Polyethyleneimine modified chitosan microspheres, preparation method and application

Polyethyleneimine modified chitosan microspheres prepared through droplet microfluidic control technology solve the problems of low efficiency and high cost of existing adsorbents, achieve efficient removal of heavy metal ions, and reduce production costs and Energy consumption.

CN119075945APending Publication Date: 2024-12-06CHIFENG UNIVERSITY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411379967.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing adsorbents have problems such as low adsorption amount, low efficiency, low selectivity and inability to reuse in heavy metal ion pollution treatment, and the preparation process is complex and costly, which limits their large-scale application and environmentally friendly implementation.

Method used

Polyethyleneimine-modified chitosan microspheres were prepared by reverse phase microemulsion method controlled by droplet microfluidic control technology. The density of amino functional groups was improved through functional functional groups surface modification technology, and efficient adsorption of heavy metal ions was achieved through simplified The process reduces production costs.

Benefits of technology

It achieves efficient removal of heavy metal ions in water, improves the reusability and stability of adsorbents, reduces usage and energy consumption, and avoids secondary pollution, meeting the needs of large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075945A_ABST
    Figure CN119075945A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of functional material preparation, and particularly relates to a polyethyleneimine modified chitosan microsphere, a preparation method and application, and the polyethyleneimine modified chitosan microsphere is prepared by adopting a reversed-phase microemulsion method controlled by a droplet microfluidic technology. The polyethyleneimine modified chitosan microsphere particles are smooth in surface, the particle size is 200-450 m, when the polyethyleneimine modified chitosan microsphere particles are applied to adsorption of heavy metal ions Cd (II), Pb (II) and Cu (II) in water, the polyethyleneimine modified chitosan microsphere particles are comprehensively superior to traditional adsorbents in the aspects of adsorption capacity, removal rate, adsorption equilibrium time, adsorbent dosage and the like, the adsorption capacity to Cd (II) is smaller than or equal to 88.62 mg / g, the adsorption capacity to Pb (II) is smaller than or equal to 156.6 mg / g, and the adsorption capacity to Cu (II) is smaller than or equal to 141.8 mg / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional material preparation, and specifically relates to polyethyleneimine-modified chitosan microspheres, a preparation method and an application thereof. Background Art

[0002] Faced with the current situation of heavy metal ion pollution with wide sources, great harm and strict national policy requirements, it is urgent to find a method that can quickly and effectively control heavy metal ion pollution, and it has become a hot topic in current research. Common heavy metal ion removal methods include chemical precipitation, membrane separation, ion exchange, biological method, adsorption method, etc. However, due to the existence of inherent defects such as low treatment efficiency, the need for other expensive reagents, incomplete removal of pollutants, high energy consumption, and the production of unexpected toxic byproducts, the application of heavy metal ion wastewater treatment has been greatly limited. The adsorption method is considered to be the most promising water purification and remediation method because of its advantages of simple operation, high treatment efficiency, wide application range, economic feasibility, and no secondary pollution. The adsorption method utilizes the selective adsorption properties of adsorbents for heavy metal ions to enrich heavy metal ions on its surface. Its adsorption mechanism mainly includes chemical and physical processes such as electrostatic action, ion exchange, metal chelation, complexation, and hydrolysis precipitation. The core of the adsorption method is the adsorbent. Various adsorbents for treating heavy metal pollutants have been developed, such as activated carbon, minerals, biomass and composite materials. However, in sewage treatment, traditional adsorbent materials have the disadvantages of low adsorption capacity, low adsorption efficiency, low adsorption selectivity and inability to be reused, which restricts the application of these adsorbents and cannot meet the needs of today's social development.

[0003] Chitosan microspheres (CS) as an adsorbent have unique advantages in adsorbing heavy metal ions in water. For example, chitosan is a natural polymer compound with biocompatibility and biodegradability, which means that the use of chitosan microspheres as an adsorbent has less impact on the environment; chitosan microspheres contain active groups such as hydroxyl and amino groups, which can interact with heavy metal ions in water through a variety of mechanisms (such as electrostatic adsorption, ion exchange, complexation, etc.), thereby achieving efficient adsorption; chitosan microspheres can be chemically or physically modified to introduce more active groups or functional side chains to improve their adsorption of specific pollutants. Adhesion performance and selectivity; magnetic chitosan microspheres can be prepared by combining chitosan microspheres with magnetic nanoparticles. This composite material is easy to recycle and reuse under the action of a magnetic field, which improves the economy and ease of operation of the adsorbent; chitosan microspheres can also exist stably under certain acidic conditions, which enables them to maintain good adsorption effects under variable water conditions; chitosan comes from a wide range of natural resources, such as the shells of crustaceans, and has a low cost, which is conducive to large-scale applications; in addition, some studies have shown that chitosan microspheres after specific modification have shown a higher adsorption capacity for dyes and heavy metal ions in water.

[0004] The prior art mainly adopts the reverse emulsion polymerization method for preparing chitosan microspheres, wherein chitosan powder is fully dissolved in an acidic aqueous solution as a dispersed phase, and a water-immiscible organic solvent to which a surfactant and an initiator (cross-linking agent) are added is used as a continuous phase. The dispersed phase and the continuous phase form a water-in-oil (W / O) microemulsion under conditions of sufficient mixing and continuous stirring, and then the cross-linking reaction of chitosan is initiated by the action of an oil-soluble initiator and a surfactant to form chitosan microspheres. This process is accompanied by initiator-induced dispersed phase cross-linking polymerization. Therefore, the chitosan microspheres prepared by this method have poor particle size uniformity, a small average particle size, and are prone to adhesion to each other.

[0005] CN111871209A discloses a method for preparing a heat-resistant polytetrafluoroethylene composite nanofiltration membrane, which solves the technical problems that the polytetrafluoroethylene microporous membrane shrinks when heated and destroys the separation functional layer, resulting in a decrease in its mechanical strength and retention performance, as well as the clogging of the pores on the membrane surface and a serious decrease in water flux caused by the filling of nano-titanium dioxide colloidal particles in the nanofiltration membrane preparation. However, there are still problems such as the large number of chemical reagents and reaction conditions in the preparation process, the impact on the environment, the high production cost that needs to be optimized, the polytetrafluoroethylene microporous membrane may still shrink during heat treatment, affecting the membrane performance, and the heat resistance and dimensional stability that need to be improved.

[0006] CN105413661A discloses a one-step synthesis method of polyethyleneimine-chitosan adsorbent, which solves the problems of complex wastewater components, small single treatment volume, long cycle, poor effect, high cost and secondary pollution in wastewater treatment in the energy and chemical industry. The method has the advantages of simple and reliable preparation, stable and effective adsorption performance, and can treat a variety of complex wastewater systems; however, there are still problems such as the preparation process involves multiple chemical reagents, precise control of conditions, complex operation, high cost, adsorption performance is affected by multiple factors, efficiency needs to be optimized and improved, and post-adsorption waste treatment and adsorbent regeneration need to be solved.

[0007] Li et al. introduced a microfluidic preparation of lanthanum hydroxide cross-linked chitosan microspheres (CIESC Journal, 2022, 73(9):3929-3939). The microspheres have a loose porous structure, which improves the utilization rate, mechanical strength and recyclability of lanthanum, has good adsorption performance for phosphate and is renewable, and improves the economy and practicality of the adsorbent; however, the following problems still exist: the complexity and precision of microfluidic technology leads to high preparation costs, which limits large-scale production; lanthanum resources are limited, and the large-scale use of lanthanum-based materials may aggravate resource consumption; lanthanum accumulation after repeated use may affect the environment; and there is no mention of performance changes caused by long-term use, which requires further research and verification; the industrial production of microfluidic technology needs to solve problems such as particle size consistency and efficiency improvement; material recovery and final treatment need to consider the complexity of lanthanum recovery to ensure environmental friendliness.

[0008] In summary, preparing a new adsorbent that is low-cost, simple to operate, reusable and environmentally friendly is an urgent problem to be solved. Summary of the invention

[0009] In order to solve the above problems, the present invention provides a polyethyleneimine-modified chitosan microsphere (PEI-CS), wherein the polyethyleneimine-modified chitosan microsphere is prepared by a reverse microemulsion method controlled by droplet microfluidics technology, the polyethyleneimine-modified chitosan microsphere particle surface is smooth, the particle size is 200-450µm, the adsorption capacity for Cd(II) is ≤88.62mg / g, the adsorption capacity for Pb(II) is ≤156.6mg / g, and the adsorption capacity for Cu(II) is ≤141.8mg / g; The chitosan microspheres modified with polyethyleneimine have a -1 、1640cm -1 、1080cm -1 There are absorption peaks at , corresponding to the stretching oscillation of −CH and −NH 2 The bending oscillation of C−OH and the stretching oscillation of C−OH; in the XRD characterization, the broad peak appearing in the 2θ range of 10°-25° is the amorphous characteristic peak of chitosan microspheres modified by polyethyleneimine.

[0010] The present invention also provides a method for preparing the polyethyleneimine-modified chitosan microspheres, the method comprising the following steps: Step 1: Prepare the solution Preparation of dispersed phase: add acetic acid solution to a three-necked flask, add chitosan powder to the three-necked flask, heat and stir for 30-120 min, the temperature is 40-80° C., the speed is 200-300 r / min, the chitosan is completely dissolved to obtain a chitosan solution, the chitosan solution is filtered and vacuum degassed 3-5 times, the filter mesh pore size is 80 μm, the vacuum degree is 0.06-0.6 MPa, and a clear and transparent light yellow chitosan solution is obtained, which is used as a dispersed phase, i.e., an aqueous phase; Preparation of continuous phase: Add Span 80 to the n-octanol solution and stir evenly. The obtained mixed solution is used as the continuous phase, i.e., the oil phase; Preparation of cross-linking curing liquid: Mix the glutaraldehyde solution and the n-octanol solution, stir evenly, and use the mixture as the cross-linking curing liquid.

[0011] Step 2: Preparation of chitosan microdroplets The aqueous phase described in step 1 is loaded into a syringe equipped with a flat needle, and enters the microfluidic chip pipeline through an aqueous phase microinjection pump at a flow rate of 2-10 mL / h. The oil phase is loaded into a syringe equipped with a flat needle, and enters the microfluidic chip pipeline through an oil phase microinjection pump at a flow rate of 20-100 mL / h. The aqueous phase and the oil phase form oil-in-water emulsion droplets at the intersection of the pipeline to obtain chitosan microdroplets, and the chitosan microdroplets are transported to the outlet of the microfluidic chip along the transport channel; Step 3: Chemical cross-linking Collect the chitosan microdroplets in step 2 into the cross-linked curing liquid in step 1, stir while collecting, at 60-80° C., the collection time is 10-20 min, and after stopping the collection, keep the temperature unchanged and continue stirring for 40-80 min at a speed of 100-200 r / min to obtain chemically cross-linked chitosan microspheres; Step 4: Wash and Dry The chemically cross-linked chitosan microspheres in step 3 are first washed with an acetone solution, then washed with an ethanol solution, and then washed with an excess of deionized water, and then transferred to a constant temperature box and dried at 30-50° C. for 1-10 hours to obtain dry chemically cross-linked chitosan microspheres; Step 5: Polyethyleneimine modified chitosan microspheres The dried chemically cross-linked chitosan microspheres described in step 4 are added to a three-necked flask, protected by inert gas, and acetone is added and stirred for 12-24 hours at a temperature of 20-40°C and a rotation speed of 100-300r / min. Subsequently, acryloyl chloride (bridging agent) is added to the three-necked flask and stirred for 10-20 hours at a temperature of 30-60°C and a rotation speed of 100-300r / min. Then, the mixture is filtered with a sand core funnel. The solid product is first washed with acetone for 3-5 times and then with methanol for 3-5 times. The washed product is transferred to a three-necked flask, and methanol and polyethyleneimine are added and stirred for 12-36 hours at a temperature of 30-60°C and a rotation speed of 100-200r / min. After the reaction is completed, the mixture is filtered, washed with methanol for 3-5 times, and dried in a vacuum drying oven at 40-60°C for 10-20 hours to obtain the polyethyleneimine-modified chitosan microspheres.

[0012] Furthermore, in step 2, the diameter of the planar needle is Φ=200-800 μm, and the volume of the syringe is 5-100 mL.

[0013] Furthermore, in step 2, the particle size of the chitosan microdroplets can be controlled to be 100-500 μm according to the needle size.

[0014] Further, in step 5, the inert gas is N 2 , any one of Ar.

[0015] The present invention also provides a method for adsorbing heavy metal ions in water using the surface amino-functionalized chitosan microspheres described in claim 1, wherein the chitosan microspheres modified with polyethyleneimine are placed in a solution containing heavy metal ions, the pH is adjusted to 2-7, the solution is placed in a constant temperature oscillator for oscillation reaction, the constant temperature is 10-40°C, the oscillation frequency is 100-200r / min, the reaction time is 5-180min, and after the reaction is completed, the upper layer solution is taken and the concentration of the heavy metal ions is determined by an atomic absorption spectrophotometer.

[0016] Furthermore, the heavy metal ions are one or more of Cd(II), Pb(II), and Cu(II).

[0017] Furthermore, at 25°C and pH=5, the adsorption capacity of the surface amino-functionalized chitosan microspheres for Cd(II) is ≤88.62 mg / g, the adsorption equilibrium time is 80 min, and the Cd(II) removal rate can reach 84.84%; at 25°C and pH=5, the adsorption capacity for Pb(II) is ≤156.6 mg / g, the adsorption equilibrium time is 90 min, and the Pb(II) removal rate can reach 91.82%; at 25°C and pH=5, the adsorption capacity for Cu(II) is ≤141.8 mg / g, the adsorption equilibrium time is 60 min, and the Cu(II) removal rate can reach 88.2%.

[0018] Furthermore, the pH value of the solution is adjusted with 1 mol / L HCl or 1 mol / L NaOH.

[0019] The beneficial effects of the present invention are as follows: (1) The present invention adopts a reverse microemulsion method controlled by droplet microfluidics technology to prepare polyethyleneimine-modified chitosan microspheres. With the help of microfluidics preparation technology, the size of microdroplets can be controlled very accurately. The prepared chitosan microspheres have highly uniform particle sizes. Whether observed at the microscale or macroscale, the sizes of these microspheres show amazing consistency. This technology also gives the preparation process a high degree of controllability of the particle size. The particle size of the microspheres can be flexibly adjusted according to different application requirements, thereby meeting the use requirements in various specific scenarios. This precise particle size control is not only conducive to improving the quality stability of the product, but also provides more possibilities for subsequent applications. (2) Through the functional group surface modification technology, the distribution density and number of amino functional groups on the surface of chitosan microspheres are greatly improved. Amino functional groups play a vital role in the adsorption process. They can strongly interact with heavy metal ions, thereby achieving efficient adsorption and more effectively removing heavy metal ions from water. At the same time, this surface modification technology can also enhance the stability and durability of the microspheres, so that they maintain good adsorption performance during long-term use, reducing the cost and workload of frequent replacement of adsorbents; this means that in practical applications, relatively fewer microspheres can be used to achieve the same adsorption effect, thereby reducing the amount and cost of adsorbents. At the same time, the efficient adsorption performance also reduces the energy consumption in the process of treating wastewater, further reducing the overall economic cost; (3) The chitosan microspheres obtained by this preparation method have excellent adsorption capacity for heavy metal ions and can effectively remove heavy metal pollutants in water, making important contributions to water resource purification and environmental protection. In addition, it avoids the secondary pollution problems that may be caused by traditional treatment methods, such as the new chemical emissions that may be caused by neutralization and reduction methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 , Schematic diagram of preparation technology Figure 2 , Scanning electron microscopy images of chitosan microspheres Figure 3 , Infrared absorption spectrum of chitosan microspheres Figure 4 , XRD patterns of chitosan microspheres Figure 5 Effect of pH value on the adsorption of Cd(II) by PEI-CS microspheres Figure 6 Effect of PEI-CS microsphere dosage on the adsorption of Cd(II) Figure 7 Effect of adsorption time on the adsorption amount of Cd(II) by PEI-CS microspheres Figure 8 Effect of pH value on the adsorption of Pb(II) by PEI-CS microspheres Fig. 9 Effect of PEI-CS microsphere dosage on the adsorption of Pb(II) Fig.10 Effect of adsorption time on the adsorption amount of Pb(II) by PEI-CS microspheres Fig.11 Effect of pH value on the adsorption of Cu(II) by PEI-CS microspheres Fig.12 Effect of PEI-CS microsphere dosage on the adsorption of Cu(II) Fig.13 Effect of adsorption time on the adsorption amount of Cu(II) by PEI-CS microspheres from Figure 2 Scanning electron microscopy characterization shows that the chitosan microspheres maintain good monodispersity and spherical morphology, with a particle size of 400µm and a smooth surface.

[0021] from Figure 3 The infrared absorption spectrum shows that at 2030cm -1 The stretching oscillation of -CH appeared at 1640cm -1 Appeared-NH 2 The bending oscillation at 1080cm -1 The stretching oscillation of C-OH appeared; at 1080cm -1 The peak at 2030 cm-1 of CS microspheres is lower than that of PEI-CS microspheres, indicating that the epoxy bond has undergone a ring-opening reaction. -1 The peak at chitosan microspheres is lower than that of PEI-CS microspheres, indicating that PEI was successfully grafted onto CS microspheres and the amino functionalization modification was completed.

[0022] Depend on Figure 4 It can be seen that the broad peak appearing in the range of 2θ of 10°-25° is the amorphous characteristic peak of chitosan microspheres modified by polyethyleneimine. DETAILED DESCRIPTION

[0023] Preparation of chitosan microspheres modified with polyethyleneimine Example 1: Preparation of PEI-CS microspheres 1 Step 1: Prepare the solution Preparation of dispersed phase: 200 mL of 4 wt% acetic acid solution was added to a 500 mL three-necked flask, 6 g of chitosan powder was weighed, added to the three-necked flask, heated and stirred for 60 min at a temperature of 50° C. and a rotation speed of 250 r / min to completely dissolve the chitosan to obtain a chitosan solution, and the chitosan solution was filtered and vacuum degassed 5 times, with a filter mesh aperture of 80 μm and a vacuum degree of 0.06 MPa to obtain a clear and transparent light yellow chitosan solution, which was used as a dispersed phase, i.e., an aqueous phase; Preparation of continuous phase: Add 200 mL of Span 80 to 500 mL of n-octanol solution and stir evenly. The resulting mixed solution is used as the continuous phase, i.e., the oil phase. Preparation of cross-linking curing liquid: 15 mL of 25 wt% glutaraldehyde solution was measured and mixed with 60 mL of n-octanol solution, and stirred evenly to obtain the cross-linking curing liquid; Step 2: Chitosan microdroplet preparation The aqueous phase described in step 1 is loaded into a 10 mL syringe equipped with a flat needle (Φ=600 μm), and enters the microfluidic chip pipeline through an aqueous phase microinjection pump at a flow rate of 2 mL / h. The oil phase is loaded into a 50 mL syringe equipped with a flat needle (Φ=600 μm), and enters the microfluidic chip pipeline through an oil phase microinjection pump at a flow rate of 20 mL / h. The aqueous phase and the oil phase form oil-in-water emulsion droplets at the intersection of the pipeline to obtain chitosan microdroplets. The particle size of the chitosan microdroplets is 300-350 μm, and the chitosan microdroplets are transported to the outlet of the microfluidic chip along the transport channel; Step 3: Chemical cross-linking The chitosan microdroplets described in step 2 are collected into the cross-linked curing liquid described in step 1, and stirred while collecting at 70° C., the collection time is 10 min, the rotation speed is 100 r / min, and after stopping the collection, the temperature is kept constant and stirring is continued for 60 min to obtain chemically cross-linked chitosan microspheres; Step 4: Wash and Dry The chemically cross-linked chitosan microspheres in step 3 are first washed with an acetone solution, then washed with an ethanol solution, and then washed with an excess of deionized water, and then transferred to a constant temperature box and dried at 35° C. for 3 h to obtain dry chemically cross-linked chitosan microspheres; Step 5: Polyethyleneimine modified chitosan microspheres Take 10 g of the dried chemically cross-linked chitosan microspheres described in step 4 and add them to a 250 mL three-necked flask. 2 Protection, add 100mL of acetone and stir for 12h, the temperature is 25℃, the speed is 100r / min, then take 20mL of acryloyl chloride (bridging agent) and add it to a three-necked flask and stir for 10h, the temperature is 40℃, the speed is 100r / min, then filter with a sand core funnel, the solid product is first washed with acetone 3 times, and then washed with methanol 3 times; the washed product is transferred to a 250mL three-necked flask, 120mL of methanol and 20g of polyethyleneimine are added and stirred for 24h, the temperature is 35℃, the speed is 100r / min, after the reaction is completed, filter, wash with methanol 3 times, put into a vacuum drying oven at 40℃ and dry for 10h, and obtain PEI-CS microspheres 1.

[0024] Example 2: Preparation of PEI-CS microspheres 2 Step 1: Prepare the solution Preparation of dispersed phase: 200 mL of 4 wt% acetic acid solution was added to a 500 mL three-necked flask, 10 g of chitosan powder was weighed and added to the three-necked flask, heated and stirred for 60 min at a temperature of 50° C. and a rotation speed of 250 r / min to completely dissolve the chitosan to obtain a chitosan solution, and the chitosan solution was filtered and vacuum degassed 5 times, with a filter mesh aperture of 80 μm and a vacuum degree of 0.06 MPa to obtain a clear and transparent light yellow chitosan solution, which was used as a dispersed phase, i.e., an aqueous phase; Preparation of continuous phase: Add 300 mL of Span 80 to 500 mL of n-octanol solution and stir evenly. The resulting mixed solution is used as the continuous phase, i.e., the oil phase. Preparation of cross-linking curing liquid: 30 mL of 25 wt% glutaraldehyde solution was measured and mixed with 60 mL of n-octanol solution, and stirred evenly to prepare the cross-linking curing liquid; Step 2: Chitosan microdroplet preparation The aqueous phase described in step 1 is loaded into a 10 mL syringe equipped with a flat needle (Φ=600 μm), and enters the microfluidic chip pipeline through an aqueous phase microinjection pump at a flow rate of 4 mL / h. The oil phase is loaded into a 50 mL syringe equipped with a flat needle (Φ=600 μm), and enters the microfluidic chip pipeline through an oil phase microinjection pump at a flow rate of 20 mL / h. The aqueous phase and the oil phase form oil-in-water emulsion droplets at the intersection of the pipeline to obtain chitosan microdroplets. The particle size of the chitosan microdroplets is 400-450 μm, and the chitosan microdroplets are transported to the outlet of the microfluidic chip along the transport channel; Step 3: Chemical cross-linking The chitosan microdroplets described in step 2 are collected into the cross-linked curing liquid described in step 1, and stirred while collecting at 70° C., the collection time is 10 min, the rotation speed is 100 r / min, and after stopping the collection, the temperature is kept constant and stirring is continued for 60 min to obtain chemically cross-linked chitosan microspheres; Step 4: Wash and Dry The chemically cross-linked chitosan microspheres were first washed with an acetone solution, then washed with an ethanol solution, and then washed with an excess of deionized water, and then transferred to a constant temperature box and dried at 35° C. for 3 hours to obtain dry chemically cross-linked chitosan microspheres; Step 5: Polyethyleneimine modified chitosan microspheres Take 15 g of the dried chemically cross-linked chitosan microspheres described in step 4 and add them to a 250 mL three-necked flask. 2 Protection, add 100mL of acetone and stir for 12h, the temperature is 25℃, the speed is 100r / min, then take 20mL of acryloyl chloride (bridging agent) and add it to a three-necked flask and stir for 10h, the temperature is 40℃, the speed is 100r / min, then filter with a sand core funnel, the solid product is first washed with acetone 3 times, and then washed with methanol 3 times; the washed product is transferred to a 250mL three-necked flask, 120mL of methanol and 20g of polyethyleneimine are added and stirred for 24h, the temperature is 35℃, the speed is 100r / min, after the reaction is completed, filter, wash with methanol 3 times, put into a vacuum drying oven at 40℃ and dry for 10h to obtain PEI-CS microspheres 2.

[0025] Example 3: Preparation of PEI-CS microspheres 3 Step 1: Prepare the solution Preparation of dispersed phase: 200 mL of 4 wt% acetic acid solution was added to a 500 mL three-necked flask, 10 g of chitosan powder was weighed and added to the three-necked flask, heated and stirred for 60 min at a temperature of 50° C. and a rotation speed of 250 r / min to completely dissolve the chitosan to obtain a chitosan solution, and the chitosan solution was filtered and vacuum degassed 5 times, with a filter mesh aperture of 80 μm and a vacuum degree of 0.06 MPa to obtain a clear and transparent light yellow chitosan solution, which was used as a dispersed phase, i.e., an aqueous phase; Preparation of continuous phase: Add 300 mL of Span 80 to 500 mL of n-octanol solution and stir evenly. The resulting mixed solution is used as the continuous phase, i.e., the oil phase. Preparation of cross-linking curing liquid: 30 mL of 25 wt% glutaraldehyde solution was measured and mixed with 20 mL of n-octanol solution, and stirred evenly to prepare the cross-linking curing liquid; Step 2: Chitosan microdroplet preparation The aqueous phase described in step 1 is loaded into a 10 mL syringe equipped with a flat needle (Φ=300 μm), and enters the microfluidic chip pipeline through an aqueous phase microinjection pump at a flow rate of 4 mL / h. The oil phase is loaded into a 50 mL syringe equipped with a flat needle (Φ=600 μm), and enters the microfluidic chip pipeline through an oil phase microinjection pump at a flow rate of 20 mL / h. The aqueous phase and the oil phase form oil-in-water emulsion droplets at the intersection of the pipeline to obtain chitosan microdroplets. The particle size of the chitosan microdroplets is 200-250 μm, and the chitosan microdroplets are transported to the outlet of the microfluidic chip along the transport channel; Step 3: Chemical cross-linking The chitosan microdroplets described in step 2 are collected into the cross-linked curing liquid described in step 1, and stirred while collecting at 70° C., the collection time is 10 min, the rotation speed is 100 r / min, and after stopping the collection, the temperature is kept constant and stirring is continued for 60 min to obtain chemically cross-linked chitosan microspheres; Step 4: Wash and Dry The chemically cross-linked chitosan microspheres in step 3 are first washed with an acetone solution, then washed with an ethanol solution, and then washed with an excess of deionized water, and then transferred to a constant temperature box and dried at 35° C. for 3 h to obtain dry chemically cross-linked chitosan microspheres; Step 5: Polyethyleneimine modified chitosan microspheres Take 15 g of the dried chemically cross-linked chitosan microspheres described in step 4 and add them to a 250 mL three-necked flask. 2After protection, 100 mL of acetone was added and stirred for 12 h at 25 °C and 100 r / min. Subsequently, 20 mL of acryloyl chloride (bridging agent) was added to a three-necked flask and stirred for 10 h at 40 °C and 100 r / min. Then, the mixture was filtered with a sand core funnel. The solid product was washed 3 times with acetone and 3 times with methanol. The washed product was transferred to a 250 mL three-necked flask, 120 mL of methanol and 20 g of polyethyleneimine were added and stirred for 24 h at 35 °C and 100 r / min. After the reaction was completed, the mixture was filtered, washed 3 times with methanol, and dried in a vacuum drying oven at 40 °C for 10 h to obtain PEI-CS microspheres 3.

[0026] Application of PEI-CS microspheres in adsorbing heavy metals in water (the PEI-CS used in the following Examples 4-6 are all PEI-CS microspheres 1 prepared in Example 1): Example 4: Adsorption performance of PEI-CS microspheres for Cd(II) Batch intermittent adsorption experiments were conducted to investigate the effects of different factors on the removal of Cd(II) by PEI-CS microspheres. 3 ) 2 4H 2 2.744 g of O crystals were dissolved in 200 mg of deionized water, and then transferred to a 1000 mL volumetric flask to obtain a 1000 mg / L solution; 50 mL of the solution was taken and fixed to volume in a 1000 mL volumetric flask to obtain a test solution with a Cd(II) content of 50 mg / L; (1) Effect of pH on the adsorption of Cd(II) by PEI-CS microspheres Take 6 portions of the test solution and add them into a conical flask, each portion is 50 mL, and the pH is adjusted to 2, 3, 4, 5, 6, and 7 with 1 mol / L HCl and 1 mol / L NaOH, respectively. Take 0.05 g of the above-mentioned dried PEI-CS microspheres and put them into the test solution respectively. The test solution is placed in a constant temperature oscillator for oscillation reaction, the constant temperature is 25°C, the oscillation frequency is 150 r / min, and the reaction time is 120 min. After the reaction is completed, take 0.5 mL of the upper solution, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Cd(II). The corresponding Cd(II) concentration is calculated with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Cd(II) is calculated by formula (1): (1) q e : Equilibrium adsorption capacity (mg / g), V : Volume of Cd(II) solution (mL), m : mass of adsorbent (mg), C0 : Initial concentration of Cd(II) solution (mg / L), C e : Cd(II) solution concentration after adsorption equilibrium (mg / L); Effect of pH value on the adsorption of Cd(II) by PEI-CS microspheres Figure 5 As shown, with the increase of pH value, the adsorption amount of PEI-CS microsphere 1 gradually increases. When the pH value reaches 5, the adsorption amount is the largest. The adsorption amount of Cd(II) by PEI-CS microsphere is 57.56 mg / g, and then gradually decreases. When pH>6, hydroxide flocculent precipitate will be generated. Therefore, the present invention controls the pH of the solution to 5.

[0027] (2) Effect of PEI-CS microsphere dosage on Cd(II) adsorption Take 6 portions of the test solution and add them to a conical flask, each portion is 50 mL, adjust the pH to 5 with 1 mol / L HCl, add 0.025 g, 0.05 g, 0.075 g, 0.1 g, 0.125 g, and 0.15 g of PEI-CS microspheres 1 to the test solution, respectively, and put the test solution into a constant temperature oscillator for oscillation reaction, with a constant temperature of 25° C., an oscillation frequency of 150 r / min, and a reaction time of 120 min; after the reaction is completed, take 0.5 mL of the upper solution, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Cd(II), and calculate the corresponding Cd(II) concentration with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Cd(II) is calculated by formula (1); Effect of PEI-CS microsphere dosage on adsorption Figure 6 As shown in the figure, with the increase of the amount of PEI-CS microspheres added, the adsorption amount gradually decreased and the removal rate gradually increased. In order to ensure the removal effect of PEI-CS microspheres on Cd(II) and consider saving the amount of PEI-CS microspheres, the amount of PEI-CS microspheres at the intersection of the removal rate curve and the adsorption amount curve was selected as 1g / L as the most suitable dosage. The adsorption amount at the intersection was 55.2mg / g, and the removal rate was 83.26%.

[0028] (3) Effect of adsorption time on the adsorption amount of Cd(II) by PEI-CS microspheres Take 50 mL of the test solution and add it to a conical flask, adjust the pH to 5 with 1 mol / L HCl, add 0.05 g of PEI-CS microsphere adsorbent, put the test solution into a constant temperature oscillator for oscillation reaction, keep the temperature at 25° C., and the oscillation frequency is 150 r / min. Take 0.5 mL of the upper solution at 5 min, 10 min, 15 min, 25 min, 30 min, 45 min, 60 min, 75 min, 90 min, 105 min, and 120 min, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Cd(II). Calculate the corresponding Cd(II) concentration with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Cd(II) is calculated by formula (1); Effect of adsorption time on the adsorption of Cd(II) by PEI-CS microspheres Figure 7 As shown in the figure, in the initial 30 minutes, as the adsorption time increases, the adsorption amount of PEI-CS microspheres on Cd(II) gradually increases. As time goes by, the increase in adsorption amount becomes gentle, and the adsorption equilibrium is reached at 90 minutes, and the adsorption amount at the equilibrium is 53.8 mg / g. Example 5: Adsorption performance of PEI-CS microspheres for Pb(II) Batch intermittent adsorption experiments were conducted to investigate the effects of different factors on the removal of Pb(II) by PEI-CS microspheres. 3 ) 2 1.598 g of the crystals were dissolved in 200 mg of deionized water, and then transferred to a 1000 mL volumetric flask and fixed to volume to obtain a 1000 mg / L solution; 50 mL of the solution was taken and fixed to volume in a 1000 mL volumetric flask to obtain a test solution with a Pb(II) content of 50 mg / L; (1) Effect of pH value on the adsorption of Pb(II) by PEI-CS microspheres Take 6 portions of the test solution and add them into a conical flask, each portion is 50 mL, and the pH is adjusted to 2, 3, 4, 5, 6, and 7 with 1 mol / L HCl and 1 mol / L NaOH, respectively. 0.1 g of the above-mentioned dried PEI-CS microspheres are respectively added into the test solution, and the test solution is placed in a constant temperature oscillator for oscillation reaction, with a constant temperature of 25° C., an oscillation frequency of 150 r / min, and a reaction time of 120 min. After the reaction is completed, take 0.5 mL of the upper solution, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Pb(II). The corresponding Pb(II) concentration is calculated with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Pb(II) is calculated by formula (2);

[0029] q e: Equilibrium adsorption capacity (mg / g), V : Volume of Pb(II) solution (mL), m : mass of adsorbent (mg), C 0 : Initial concentration of Pb(II) solution (mg / L), C e : concentration of Pb(II) solution after adsorption equilibrium (mg / L); Effect of pH value on the adsorption of Pb(II) by PEI-CS microspheres Figure 8 As shown, the adsorption performance is best when pH=5, and the adsorption amount of Cu(II) by PEI-CS microspheres is 55.2 mg / g, which then gradually decreases.

[0030] (2) Effect of PEI-CS microsphere dosage on Pb(II) adsorption Take 6 portions of the test solution and add them to a conical flask, each portion is 50 mL, adjust the pH to 5 with 1 mol / L HCl, add 0.025 g, 0.05 g, 0.075 g, 0.1 g, 0.125 g, and 0.15 g of PEI-CS microspheres to the test solution respectively, put the test solution into a constant temperature oscillator for oscillation reaction, the constant temperature is 25° C., the oscillation frequency is 150 r / min, and the reaction time is 120 min; after the reaction is completed, take 0.5 mL of the upper solution, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Pb(II), and calculate the corresponding Pb(II) concentration with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Pb(II) is calculated by formula (2); Effect of PEI-CS microsphere dosage on adsorption Fig. 9 As shown in the figure, with the increase of the amount of PEI-CS microspheres added, the adsorption amount gradually decreased and the removal rate gradually increased. In order to ensure the removal effect of PEI-CS microspheres on Pb(II) and consider saving the amount of PEI-CS microspheres, the amount of PEI-CS microspheres at the intersection of the adsorption rate curve and the adsorption amount curve was selected as 1.5 g / L as the most suitable dosage. The adsorption amount at the intersection was 80.2 mg / g and the removal rate was 90.4%.

[0031] (3) Effect of adsorption time on the amount of Pb(II) adsorbed by PEI-CS microspheres Take 50 mL of the test solution and add it to a conical flask, adjust the pH to 5 with 1 mol / L HCl, add 0.1 g of PEI-CS microsphere adsorbent, put the test solution into a constant temperature oscillator for oscillation reaction, keep the temperature at 25°C, and the oscillation frequency is 150 r / min. Take 0.5 mL of the upper solution at 5 min, 10 min, 15 min, 25 min, 30 min, 45 min, 60 min, 75 min, 90 min, 105 min, and 120 min, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Pb(II). Calculate the corresponding Pb(II) concentration with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Pb(II) is calculated by formula (2); Effect of adsorption time on the adsorption of Pb(II) by PEI-CS microspheres Fig.10 As shown in the figure, within the initial 60 min, as the adsorption time increases, the adsorption amount of Pb(II) by PEI-CS microspheres gradually increases. As time goes by, the increase in adsorption amount becomes gentle, and the adsorption equilibrium is reached at 100 min, and the adsorption amount at the equilibrium is 91.4 mg / g. Example 6: Adsorption performance of PEI-CS microspheres on Cu(II) Batch intermittent adsorption experiments were conducted to investigate the effects of different factors on the removal of Cu(II) by PEI-CS microspheres. Cu(NO 3 ) 2 ·3H 2 3.775 g of Cu(II) O crystals were dissolved in 200 mg of deionized water, and then transferred to a 1000 mL volumetric flask to obtain a solution with a Cu(II) content of 1000 mg / L; 50 mL of the solution was taken and added to a 1000 mL volumetric flask to obtain a solution to be tested with a Cu(II) content of 50 mg / L; (1) Effect of pH value on the adsorption of Cu(II) by PEI-CS microspheres Take 6 portions of the test solution and add them into a conical flask, each portion is 50 mL, and the pH is adjusted to 2, 3, 4, 5, 6, and 7 with 1 mol / L HCl and 1 mol / L NaOH, respectively. 0.05 g of the above-mentioned dried PEI-CS microspheres are respectively added into the test solution, and the test solution is placed in a constant temperature oscillator for oscillation reaction, with a constant temperature of 25° C., an oscillation frequency of 150 r / min, and a reaction time of 120 min. After the reaction is completed, take 0.5 mL of the upper solution, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Cd(II). The corresponding Cd(II) concentration is calculated with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Cu(II) is calculated by formula (3): (3) qe : Equilibrium adsorption capacity (mg / g), V : Volume of Cu(II) solution (mL), m : mass of adsorbent (mg), C 0 : Initial concentration of Cu(II) solution (mg / L), C e : Concentration of Cu(II) solution after adsorption equilibrium (mg / L); Effect of pH value on the adsorption of Cu(II) by PEI-CS microspheres Fig.11 As shown in Figure 2, with the increase of pH value, the adsorption amount of PEI-CS microspheres gradually increased, but due to the generation of Cu(OH) 2 Precipitation, and Cu(II) completely precipitates at pH=6.4, which is not conducive to the adsorption of the adsorbent. Therefore, the optimal adsorption condition is pH=5. At this time, the adsorption amount of Cu(II) by PEI-CS microspheres is 63.8 mg / g; (2) Effect of PEI-CS microsphere dosage on Cu(II) adsorption Take 6 portions of the test solution and add them to a conical flask, each portion is 50 mL, adjust the pH to 5 with 1 mol / L HCl, add 0.025 g, 0.05 g, 0.075 g, 0.1 g, 0.125 g, and 0.15 g of PEI-CS microspheres to the test solution respectively, put the test solution into a constant temperature oscillator for oscillation reaction, the constant temperature is 25°C, the oscillation frequency is 150 r / min, and the reaction time is 120 min; after the reaction is completed, take 0.5 mL of the upper solution, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Cu(II), and calculate the corresponding Cu(II) concentration with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Cu(II) is calculated by formula (3); Effect of PEI-CS microsphere dosage on adsorption Fig.12 As shown in the figure, with the increase of the amount of PEI-CS microspheres added, the adsorption amount gradually decreased. In order to ensure the removal effect of PEI-CS microspheres on Cu(II), the amount of PEI-CS microspheres at the intersection of the adsorption rate curve and the adsorption amount curve was selected as 2 g / L. The adsorption amount at the intersection was 73.5 mg / g, and the removal rate was 85.2%.

[0032] (3) Effect of adsorption time on the amount of Cu(II) adsorbed by PEI-CS microspheres Take 50 mL of the test solution and add it to a conical flask, adjust the pH to 5 with 1 mol / L HCl, add 0.1 g of PEI-CS microsphere adsorbent, put the test solution into a constant temperature oscillator for oscillation reaction, keep the temperature at 25°C, and the oscillation frequency is 150 r / min. Take 0.5 mL of the upper solution at 5 min, 10 min, 15 min, 25 min, 30 min, 45 min, 60 min, 75 min, 90 min, 105 min, and 120 min, dilute it 50 times, and use an atomic absorption spectrophotometer to determine the concentration of Cu(II). Calculate the corresponding Cu(II) concentration with reference to the standard curve. The adsorption capacity of PEI-CS microspheres for Cu(II) is calculated by formula (3); Effect of adsorption time on the adsorption of Cu(II) by PEI-CS microspheres Fig.13 As shown in the figure, in the initial 60 minutes, as the adsorption time increases, the adsorption amount of PEI-CS microspheres on Cu(II) gradually increases. As time goes by, the increase in adsorption amount becomes gentle, and the adsorption equilibrium is reached at 90 minutes. The adsorption amount at the equilibrium is 85.1 mg / g. Comparative Example Comparative Example 1: Adsorption of Cadmium Ions by Coconut Shell Activated Carbon (Jiangsu Macot Carbon Co., Ltd., product model: YK212) The method of Example 4-6 for the adsorption performance of heavy metals in water was adopted, and the PEI-CS microspheres 1 in Example 1 were replaced with coconut shell activated carbon (Jiangsu Macot Carbon Co., Ltd., product model: YK212), and the adsorption performance for Cd(II), Pb(II), and Cu(II) was obtained as shown in Table 1.

[0033] Comparative Example 2: Adsorption of copper ions by montmorillonite (Inner Mongolia Heyuan Bentonite Technology Co., Ltd., product model: z002) The method of Example 4-6 for the adsorption performance of heavy metals in water was adopted, and the PEI-CS microsphere 1 in Example 1 was replaced with montmorillonite (Inner Mongolia Heyuan Bentonite Technology Co., Ltd., product model: z002), and the adsorption performance for Cd(II), Pb(II), and Cu(II) was obtained as shown in Table 1.

[0034] Comparative Example 3: Adsorption performance of diatomite (Hebei Hengguang Mineral Products Co., Ltd., product model: 400 mesh) on Pb(II) The method of Example 4-6 for the adsorption performance of heavy metals in water was adopted, and the PEI-CS microsphere 1 in Example 1 was replaced with diatomaceous earth (Hebei Hengguang Mineral Products Co., Ltd., product model: 400 mesh), and the adsorption performance for Cd(II), Pb(II), and Cu(II) was obtained as shown in Table 1.

[0035] Table 1 shows the best adsorption performance of the adsorbents in Examples 4-6 and Comparative Examples 1-3 for heavy metals in water (the data in Table 1 are the best adsorption performance data obtained during the experiment, not the data obtained under the conditions of Examples 4-6).

[0036]

[0037] Since the above adsorptions all conform to the Langmuir isotherm adsorption model, the adsorption capacity in Table 1 is calculated by the Langmuir adsorption isotherm, and its expression is:

[0038] where qe is the equilibrium adsorption amount, Ce is the equilibrium concentration, qm is the adsorption capacity, and b is the Langmuir adsorption constant.

[0039] As can be seen from Table 1, the polyethyleneimine-modified chitosan microspheres of the present invention are superior to traditional adsorbents in terms of adsorption capacity, removal rate, adsorption equilibrium time, and adsorbent dosage in the application of adsorbing heavy metal ions Cd (II), Pb (II), and Cu (II) in water. This is because the polyethyleneimine-modified chitosan microspheres prepared by the reverse microemulsion method controlled by droplet microfluidics technology have highly uniform particle size and high controllability of particle size during the preparation process. The particle size of the microspheres can be flexibly adjusted according to different application requirements, thereby meeting the use requirements of various heavy metal ion adsorption; in addition, through the functional functional group surface modification technology, the distribution density and number of amino functional groups on the surface of chitosan microspheres are greatly improved, thereby achieving high adsorption efficiency and short adsorption equilibrium time, and can more effectively remove heavy metal ions in water, and keep good adsorption performance during use, and can use relatively less adsorbent dosage to achieve better adsorption effect, thereby reducing the amount and cost of adsorbent.

Claims

1. A polyethyleneimine-modified chitosan microsphere, characterized in that: The chitosan microspheres modified with polyethyleneimine are prepared by a reverse microemulsion method controlled by droplet microfluidics technology. The chitosan microspheres modified with polyethyleneimine have smooth particle surfaces, a particle size of 200-450 μm, an adsorption capacity of ≤88.62 mg / g for Cd(II), ≤156.6 mg / g for Pb(II), and ≤141.8 mg / g for Cu(II). The chitosan microspheres modified with polyethyleneimine have a -1 、1640cm -1 、1080cm -1 Absorption peaks appear at , corresponding to the stretching oscillation of −CH, the bending oscillation of −NH2, and the stretching oscillation of C−OH; in the XRD characterization, the broad peak that appears in the 2θ range of 10°-25° is the amorphous characteristic peak of chitosan microspheres modified by polyethyleneimine.

2. A method for preparing polyethyleneimine-modified chitosan microspheres according to claim 1, characterized in that: The method comprises the following steps: Step 1: Prepare the solution Preparation of dispersed phase: add acetic acid solution to a three-necked flask, add chitosan powder to the three-necked flask, heat and stir for 30-120 min, the temperature is 40-80° C., the speed is 200-300 r / min, the chitosan is completely dissolved to obtain a chitosan solution, the chitosan solution is filtered and vacuum degassed 3-5 times, the filter mesh pore size is 80 μm, the vacuum degree is 0.06-0.6 MPa, and a clear and transparent light yellow chitosan solution is obtained, which is used as a dispersed phase, i.e., an aqueous phase; Preparation of continuous phase: Add Span 80 to the n-octanol solution and stir evenly. The obtained mixed solution is used as the continuous phase, i.e., the oil phase; Preparation of cross-linking curing liquid: Mix the glutaraldehyde solution and the n-octanol solution, stir evenly, and use the mixture as the cross-linking curing liquid. Step 2: Preparation of chitosan microdroplets The aqueous phase described in step 1 is loaded into a syringe equipped with a flat needle, and enters the microfluidic chip pipeline through an aqueous phase microinjection pump at a flow rate of 2-10 mL / h. The oil phase is loaded into a syringe equipped with a flat needle, and enters the microfluidic chip pipeline through an oil phase microinjection pump at a flow rate of 20-100 mL / h. The aqueous phase and the oil phase form oil-in-water emulsion droplets at the intersection of the pipeline to obtain chitosan microdroplets, and the chitosan microdroplets are transported to the outlet of the microfluidic chip along the transport channel; Step 3: Chemical cross-linking Collect the chitosan microdroplets in step 2 into the cross-linked curing liquid in step 1, stir while collecting, at 60-80° C., the collection time is 10-20 min, and after stopping the collection, keep the temperature unchanged and continue stirring for 40-80 min at a speed of 100-200 r / min to obtain chemically cross-linked chitosan microspheres; Step 4: Wash and Dry The chemically cross-linked chitosan microspheres in step 3 are first washed with an acetone solution, then washed with an ethanol solution, and then washed with an excess of deionized water, and then transferred to a constant temperature box and dried at 30-50° C. for 1-10 hours to obtain dry chemically cross-linked chitosan microspheres; Step 5: Polyethyleneimine modified chitosan microspheres The dried chemically cross-linked chitosan microspheres described in step 4 are added to a three-necked flask, protected by inert gas, and acetone is added and stirred for 12-24 hours at a temperature of 20-40°C and a rotation speed of 100-300r / min. Subsequently, acryloyl chloride is added to the three-necked flask and stirred for 10-20 hours at a temperature of 30-60°C and a rotation speed of 100-300r / min. Then, the mixture is filtered with a sand core funnel. The solid product is first washed with acetone for 3-5 times and then with methanol for 3-5 times. The washed product is transferred to a three-necked flask, and methanol and polyethyleneimine are added and stirred for 12-36 hours at a temperature of 30-60°C and a rotation speed of 100-200r / min. After the reaction is completed, the mixture is filtered, washed with methanol for 3-5 times, and dried in a vacuum drying oven at 40-60°C for 10-20 hours to obtain the polyethyleneimine-modified chitosan microspheres.

3. The method for preparing polyethyleneimine-modified chitosan microspheres according to claim 2, characterized in that: In step 2, the diameter of the planar needle is Φ=200-800 μm, and the volume of the syringe is 5-100 mL.

4. The method for preparing polyethyleneimine-modified chitosan microspheres according to claim 2, characterized in that: In step 2, the particle size of the chitosan microdroplets can be controlled to be 100-500 μm according to the needle size.

5. The method for preparing polyethyleneimine-modified chitosan microspheres according to claim 2, characterized in that: In step 5, the inert gas is any one of N2 and Ar.

6. A method for adsorbing heavy metal ions in water using the surface amino-functionalized chitosan microspheres of claim 1, characterized in that: The chitosan microspheres modified with polyethyleneimine are placed in a solution containing heavy metal ions, the pH is adjusted to 2-7, and the solution is placed in a constant temperature oscillator for oscillation reaction, the constant temperature is 10-40°C, the oscillation frequency is 100-200r / min, the reaction time is 5-180min, and after the reaction is completed, the upper layer solution is taken to determine the concentration of heavy metal ions.

7. The method for adsorbing heavy metal ions in water by polyethyleneimine-modified chitosan microspheres according to claim 5, wherein the heavy metal ions are one or more of Cd(II), Pb(II), and Cu(II).

8. The method for adsorbing heavy metal ions in water by chitosan microspheres modified with polyethyleneimine according to claim 6, characterized in that: At 25°C and pH=5, the adsorption capacity of the surface amino-functionalized chitosan microspheres for Cd(II) is ≤88.62 mg / g, the adsorption equilibrium time is 80 min, and the Cd(II) removal rate can reach 84.84%; at 25°C and pH=5, the adsorption capacity for Pb(II) is ≤156.6 mg / g, the adsorption equilibrium time is 90 min, and the Pb(II) removal rate can reach 91.82%; at 25°C and pH=5, the adsorption capacity for Cu(II) is ≤141.8 mg / g, the adsorption equilibrium time is 60 min, and the Cu(II) removal rate can reach 88.2%.

Citation Information

Patent Citations

  • Polyethyleneimine-chitosan adsorbent one-step synthesis method

    CN105413661A

  • Preparation method of heat-shrinkage-resistant polytetrafluoroethylene composite nanofiltration membrane