer in order to establish an interlayer connection between the semiconductor chip and the redistribution forming layer.

[0241] The through hole is usually formed by performing an exposure process and a development process, in which the surface of the photosensitive resin composition layer for forming the redistribution forming layer is irradiated with active light through a mask pattern, and in the development process, the non-exposed portion not irradiated by the active light is removed by development. The irradiation amount and irradiation time of the active light can be appropriately set according to the photosensitive resin composition layer. As the exposure method, for example, a contact exposure method in which the mask pattern is closely attached to the photosensitive resin composition layer and exposed; a non-contact exposure method in which the mask pattern is not closely attached to the photosensitive resin composition layer, but exposed using parallel light, etc. can be cited. The exposure and development methods can be performed as described in the first example.

[0242] The shape of the through hole is not particularly limited, and is usually set to be circular (substantially circular). The top diameter of the through hole is preferably 100 μm or less, more preferably 90 μm or less, and further preferably 80 μm or less, and is preferably 0.1 μm or more, preferably 0.5 μm or more, and more preferably 1.0 μm or more. Here, the top diameter of the through hole refers to the opening diameter of the through hole on the surface of the redistribution formation layer.

[0243] After forming the photosensitive resin composition layer and forming the through hole as needed, a thermal curing step may be performed. The thermal curing method may be performed as described in the first example.

[0244] <Process (F)> Step (F) is a step of forming a redistribution layer as a conductor layer on the redistribution formation layer. The method of forming the redistribution layer on the redistribution formation layer may be the same as the method of forming the conductor layer on the insulating layer in the first example. Alternatively, steps (E) and (F) may be repeated to alternately stack (build up) the redistribution layer and the redistribution formation layer.

[0245] <Step (G)> Step (G) is a step of forming a solder resist layer on the redistribution layer. The material of the solder resist layer can use any material with insulating properties. Among them, from the perspective of ease of manufacturing of the semiconductor package substrate, photosensitive resins and thermosetting resins are preferred. In addition, the above-mentioned first or second photosensitive resin composition can be used.

[0246] In step (G), a convex process to form a bump can be performed as needed. The convex process can be performed by a solder ball, solder, etc. In addition, the formation of a through hole in the convex process can be performed in the same manner as in step (E).

[0247] The method for manufacturing a semiconductor package substrate may include step (H) in addition to steps (A) to (G). Step (H) is a step of cutting a plurality of semiconductor package substrates into individual semiconductor package substrates to achieve singulation. The method for cutting a semiconductor package substrate into individual semiconductor package substrates is not particularly limited.

[0248] [Semiconductor devices] The semiconductor device includes the semiconductor package substrate. As the semiconductor device on which the semiconductor package substrate is mounted, various semiconductor devices for electrical products (such as computers, mobile phones, smart phones, tablet devices, wearable devices, digital cameras, medical equipment, and televisions) and vehicles (such as motorcycles, automobiles, trains, ships, and aircrafts) can be cited. Example

[0249] The present invention is specifically described below with reference to the examples, but the present invention is not limited to these examples. It should be noted that, in the following description, the "parts" and "%" indicating the amount refer to "parts by mass" and "% by mass" respectively unless otherwise expressly stated. In addition, the operations described below are performed in an atmosphere at normal temperature and pressure (25° C., 1 atm) unless otherwise expressly stated.

[0250] [Synthesis Example 1: Synthesis of Polymer A-1] Under a nitrogen stream, 105.6 g of 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride (MCTC) and 500 g of γ-butyrolactone were added to a 1 L separable flask and dissolved. 104.3 g of 1-(4-aminophenyl)-1,3,3-trimethylindaneamine (PIDA) was added thereto, and the mixture was reacted at 50°C for 20 hours to obtain polyamic acid. 111.3 g of glycidyl methacrylate and 0.42 g of 4-methoxyphenol were added thereto, and the mixture was reacted at 50°C for 20 hours to obtain a solution of polymer A-1 (solid content: 33%) as a polyimide precursor. When the molecular weight of polymer A-1 was measured by gel permeation chromatography (standard polystyrene conversion), the weight average molecular weight (Mw) was 16,000. The structural units of the polymer A-1 which is a polyimide precursor are shown below (n represents an integer of 5 to 200). [Chemistry 48]

[0251] [Synthesis Example 2: Synthesis of Polymer A-2] In a dry reactor equipped with a stirrer, a condenser, an internal thermometer and a flat-bottomed joint, 20.0 g (64.5 mmol) of oxydiphthalic dianhydride was suspended in 140 mL of diglyme while removing water. 16.8 g (129 mmol) of 2-hydroxyethyl methacrylate, 0.05 g of hydroquinone, 0.05 g of pure water and 10.7 g (135 mmol) of pyridine were added, and the mixture was stirred at 60°C for 18 hours. Then, after the mixture was cooled to -20°C, 16.1 g (135.5 mmol) of thionyl chloride was added dropwise over 90 minutes. A white precipitate of pyridinium hydrochloride was obtained. Then, the mixture was heated to room temperature and stirred for 2 hours, and then 9.7 g (123 mmol) of pyridine and 25 mL of N-methylpyrrolidone (NMP) were added to obtain a transparent solution. Next, add the substance obtained by dissolving 4,4'-diaminodiphenyl ether 11.8g (58.7 mmol) in NMP100mL to the obtained transparent solution by dropwise addition for 1 hour. Then, add 5.6g (17.5 mmol) of methanol and 0.05g of 3,5-di-tert-butyl-4-hydroxytoluene, and stir the mixture for 2 hours. Next, precipitate the polymer A-2 as a polyimide precursor in 4 liters of water, and stir the water-polyimide precursor resin mixture at a speed of 500rpm for 15 minutes. Filter the polymer A-2, stir again in 4 liters of water for 30 minutes, and filter again. Then, the obtained polymer A-2 is dried at 45°C under reduced pressure for 3 days. The weight average molecular weight of the obtained polymer A-2 is 24,800 and the number average molecular weight is 10,500. The structural unit of the polymer A-2 as a polyimide precursor is shown below. [Chemistry 49]

[0252] [Synthesis Example 3: Synthesis of Polyimide A-3] Under a nitrogen stream, in a 1L separable flask, 104g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) was added to 383g of γ-butyrolactone to dissolve it. 60.1g of 5,5'-methylenebis(2-aminobenzoic acid) (MBAA) was added thereto, and the reaction was carried out at 50°C for 20 hours to obtain polyamic acid (polyimide precursor). 55g of toluene was added thereto, and azeotropic dehydration was carried out for 5 hours. Thereafter, the reaction solution was heated to a temperature of 204°C to remove the toluene to obtain a polyimide solution. After cooling to room temperature, 59.6g of glycidyl methacrylate and 0.45g of 4-methoxyphenol were added, and the reaction was carried out at 100°C for 5 hours to obtain a polyimide solution (A-3) (solid content of 33%). When the molecular weight of the polyimide solution (A-3) was measured by gel permeation chromatography (in terms of standard polystyrene), the weight average molecular weight (Mw) was 30,000. The structural units of the polymer A-3 as the polyimide are shown below. [Chemistry 50]

[0253] [Examples 1 to 13 and Comparative Examples 1 to 4] (Preparation of First Photosensitive Resin Composition and Second Photosensitive Resin Composition) The reagents shown in the table described below are mixed in the amounts (parts by mass) shown in the table, stirred using a high-speed rotating stirrer, and a varnish-like first photosensitive resin composition is prepared. A varnish-like second photosensitive resin composition is prepared in the same manner as the first photosensitive resin composition. In the table, the amount of each reagent represents the amount of solid components of each reagent when the solid component (polyimide precursor) contained in the (A) component solution manufactured in the above-mentioned synthesis example is set to 100 parts by mass. In the table, the solid content represents the content when the (A) component is converted to 100 parts by mass. The addition amount of the (B-1) component represents the content of the (B-1) component in the photosensitive resin composition when the (A) component is set to 100 parts by mass, the addition amount of the (B-2) component represents the content of the (B-2) component in the photosensitive resin composition when the (A) component is set to 100 parts by mass, and the addition amount of the (B) component represents the content of the (B) component in the photosensitive resin composition when the (A) component is set to 100 parts by mass. In addition, polymer A-2 was used as a γ-butyrolactone solution having a solid content of 33%.

[0254] (Manufacturing of photosensitive film) As a support, a PET film ("Lumirror T6AM" manufactured by Toray Industries, Ltd., with a thickness of 38 μm) was prepared. The first photosensitive resin composition prepared in each example and comparative example was uniformly applied to the support using a die coater so that the thickness of the photosensitive resin composition layer after drying was 30 μm, and dried at 80° C. to 120° C. for 6 minutes to form a first photosensitive resin composition layer. This is referred to as photosensitive sheet A.

[0255] Similarly, a PET film ("Lumirror T6AM" manufactured by Toray Industries, Ltd., thickness 38 μm) was prepared as a support. The second photosensitive resin composition prepared in each example and comparative example was uniformly applied to the support using a die coater so that the thickness of the photosensitive resin composition layer after drying was 30 μm, and dried at 80° C. to 120° C. for 6 minutes to form a second photosensitive resin composition layer. This is referred to as a photosensitive sheet B.

[0256] The photosensitive sheets A and B were laminated using a manual vacuum press laminator (manufactured by NICO MATERIALS, diaphragm laminator "V-160") so that the first photosensitive resin composition and the second photosensitive resin composition layer were bonded to each other, thereby obtaining a 60 μm two-layer photosensitive resin composition layer. The pressing conditions were as follows: vacuuming time 30 seconds, pressing temperature 60°C, pressing pressure 0.7 MPa, and pressing time 180 seconds.

[0257] (Determination of absorbance) Photosensitive sheets A and B were prepared (only photosensitive sheet B was prepared in Comparative Example 1). The first photosensitive resin composition layer and the second photosensitive resin composition layer in the photosensitive sheets A and B were cut into 3 cm squares, and the reference was set to the PET film "Lumirror T6AM" used as a support, and the total transmittance at 3 points was measured. The thickness of the sheet used in the measurement was measured, and the average value of the transmittance at 3 points was converted into a value of 30 μm in thickness as the absorbance. Here, the absorbance of the first photosensitive resin composition layer and the second photosensitive resin composition layer was obtained by measuring the total transmittance T (%) at a wavelength of 365 nm for each photosensitive resin composition layer and using the following formula. Absorbance = 2-log(T)

[0258] [Table 1] [Table 2]

[0259] The details of each reagent in the table are as follows. (A)Ingredients Polymer A-1: ​​Polymer A-1 synthesized in Synthesis Example 1 Polymer A-2: Polymer A-2 synthesized in Synthesis Example 2 Polymer A-3: Polymer A-3 synthesized in Synthesis Example 3 (B) Ingredients (B-1) Ingredients · Irgacure OXE02: Oxime ester-based photoradical generator, photopolymerization initiator represented by the following formula ("Irgacure OXE02" manufactured by BASF Corporation) [Chemistry 51] · Irgacure OXE01: Oxime ester-based photoradical generator, photopolymerization initiator represented by the following formula ("Irgacure OXE01" manufactured by BASF Corporation) [Chemistry 52] (B-2) Ingredients · Omnirad819: (acylphosphine-based photoradical generator, manufactured by IGM, “Omnirad819”) · Omnirad TPO: (acylphosphine-based photoradical generator, manufactured by IGM, "Omnirad TPO") (C) Ingredients TMPT: a tetrafunctional or less photocrosslinking agent represented by the following formula ("TMPT" manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) [Chemistry 53] DPHA: Dipentaerythritol hexaacrylate, made by Nippon Kayaku Co., Ltd., 5-functional or 6-functional · A-TMPT: a tetrafunctional or less photocrosslinking agent represented by the following formula ("A-TMPT" manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) [Chemistry 54] ·M-933: Dipentaerythritol tetraacrylate, manufactured by Toa Gosei Co., Ltd.

[0260] <Evaluation of limiting resolution> A copper-plated layer is stacked on a silicon wafer with a thickness of 5 μm, and a roughening treatment is performed for 60 seconds using a 1% hydrochloric acid aqueous solution. A second photosensitive resin composition layer of a photosensitive film is arranged on the substrate thus obtained in a manner in contact with the surface of the copper layer, and stacked using a vacuum laminator (manufactured by Meiki Manufacturing Co., Ltd., MVLP5000 / 600-IIW) to form a laminated body in which a copper-plated layer, a second photosensitive resin composition layer, a first photosensitive resin composition layer and a support are stacked in sequence (Comparative Example 1 is a laminated body in which a copper-plated layer, a second photosensitive resin composition layer and a support are stacked in sequence). The pressing conditions are set to a vacuum time of 30 seconds, a pressing temperature of 80°C, a pressing pressure of 0.7 MPa, and a pressing time of 30 seconds. After standing at room temperature for 30 minutes, the support is peeled off from the aforementioned laminated body. The laminated body after the support is peeled off is subjected to ultraviolet light (wavelength 365nm, intensity 40mW / cm 2 ) for exposure. The exposure amount was set to 200 mJ / cm 2 range. The exposure pattern uses a quartz glass mask depicting circular holes (through holes) with opening diameters of 20μm, 30μm, 40μm, 50μm, 60μm, and 70μm. After standing at room temperature for 5 minutes, a heat treatment is performed at 100°C for 3 minutes. For the entire surface of the photosensitive resin composition layer on the laminate, 23°C cyclopentanone as a developer is sprayed for development at a spray pressure of 0.1MPa for an optimal time between 30 seconds and 100 seconds, and then propylene glycol monomethyl ether acetate is sprayed for 30 seconds at a spray pressure of 0.1MPa. Furthermore, a heat treatment of 180°C for 180 minutes is performed to cure the photosensitive resin composition layer. It is referred to as an evaluation sample. The bottom diameter of the through hole of the evaluation sample is observed using a scanning electron microscope (SEM) (magnification of 1000 times), and the minimum size that can be opened without residue and peeling is set as the limit opening through hole. The evaluation is performed according to the following evaluation criteria. ○: The aspect ratio of the maximum opening through-hole diameter (film thickness (μm) / through-hole diameter (μm)) is 1.0 or more △: The aspect ratio of the critical opening through-hole diameter (film thickness (μm) / through-hole diameter (μm)) is 0.5 or more and less than 1.0 ×: The aspect ratio of the maximum opening hole diameter (film thickness (μm) / hole diameter (μm)) is less than 0.5

[0261] In addition, the exposure was set to 300 mJ / cm 2 、400mJ / cm 2 and 500mJ / cm 2 The same evaluation is also carried out for the situation with a range of .

[0262] <Evaluation of Cross-sectional Shape (Undercut Resistance)> Regarding the observation of undercut, for the evaluation sample, a through hole with an opening diameter of 70 μm was observed using SEM (magnification 2000 times). The radius (μm) of the top and the radius (μm) of the bottom of the cross section of the through hole were measured using SEM, and the difference between the radius of the bottom and the radius of the top was calculated (radius of the bottom - radius of the top), and the calculated value was set as undercut, and the evaluation was performed according to the following evaluation criteria. ◎: No undercut. ○: Undercut is less than 2 μm. △: Undercut is 2 μm or more and 4 μm or less. ×: The undercut is larger than 4 μm or a through hole with an opening diameter of 70 μm is not opened.

[0263] <Evaluation of Adhesion> A copper plating layer is stacked on a silicon wafer with a thickness of 5 μm, and a roughening treatment is performed for 60 seconds using a 1% hydrochloric acid aqueous solution. On the substrate thus obtained, the second photosensitive resin composition layer of the photosensitive film is arranged in contact with the surface of the copper layer, and a vacuum laminator (manufactured by Nicol Materials, VP160) is used for lamination to form a laminate having a copper plating layer, a second photosensitive resin composition layer, a first photosensitive resin composition layer and a support laminated in sequence. The pressing conditions are set to a vacuum time of 30 seconds, a pressing temperature of 60°C, a pressing pressure of 0.7 MPa, and a pressing time of 30 seconds. After standing at room temperature for 30 minutes, the support is peeled off from the aforementioned laminate. The laminate after the support is peeled off is subjected to ultraviolet light (wavelength 365 nm, intensity 40 mW / cm 2 ) for exposure. The exposure amount was set to 200 mJ / cm 2 range. The exposure pattern uses a quartz glass mask depicting a circular hole (through hole) with an opening diameter of 70 μm. After standing at room temperature for 5 minutes, a heat treatment is performed at 100°C for 3 minutes. For the entire surface of the photosensitive resin composition layer on the laminate, 23°C cyclopentanone as a developer is sprayed for development at a spray pressure of 0.1 MPa for an optimal time between 30 seconds and 100 seconds, and then propylene glycol monomethyl ether acetate is sprayed for 30 seconds at a spray pressure of 0.1 MPa. Then, a heat treatment of 170°C for 180 minutes is performed to cure the photosensitive resin composition layer. For the bottom diameter of the through hole, the cross-section of the 70 μm circular hole is observed using SEM (magnification of 2000 times) to confirm whether there is peeling between the substrate and the photosensitive resin composition layer of the photosensitive film (hereinafter, the peeling between the substrate and the photosensitive resin composition layer of the photosensitive film is sometimes referred to as a halo). When a halo was observed, the distance of peeling from the side surface of the through-hole was measured and the distance was taken as the halo distance, and the evaluation was performed according to the following evaluation criteria. ◎: No halo. ○: Halo distance is less than 2 μm. △: The halo distance is 2 μm or more and 4 μm or less. ×: The halo distance is greater than 4 μm or a through hole with a through hole diameter of 70 μm is not opened.

[0264] [Table 3] [Table 4]

Claims

1. A photosensitive film comprising a support and a photosensitive resin composition layer provided on the support, The photosensitive resin composition layer includes, in order from the support side, a first photosensitive resin composition layer including a first photosensitive resin composition and a second photosensitive resin composition layer provided on the first photosensitive resin composition layer including a second photosensitive resin composition. The first photosensitive resin composition and the second photosensitive resin composition respectively include: (A) one or more resins selected from polyimide and polyimide precursors; (B) a photoradical generator; and (C) a photocrosslinking agent, The difference between the absorbance of the second photosensitive resin composition layer and the absorbance of the first photosensitive resin composition layer (absorbance of the second photosensitive resin composition layer−absorbance of the first photosensitive resin composition layer) is 0.05 or more and 0.5 or less.

2. The photosensitive film according to claim 1, wherein The component (A) contains a structural unit represented by the following formula (A-1): [Chemistry 1] In formula (A-1), A each independently represents a tetravalent organic group, B represents a divalent organic group, and R 1 and R 2 Each independently represents a hydrogen atom or a monovalent organic group.

3. The photosensitive film according to claim 2, wherein R in formula (A-1) 1 and R 2 Each independently, and at least one is a free radical reactive group.

4. The photosensitive film according to claim 3, wherein The free radical reactive groups are each independently represented by the following formula (A-2): [Chemistry 2] In formula (A-2), R 4a , R 5a and R 6a Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, X represents a divalent organic group, and * represents a bond.

5. The photosensitive film according to claim 1, wherein (B) The component contains (B-1) a highly reactive photoradical generator and (B-2) a photoradical generator having excellent deep curing properties.

6. The photosensitive film according to claim 1, wherein The content of the component (B) contained in the first photosensitive resin composition is smaller than the content of the component (B) contained in the second photosensitive resin composition.

7. The photosensitive film according to claim 1, wherein The content of the component (B) in the first photosensitive resin composition is 0.03 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the component (A) in the first photosensitive resin composition.

8. The photosensitive film according to claim 1, wherein The content of the component (B) in the second photosensitive resin composition is 0.05 parts by mass or more and 8 parts by mass or less relative to 100 parts by mass of the component (A) in the second photosensitive resin composition.

9. The photosensitive film according to claim 1, wherein The absorbance of the first photosensitive resin composition layer is 0.2 or more and 1.5 or less.

10. The photosensitive film according to claim 1, wherein The absorbance of the second photosensitive resin composition layer is 0.3 or more and 1.5 or less.

11. The photosensitive film according to claim 1, wherein The nonvolatile component of the first photosensitive resin composition is 100 mass %, and the content of the component (B-1) in the first photosensitive resin composition is b 1-1 , the content of the component (B-1) in the second photosensitive resin composition is set to b 1-2 When b 1-1 / b 1-2 It is 0.1 or more and 3 or less. 12 . A semiconductor package substrate comprising an insulating layer comprising a cured product of a photosensitive resin composition layer of the photosensitive film according to claim 1 .

13. A semiconductor device comprising the semiconductor package substrate according to claim 12.

14. A method for manufacturing a semiconductor package substrate, comprising: A step of laminating a photosensitive resin composition layer of the photosensitive film according to any one of claims 1 to 11 on a circuit board; a step of irradiating the photosensitive resin composition layer with active light; and A step of developing the photosensitive resin composition layer.

15. A method for manufacturing a semiconductor package substrate, comprising: A step of coating a second photosensitive resin composition on a circuit substrate to form a second photosensitive resin composition layer; A step of coating the first photosensitive resin composition on the second photosensitive resin composition layer to form the first photosensitive resin composition layer; a step of irradiating the first photosensitive resin composition layer and the second photosensitive resin composition layer with active light; and a step of developing the first photosensitive resin composition layer and the second photosensitive resin composition layer, The first photosensitive resin composition and the second photosensitive resin composition respectively include: (A) one or more resins selected from polyimide and polyimide precursors; (B) a photoradical generator; and (C) a photocrosslinking agent, The difference in absorbance between the first photosensitive resin composition layer and the second photosensitive resin composition layer is 0.05 or more and 0.5 or less.

Citation Information

Patent Citations

  • Photosensitive polyimide precursor composition and its manufacture

    JP1999015152A

  • Negative photosensitive resin composition, method for producing pattern and electronic parts

    JP2003084435A

  • Polyamic acid composition and polyimide composition

    JP2015209461A

  • Polyamic acid composition and polyimide composition

    JP2015214680A