Negative electrode active material for nonaqueous electrolyte secondary battery comprising silicon oxide composite and method for preparing same

By introducing a silicon oxide composite with a porous structure of 50nm to 300nm into the negative electrode material of the lithium secondary battery, buffering the expansion pressure, the volume change problem caused by lithium ion reaction is solved, and the life and capacity characteristics of the lithium secondary battery are improved.

CN119069675APending Publication Date: 2024-12-03DAEJOO ELECTRONICS MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411207901.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-12-01
Filing Date
2018-12-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The negative electrode material of lithium secondary batteries has volume expansion and contraction due to lithium-ion alloying/non-alloyation reaction, resulting in a decrease in life characteristics. The average unit mass capacity of existing carbon materials is small, making it difficult to achieve high capacity.

Method used

The silicon oxide composite containing silicon oxide composite as the negative electrode active material and contains a pore structure with a diameter of 50nm to 300nm. The life characteristics of the lithium secondary battery are improved through the pore buffering expansion pressure, and the lithium secondary battery is secondary. Preparation method of battery preparation this material.

Benefits of technology

Effectively control the volume expansion and contraction of lithium secondary batteries during charging and discharging, improve the life characteristics and capacity maintenance of lithium secondary batteries, and enhance the mechanical strength and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069675A_ABST
    Figure CN119069675A_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery, the negative electrode active material for a non-aqueous electrolyte secondary battery according to an embodiment of the present invention comprising silicon, silicon oxide (SiOx, 0 < x < = 2), and magnesium silicate, the inside of the silicon oxide composite containing pores having a diameter of 50-300 nm, the negative electrode active material for a non-aqueous electrolyte secondary battery, comprising the silicon oxide composite, according to the present invention, has a function of buffering expansion during charging through internal pores, thereby solving the problem of swelling. According to the present invention, stress generated by expansion and contraction during charging and discharging is concentrated in internal pores to effectively control volume expansion, thereby improving life characteristics of a lithium secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of a patent application with an application date of December 3, 2018, an application number of 201880077812.2, and an invention name of “Negative electrode active material for non-aqueous electrolyte secondary batteries containing silicon oxide composites and preparation method thereof”. Technical Field

[0002] The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite and a preparation method thereof. Background Art

[0003] Lithium secondary batteries, which have recently attracted much attention as power sources for small portable electronic devices, are high-energy-density batteries that can release a discharge voltage more than twice that of existing alkaline aqueous solution batteries by using organic electrolytes.

[0004] As the positive electrode active material of lithium secondary batteries, LiCoO2, LiMn2O4, LiNi 1-x Co x Oxides composed of transition metals that can insert and remove lithium, such as O2 (0<x<1), can be used as negative electrode active materials. Various forms of carbon materials that can insert and remove lithium, including artificial graphite, natural graphite and hard carbon, can be used.

[0005] Although graphite is mainly used as a negative electrode material for lithium secondary batteries, it is difficult to achieve a high capacity of lithium secondary batteries because the average capacity per unit mass of graphite is small, only 372 mAh / g.

[0006] As new materials that can replace carbon-based negative electrode active materials, metal materials such as silicon (Si), tin (Sn), aluminum (Al), and antimony (Sb) are being studied. These metal materials can achieve charge / discharge through alloying / non-alloying reactions with lithium (Li), and can show higher capacity than graphite, which is a conventional negative electrode active material. However, metals such as silicon (Si), tin (Sn), aluminum (Al), and antimony (Sb) can cause large volume expansion and contraction during the alloying / non-alloying reaction with lithium (Li), so they have the following problems, that is, they may cause a decrease in life characteristics due to undifferentiation and loss of conductive paths. In particular, in terms of discharge capacity (4200mAh / g) and discharge voltage (0.4V), although silicon (Si) is the most suitable material as a high-capacity negative electrode material, the large volume expansion of about 400% caused by the insertion (charging) of lithium (Li) ions into the material can lead to the degradation (pulverization) of the active material, resulting in a sharp decrease in life characteristics.

[0007] The prior art patent is Patent Publication No. 10-2014-0042146 (published on April 7, 2014). Summary of the invention

[0008] In order to solve the above-mentioned problems of the prior art, an object of the present invention is to provide a negative electrode active material for a non-aqueous electrolyte secondary battery comprising a novel silicon oxide composite capable of preventing a rapid deterioration in life due to volume expansion and contraction of lithium.

[0009] Furthermore, another object of the present invention is to provide a method for preparing a negative electrode active material for a non-aqueous electrolyte secondary battery comprising a silicon oxide composite.

[0010] Furthermore, another object of the present invention is a non-aqueous electrolyte lithium secondary battery comprising a negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite.

[0011] The negative electrode active material for a non-aqueous electrolyte secondary battery according to an embodiment of the present invention comprises silicon, silicon oxide (SiO x , 0<x≤2) and magnesium silicate, containing a silicon oxide composite having pores with a diameter of 50nm to 300nm inside.

[0012] Figure 1 The surface of the silicon oxide composite of an embodiment of the present invention was photographed using a field emission scanning electron microscope (FE-SEM). Figure 1 The negative electrode active material for a non-aqueous electrolyte secondary battery of an embodiment of the present invention is a negative electrode active material comprising a silicon oxide composite, wherein the silicon oxide composite comprises silicon, silicon oxide (SiO x , 0<x≤2) and magnesium carbonate, containing a silicon oxide composite having pores with a diameter of 50nm to 300nm inside.

[0013] The pores inside the negative electrode active material for a non-aqueous electrolyte secondary battery including the silicon oxide composite of the present invention can be displayed by image processing.

[0014] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising a silicon oxide composite of the present invention, the pores disposed inside the silicon oxide composite can buffer the expansion during charging, thereby solving the swelling problem. The negative electrode active material for a non-aqueous electrolyte secondary battery comprising a silicon oxide composite of the present invention effectively controls volume expansion by concentrating the stress generated by expansion and contraction during charging and discharging in the internal pores, thereby improving the life characteristics of the lithium secondary battery.

[0015] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention, the pores may be closed pores disposed inside the silicon oxide composite, and a part of the pores may include open pores communicating with the outside.

[0016] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention, the pores may be closed pores disposed inside the silicon oxide composite.

[0017] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention, the average diameter of the pores may be 50 nm to 300 nm.

[0018] In the negative electrode active material for non-aqueous electrolyte secondary batteries containing silicon oxide composites of the present invention, when the average diameter of the pores is less than 50 nm, the pore size is too small to accommodate the volume expansion of silicon (Si) during the charging and discharging of the lithium secondary battery. When the average diameter of the pores is greater than 300 nm, a large number of residual pores are left after the volume expansion of silicon (Si), so the energy density can be reduced and the mechanical strength of the negative electrode active material including a large number of pores can be reduced. In addition, if the mechanical strength of the negative electrode active material is reduced, the negative electrode active material in the battery preparation process such as mixing of slurry, rolling after coating, etc. can be damaged.

[0019] The negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention allows lithium ions to penetrate into the interior of the silicon oxide composite by impregnating the non-aqueous electrolyte in the pores, thereby effectively diffusing lithium ions and improving the charging and discharging efficiency of the lithium secondary battery.

[0020] The area ratio of the pores may be 3 to 40% relative to the total cross-sectional area of ​​the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention.

[0021] When the area ratio of the above-mentioned pore part is less than 3%, the volume expansion of the negative electrode active material during charging and discharging of the lithium secondary battery cannot be suppressed. When it is greater than 40%, the large number of pores present inside the negative electrode active material can reduce the mechanical strength and damage the negative electrode active material during the preparation of the battery (mixing of slurry, calendering after coating, etc.).

[0022] In the negative electrode active material for non-aqueous electrolyte secondary batteries containing the silicon oxide composite of the present invention, the silicon can be crystalline or amorphous. In the case of amorphous silicon, the expansion and contraction during charging and discharging can be reduced, and the battery performance can be improved when used as a negative electrode active material for secondary batteries.

[0023] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention, the silicon oxide may be silicon dioxide.

[0024] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising a silicon oxide composite of the present invention, the silicon oxide (SiO x , 0<x≤2) can form Li-Si-O, Si+Li2O by irreversible reaction with lithium ions during discharge in an amorphous state. Therefore, the higher the content of silicon oxide, the lower the initial efficiency as the initial irreversible reaction increases. Preferably, in the negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention, 5 to 45 mole percent of the silicon oxide is contained relative to the total mole number of the silicon oxide composite.

[0025] In the case of using the negative electrode active material for a non-aqueous electrolyte secondary battery containing the above-mentioned silicon oxide composite of the present invention, when the content of the above-mentioned silicon oxide is less than 5 mol percent, the volume expansion and life characteristics can be reduced, and when it is greater than 45 mol percent, the life of the secondary battery can be reduced as the initial irreversible reaction increases.

[0026] When the negative electrode active material for non-aqueous electrolyte secondary batteries containing the above-mentioned silicon oxide composite of the present invention is subjected to X-ray diffraction analysis, the diffraction peak of silicon (III) may appear at 2θ=27.5°~29.5°, and the size of the silicon crystal calculated by the half-maximum full width of the above-mentioned diffraction peak may be 1nm~20nm.

[0027] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention, the ratio of the number of silicon atoms to the number of oxygen atoms (Si / O) in the silicon oxide may be 0.5 to 2.

[0028] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite of the present invention, since the silicon can be dispersed in the magnesium silicate, the expansion and contraction of silicon are further suppressed, thereby further improving the battery performance when used as a negative electrode active material for a secondary battery.

[0029] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention, the magnesium silicate may contain one or more of magnesium silicate (MgSiO3) or forsterite (Mg2SiO4). The magnesium silicate may contain magnesium silicate (MgSiO3) as a main component. In the negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention, the magnesium silicate may be a material having the general formula Mg x SiO yA compound represented by (0.5≤x≤2, 2.5≤y≤4).

[0030] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention, 2 to 40 weight percent of magnesium may be contained, relative to the total weight of the silicon oxide composite, preferably 4 to 30 weight percent, and more preferably 4 to 20 weight percent.

[0031] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising a silicon oxide composite of the present invention, when the magnesium content is less than 2 weight percent, the initial charge and discharge efficiency may be reduced, and when it is greater than 40 weight percent, the capacity retention rate and the processing stability may be reduced.

[0032] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising a silicon oxide composite of the present invention, since the magnesium silicate is difficult to react with lithium (Li) ions, when used as a negative electrode active material, the magnesium silicate can inhibit the initial irreversible reaction in a lithium secondary battery, and when the lithium (Li) ions increase dramatically, the life characteristics can be improved by reducing the expansion and contraction of the electrode.

[0033] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite of the present invention, the specific gravity of the silicon oxide composite may be 1.8 to 3.2, the average particle size may be 0.5 μm to 20 μm, and the specific surface area may be 1 m 2 / g~40m 2 / g. When the specific gravity of the silicon oxide composite is less than 1.8, the mechanical stability may be reduced, and when the specific gravity is greater than 3.2, the charge and discharge capacity when used as a negative electrode active material of a secondary battery may be reduced. When the average particle size of the silicon oxide composite is less than 0.5 μm, as the volume density decreases, the charge and discharge capacity per unit volume may be reduced. If it is prepared as a negative electrode active material, it is difficult to disperse the slurry, thereby generating a cohesive shape.

[0034] If the average particle size of the silicon oxide composite is greater than 20 μm, it is difficult to prepare an electrode film, and the negative electrode active material containing the silicon oxide composite may be peeled off from the collector. Since the negative electrode active material is difficult to react evenly with lithium, the life of the secondary battery may be reduced.

[0035] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite of the present invention, magnesium may be contained in an amount of 2 to 40 weight percent relative to the total weight of the silicon oxide composite.

[0036] In the negative electrode active material for a non-aqueous electrolyte secondary battery including the silicon oxide composite of the present invention, 25 to 40 weight percent of oxygen may be included relative to the total weight of the silicon oxide composite.

[0037] Furthermore, the negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention may also contain a coating layer containing carbon on the surface. In the negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention, the coating layer may be in a ratio of 2 weight percent to 20 weight percent relative to the total weight of the silicon oxide composite, and more preferably, may be 2 weight percent to 10 weight percent. If the content of the coating layer containing carbon is less than 2 weight percent, it is difficult to expect to obtain the effect of fully improving the conductivity and reducing the electrode life of the lithium secondary battery. If it is greater than 20 weight percent, the discharge capacity may be reduced and the charge and discharge capacity per unit volume may be reduced.

[0038] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising a silicon oxide composite according to the present invention, the coating layer comprising carbon may comprise at least one selected from the group consisting of amorphous carbon, carbon nanofibers, graphene, and graphene oxide.

[0039] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention, the coating layer can provide excellent conductivity between particles of the silicon oxide composite, so the performance of the lithium secondary battery can be further improved. In the negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention, the coating layer containing the carbon can improve the performance of the lithium secondary battery by inhibiting side reactions with the electrolyte.

[0040] In the negative electrode active material for non-aqueous electrolyte secondary batteries comprising the silicon oxide composite of the present invention, the average thickness of the carbon-containing coating layer disposed on the surface of the silicon oxide composite may be 1 nm to 5 μm, preferably 5 nm to 2 μm, and more preferably 10 nm to 1 μm.

[0041] If the average thickness of the coating layer is 1 nm or more, the conductivity can be improved. If the thickness is 5 μm or less, when used as a negative electrode active material of a lithium ion battery, the reduction in battery capacity can be suppressed. If the average thickness of the coating layer is less than 1 nm, the effect of increasing the conductivity through the carbon film becomes negligible. When applied to a negative electrode active material, the initial efficiency can be reduced due to the high reactivity with the electrolyte. When the average thickness of the coating layer is greater than 5 μm, the mobility of lithium ions is disturbed, which may cause a problem of increased resistance.

[0042] When the negative electrode active material of the secondary battery containing the non-aqueous electrolyte of the silicon oxide composite of the present invention contains a carbon coating layer, the specific gravity of the silicon oxide composite can be 1.8 to 3.2, the average particle size can be 0.5 μm to 20 μm, and the specific surface area can be 1 m 2 / g~40m 2 / g.

[0043] The silicon oxide composite including the coating layer of the present invention may contain 1.5 to 30 weight percent of magnesium relative to the total weight of the silicon oxide composite.

[0044] The silicon oxide composite including the coating layer of the present invention may contain 15 to 33 weight percent of oxygen relative to the total weight of the composite.

[0045] The non-aqueous electrolyte lithium secondary battery according to the embodiment of the present invention includes the negative electrode active material for a non-aqueous electrolyte secondary battery.

[0046] The preparation method of the non-aqueous electrolyte lithium secondary battery of an embodiment of the present invention may include: a first step, placing a mixture of silicon particles with an average particle size of 0.1μm to 20μm and silicon dioxide particles with an average particle size of 10nm to 100nm and magnesium into a reactor; a second step, adjusting the pressure of the above-mentioned reactor to 0.001torr to 1torr; a third step, preparing a silicon oxide composite by heating the above-mentioned mixture and the above-mentioned magnesium to 600℃ to 1600℃; a fourth step, cooling the above-mentioned silicon oxide composite and vapor-depositing it on a metal plate; and a fifth step, crushing the above-mentioned silicon oxide composite that has been cooled and vapor-deposited on the metal plate into an average particle size of 0.5μm to 15μm.

[0047] In the preparation method of the non-aqueous electrolyte lithium secondary battery of the embodiment of the present invention, if the above-mentioned evaporation temperature is above 1200°C, the silicon oxide composite particles in the vapor state are densely evaporated on the metal plate, so that almost no pores are generated inside the ions. If the evaporation temperature is below 500°C, the silicon oxide composite particles in the vapor state cannot be evaporated on the metal plate. In addition, when the evaporation temperature is in the range of 700°C to 1000°C, the silicon oxide composite particles in the vapor state can easily form pores on the metal plate. The evaporated block can be crushed and classified using a coarse crusher and a jet mill to adjust the particle size, thereby preparing a silicon oxide composite powder with nanopores.

[0048] The preparation method of the non-aqueous electrolyte lithium secondary battery of the embodiment of the present invention may also include a sixth step, mixing the silicon oxide composite of the above-mentioned fifth step and one or more carbon sources selected from the group consisting of methane, propane, butane, acetylene, benzene and toluene, and forming a coating layer containing carbon on the surface of the silicon oxide composite by heat treatment at a temperature of 600°C to 1200°C.

[0049] The carbon-containing coating layer configured on the above-mentioned silicon oxide composite can be formed by mixing a carbon source including one or a combination of carbon dioxide, argon, methane, ethane, propane, butane, water vapor or hydrogen, hydrogen, acetylene, benzene and toluene, and reacting at a temperature of 600°C to 1200°C.

[0050] The carbon source gas may be methane, a mixed gas containing methane and an inert gas, or a mixed gas containing methane and an oxygen-containing gas.

[0051] In addition to the carbon source gas, the gas mixture may further include a plurality of inert gases selected from the group consisting of nitrogen, helium, and argon.

[0052] In one embodiment, the carbon source gas is a methane (CH4) : carbon dioxide (CO2) mixed gas, and the molar ratio of the methane (CH4) : carbon dioxide (CO2) mixed gas can be about 1:0.20-0.50, preferably, about 1:0.25-0.45, and more preferably, about 1:0.30-0.40.

[0053] In one embodiment, the carbon source may be a mixed gas of methane (CH4): carbon dioxide (CO2): water vapor (H2O). The molar ratio of the mixed gas of methane (CH4): carbon dioxide (CO2): water vapor (H2O) may be about 1: 0.20-0.50: 0.01-1.45, preferably, 1: 0.25-0.45: 0.10-1.35, and more preferably, about 1: 0.30-0.40: 0.50-1.0.

[0054] In one embodiment, the carbon source may be carbon monoxide (CO) or carbon dioxide (CO2).

[0055] In one embodiment, the carbon source may be a mixed gas of methane (CH4) and nitrogen (N2).

[0056] The molar ratio of the mixed gas of methane (CH4) and nitrogen (N2) can be about 1:0.20-0.50, preferably, about 1:0.25-0.45, and more preferably, about 1:0.30-0.40.

[0057] When the gas mixture contains water vapor, the silicon oxide composite with the coating layer on the surface can exhibit high conductivity through the coating layer. The water vapor content in the gas mixture is not limited. Preferably, the water vapor content can be 0.01 to 10 volume percent based on 100 volume percent of the total carbon source gas.

[0058] The non-aqueous electrolyte lithium secondary battery according to the embodiment of the present invention includes the negative electrode active material for a non-aqueous electrolyte secondary battery.

[0059] A non-aqueous electrolyte secondary battery using a silicon oxide composite material in a negative electrode can have excellent capacity retention and initial efficiency.

[0060] The silicon oxide composite may include a negative electrode active material, a positive electrode active material, a binder and a conductive material for a non-aqueous electrolyte secondary battery. The negative electrode active material may absorb and release lithium ions.

[0061] The negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite of the present invention contains a silicon oxide composite, and by containing pores with a diameter of 50 nm to 300 nm inside, the secondary battery containing the negative electrode active material of the present invention is prevented from rapidly deteriorating in life due to the volume expansion and contraction of silicon (Si), thereby showing an effect of improving capacity characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is a picture of the surface of the silicon oxide composite of Example 1 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 30,000.

[0063] Figure 2 This is a picture of the surface of the silicon oxide composite of Example 1 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 100,000.

[0064] Figure 3 This is a picture of the surface of the silicon oxide composite of Example 2 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 20,000.

[0065] Figure 4 This is a picture of the surface of the silicon oxide composite of Example 2 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 100,000.

[0066] Figure 5 This is a picture of the surface of the silicon oxide composite of Example 3 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 20,000.

[0067] Figure 6 This is a picture of the surface of the silicon oxide composite of Example 3 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 100,000.

[0068] Figure 7 This is a picture of the surface of the silicon oxide composite of Comparative Example 1 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 30,000.

[0069] Figure 8 This is a picture of the surface of the silicon oxide composite of Comparative Example 1 taken with a field emission scanning electron microscope (FE-SEM) at a magnification of 100,000. DETAILED DESCRIPTION

[0070] Hereinafter, the present invention will be described in further detail by way of examples, but the present invention is not limited to the following examples.

[0071] Example 1. Preparation of a silicon oxide composite containing magnesium

[0072] 15 kg of a powder of silicon powder and silicon dioxide (SiO2) powder uniformly mixed in a molar ratio of 1:1 and 1.5 kg of magnesium were heat-treated at 1400° C. in a reduced pressure atmosphere of 0.01 to 1 torr, so that silicon oxide vapor and magnesium vapor of the mixed powder of silicon and silicon dioxide (SiO2) were simultaneously generated and reacted in the gas phase, and then cooled at 700° C. and precipitated, and then pulverized and classified by a jet mill, thereby obtaining a granular material having an average particle size (D 50 ) is a magnesium-silicon oxide composite powder of 6.3 μm.

[0073] In order to form a coating layer containing carbon, a recovered silicon oxide composite powder containing magnesium was placed in a mixed gas of argon (Ar) and methane (CH4) at a temperature of 1000°C using a tubular electric furnace and treated by chemical vapor deposition (CVD) for 2 hours to prepare a silicon oxide composite (sample 1) containing 9 weight percent of magnesium in a carbon coating layer having a carbon content of 5 weight percent.

[0074] It was confirmed from the silicon oxide composite (Sample 1) containing magnesium that the BET specific surface area was 5.5 m 2 / g, specific gravity is 2.3g / cm 3 , average particle size (D 50 ) was 6.3 μm, and the size of the silicon crystal measured by X-ray diffraction analysis (CuKα) was 8 nm.

[0075] Example 2. Preparation of a silicon oxide composite containing magnesium

[0076] A silicon oxide composite containing 9 weight percent of magnesium (Sample 2) was prepared by the same method as in Example 1 except that precipitation was performed after cooling at 800° C., and a silicon oxide composite powder forming a carbon coating layer having a carbon content of 5 weight percent was prepared.

[0077] It was confirmed from the silicon oxide composite (Sample 2) containing magnesium that the BET specific surface area was 6.2 m 2 / g, specific gravity is 2.3g / cm 3 , average particle size (D50 ) was 6.5 μm, and the size of the silicon crystals measured by X-ray diffraction analysis (CuKα) was 8 nm.

[0078] Example 3. Preparation of silicon oxide composite containing magnesium

[0079] A silicon oxide composite containing 4 weight percent of magnesium (Sample 3) was prepared by the same method as in Example 1 except that precipitation was performed after cooling at 900° C., and a silicon oxide composite powder forming a carbon coating layer having a carbon content of 10 weight percent was prepared.

[0080] It was confirmed from the silicon oxide composite (Sample 3) containing magnesium that the BET specific surface area was 6.3 m 2 / g, specific gravity is 2.4g / cm 3 , average particle size (D 50 ) was 6.2 μm, and the size of the silicon crystal measured by X-ray diffraction analysis (CuKα) was 11 nm.

[0081] Example 4. Preparation of a silicon oxide composite containing magnesium

[0082] A silicon oxide composite containing 12 weight percent of magnesium (Sample 4) was prepared by the same method as in Example 1 except that precipitation was performed after cooling at 1000° C., and a silicon oxide composite powder forming a carbon coating layer having a carbon content of 7 weight percent was prepared.

[0083] It was confirmed from the silicon oxide composite (Sample 4) containing magnesium that the BET specific surface area was 5.8 m 2 / g, specific gravity is 2.3g / cm 3 , average particle size (D 50 ) was 6.8 μm, and the size of the silicon crystals measured by X-ray diffraction analysis (CuKα) was 13 nm.

[0084] Example 5. Preparation of a silicon oxide composite containing magnesium

[0085] A silicon oxide composite containing 16 weight percent of magnesium (Sample 5) was prepared by the same method as in Example 1 except that precipitation was performed after cooling at 1100° C., and a silicon oxide composite powder forming a carbon coating layer having a carbon content of 4 weight percent was prepared.

[0086] It was confirmed from the silicon oxide composite (Sample 5) containing magnesium that the BET specific surface area was 6.7 m 2 / g, specific gravity is 2.4g / cm 3 , average particle size (D 50) was 6.7 μm, and the size of the silicon crystals measured by X-ray diffraction analysis (CuKα) was 14 nm.

[0087] Example 6. Preparation of a silicon oxide composite containing magnesium

[0088] A silicon oxide composite containing 15 weight percent of magnesium (Sample 6) was prepared by the same method as in Example 1 except that precipitation was performed after cooling at 800° C., and a silicon oxide composite powder forming a carbon coating layer having a carbon content of 5 weight percent was prepared.

[0089] It was confirmed from the silicon oxide composite (Sample 6) containing magnesium that the BET specific surface area was 5.2 m 2 / g, specific gravity is 2.3g / cm 3 , average particle size (D 50 ) was 6.6 μm, and the size of the silicon crystals measured by X-ray diffraction analysis (CuKα) was 14 nm.

[0090] Example 7. Preparation of a silicon oxide composite containing magnesium

[0091] A silicon oxide composite containing 15 weight percent of magnesium in a carbon coating layer having a carbon content of 15 weight percent was prepared by the same method as in Example 1 except that precipitation was performed after rapid cooling (Sample 7).

[0092] It was confirmed from the silicon oxide composite (Sample 7) containing magnesium that the BET specific surface area was 7.2 m 2 / g, specific gravity is 2.0g / cm 3 , average particle size (D 50 ) was 6.5 μm, and the size of the silicon crystals measured by X-ray diffraction analysis (CuKα) was 12 nm.

[0093] Comparative Example 1. Preparation of a silicon oxide composite containing magnesium

[0094] A silicon oxide composite (Sample 8) containing 1 weight percent of magnesium in a carbon coating layer having a carbon content of 5 weight percent was prepared by the same method as in Example 1 except that precipitation was performed after natural cooling.

[0095] It was confirmed from the silicon oxide composite (Sample 8) containing magnesium that the BET specific surface area was 5 m 2 / g, specific gravity is 2.2g / cm 3 , average particle size (D 50 ) was 6.5 μm, and the size of the silicon crystals measured by X-ray diffraction analysis (CuKα) was 8 nm.

[0096] Comparative Example 2. Preparation of a silicon oxide composite not containing magnesium

[0097] A silicon oxide composite (Sample 9) formed with a carbon coating layer having a carbon content of 5 weight percent was prepared by the same method as in Example 1 except that magnesium was not added for the heat treatment.

[0098] It was confirmed from the silicon oxide composite (Sample 9) that the BET specific surface area was 6.5 m 2 / g, specific gravity is 2.0g / cm 3 , average particle size (D 50 ) was 6.0 μm, and the size of the silicon crystal measured by X-ray diffraction analysis (CuKα) was 5 nm.

[0099] Experimental Example 1

[0100] The size of the pores of the silicon oxide composites prepared in Examples 1 to 6 and Comparative Examples 1 and 2, the area ratio of the pores (the area ratio of the pores to the total area in the image-processed cross section), the D 50 , the specific gravity and specific surface area of ​​the silicon composite, the size of the silicon (Si) crystal, the initial efficiency of the discharge capacity, and the capacity maintenance rate are shown in Table 1.

[0101] As can be seen from Table 1 below, when magnesium was not included (Comparative Example 2) or when prepared by natural cooling (Comparative Example 1), even if magnesium was included, pores were not generated inside the particles.

[0102] Table 1

[0103] Comparison of the silicon oxide composites prepared by Examples 1 to 6 and Comparative Examples 1 and 2

[0104]

[0105] Preparation Example

[0106] A negative electrode for a lithium secondary battery and a battery (button battery) including the silicon oxide composite powder prepared by the above-described Examples and Comparative Examples as an electrode active material were manufactured.

[0107] The active material, conductive carbon black (SUPER-P) as a conductive material, polyacrylic acid, and water were mixed in a weight ratio of 80:10:10 to prepare a negative electrode slurry.

[0108] An electrode with a thickness of 70 μm was prepared by coating the above composition with a copper foil with a thickness of 18 μm and drying it. The copper foil coated with the above electrode was punched into a circle with a diameter of 14 mm to prepare a negative electrode for a button battery. A metal lithium foil with a thickness of 0.3 mm was used for the opposite electrode.

[0109] As a separation membrane, a porous polyethylene sheet with a thickness of 0.1 mm was used, and as an electrolyte, lithium hexafluorophosphate (LiPF6) with a concentration of 1 M was dissolved in a solution of ethylene carbonate (EC) and diethylene carbonate (DEC) mixed in a volume ratio of 1:1. By using multiple of the above-mentioned structural elements, a button cell (battery) with a thickness of 2 mm and a diameter of 32 mm (so-called 2032 type) was manufactured.

[0110] Experimental example

[0111] The button cell prepared in the above preparation example was charged at a constant current of 0.1C until the voltage almost reached 0.005V, and discharged at a constant current of 0.1C until the voltage reached 2.0V, thereby calculating the charge capacity (mAh / g), discharge capacity (mAh / g) and initial charge / discharge efficiency (%). The results are shown in Table 1 above.

[0112] Furthermore, the button battery manufactured using each sample in the above preparation example was charged and discharged once, and then charged at a constant current of 0.5C from the second charge and discharge until the voltage reached 0.005V, and discharged at a constant current of 0.5C until the voltage reached 2.0V, thereby calculating the cycle characteristics (50 times capacity retention rate), and the results are shown in the above Table 1.

[0113] It can be confirmed from Table 1 that when pores are generated inside the particles, the 50-cycle capacity retention rate is greatly improved.

Claims

1. A negative electrode active material for a non-aqueous electrolyte secondary battery, characterized in that: The invention comprises silicon, silicon oxide and magnesium silicate, and contains a silicon oxide composite having pores with a diameter of 50nm to 300nm inside, wherein the chemical formula of the silicon oxide is SiO x , 0<x≤2.

2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: The silicon oxide composite contains 2 to 40 weight percent of magnesium relative to the total weight of the silicon oxide composite.

3. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: The partial area ratio of the pores is 3% to 40% with respect to the total area of ​​the cross section of the silicon oxide composite.

4. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: When the silicon oxide composite is subjected to X-ray diffraction analysis, the diffraction peak of silicon (III) appears at 2θ=27.5° to 29.5°, and the size of the silicon crystal calculated from the full width at half maximum of the diffraction peak is 1 nm to 20 nm.

5. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: The ratio of the number of silicon atoms to the number of oxygen atoms in the above silicon oxide is 0.5 to 2.

6. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: The magnesium silicate mentioned above includes magnesium silicate or forsterite.

7. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: The silicon oxide composite has a specific gravity of 1.8 to 3.2, an average particle size of 0.5 μm to 20 μm, and a specific surface area of ​​1 m 2 / g~40m 2 / g.

8. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: The silicon oxide composite contains 25 to 40 weight percent of oxygen relative to the total weight of the silicon oxide composite.

9. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: The silicon oxide composite further includes a coating layer containing carbon on the surface, and the coating layer is included in an amount of 2 to 20 weight percent relative to the total weight of the silicon oxide composite.

10. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 9, characterized in that: The coating layer containing carbon includes one or more selected from the group consisting of amorphous carbon, carbon nanofibers, graphene, and graphene oxide.

11. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 9, characterized in that: The silicon oxide composite has a specific gravity of 1.8 to 3.2, an average particle size of 0.5 μm to 20 μm, and a specific surface area of ​​1 m 2 / g~40m 2 / g.

12. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 9, characterized in that: The silicon oxide composite contains 1.5 to 30 weight percent of magnesium relative to the total weight of the silicon oxide composite.

13. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 9, characterized in that: The silicon oxide composite includes 15 weight percent to 33 weight percent of oxygen relative to the total weight of the silicon oxide composite.

14. A negative electrode, characterized in that: A negative electrode active material for a non-aqueous electrolyte secondary battery comprising the negative electrode active material according to any one of claims 1 to 13.

15. A non-aqueous electrolyte lithium secondary battery, characterized in that: The negative electrode according to claim 14 is included.

16. A method for preparing a negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, characterized in that: include: In the first step, a mixture of silicon particles with an average particle size of 0.1 μm to 20 μm and silicon dioxide particles with an average particle size of 10 nm to 100 nm and magnesium with an average particle size of 1 mm to 100 mm are placed in a reactor; The second step is to adjust the pressure of the reactor to 0.001 torr to 1 torr; The third step is to prepare a silicon oxide composite by heating the mixture and the magnesium metal particles to 600° C. to 1600° C.; The fourth step is to cool the silicon oxide composite and evaporate it on the metal plate; and In the fifth step, the silicon oxide composite that has been cooled and deposited on the metal plate is crushed into particles with an average particle size of 0.5 μm to 15 μm and then classified.

17. The method for preparing a negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 16, characterized in that: The method further comprises a sixth step of mixing the silicon oxide composite obtained in the fifth step with a carbon source and performing a heat treatment at a temperature of 600° C. to 1200° C. to form a coating layer containing carbon on the surface of the silicon oxide composite.

18. The method for preparing a negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 17, characterized in that: The carbon source is at least one selected from the group consisting of methane, propane, butane, acetylene, benzene and toluene.

19. The method for preparing a negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 18, characterized in that: The mixture of the silicon oxide composite and the carbon source further comprises at least one selected from the group consisting of nitrogen, helium, argon, carbon dioxide gas, and water vapor.

20. A negative electrode, characterized in that: A negative electrode active material for a non-aqueous electrolyte secondary battery comprising any one of claims 16 to 19.

21. A non-aqueous electrolyte lithium secondary battery, characterized in that: Comprising the negative electrode according to claim 20.