Catalyst for hydrogenation of phenyl derivatives and preparation thereof

The ruthenium/palladium-based SiO2 catalyst prepared by acid soaking pretreatment and inert gas calcination solves the problem that benzene cyclohydrogenation affects substituent groups in the prior art, and achieves a highly efficient hydrogenation reaction that retains substituent groups, with high conversion rate and multiple use.

CN119075979AActive Publication Date: 2024-12-06XIAMEN JIAHYDROGEN TECH CO LTD

Patent Information

Application Number
CN202411176529.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing catalysts are prone to affect the substituted groups on the ring during the benzene cyclohydrogenation process, resulting in the need of secondary oxidation in some processes to increase production steps and costs, and it is difficult to effectively retain substituted groups.

Method used

The pretreated carrier was soaked with acid, and the solution of o-chlorophenyl glycine and ruthenium were dispersed in water. The palladium solution was slowly added dropwise and reduced to adjust the pH value. Then, calcined under an inert and reducing gas atmosphere to prepare ruthenium/palladium-based SiO2 Supported catalyst ensures hydrogenation reactions with retained substituents.

Benefits of technology

It is achieved efficiently retaining substituent groups in the phenyl derivative hydrogenation reaction, with a conversion rate of more than 98%, a selectivity of more than 96%, and a catalyst can be used multiple times, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention relates to the field of catalysts, and particularly discloses a catalyst for phenyl derivative hydrogenation and a preparation method thereof.The catalyst is prepared by adopting SiO2 as a carrier, conducting template positioning on ruthenium ions and palladium ions through 2-chlorophenylglycine, reducing the positioned ruthenium and palladium metal ions, and conducting calcination in the inert and reducing mixed gas atmosphere, reduced ruthenium and palladium atoms are positioned and supported on SiO2, and the catalyst can be represented by a formula of 2.0 Och-0. 43Ru-0.53 Pd / SiO2. The invention develops a universal SiO2 carrier supported ruthenium and palladium catalyst, under the action of the catalyst, benzene rings can be selectively hydrogenated, functional groups, such as 1, 4-phthalic acid, are kept unchanged in the hydrogenation process, the benzene rings can be pertinently hydrogenated, and the hydrogenation efficiency is improved. By adjusting different process parameters, the conversion rate of a plurality of raw materials is greater than 98%, the selectivity of a target product is greater than 96%, and the catalyst still keeps higher activity after being used repeatedly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalytic hydrogenation, and particularly relates to a catalyst for hydrogenation of phenyl derivatives and its preparation. Background Art

[0002] Benzene and its derivatives are one of the basic raw materials for petrochemical industry. Through its relative activity, a wide variety of phenyl derivatives can be synthesized by adding substituents. The hydrogenation reaction of benzene ring with retained substituents is an extremely important reaction. It not only solves health problems, but also plays an important role in the production of various aliphatic compounds. Such substances are also important fine chemicals and have been widely used as important intermediates for medicines and pesticides, or key starting materials for the synthesis of dyes, resins and polymers. Because benzene is carcinogenic, phenyl derivatives containing benzene rings are also potentially harmful to human health.

[0003] Industrial catalysts for benzene ring hydrogenation are mainly nickel-based catalysts and ruthenium-based catalysts, such as the following:

[0004] CN110105223A discloses a method for preparing 1,3-cyclohexylenediamine by a continuous process, wherein the catalyst contains 0.5-3% ruthenium metal, 0.2-2% auxiliary metals Mn, Co and Mg, and the carrier is alumina. Under the condition of adding a small amount of auxiliary agents, m-xylylenediamine is continuously hydrogenated to achieve a m-xylylenediamine conversion rate of >90% and a selectivity of 91%.

[0005] CN112058259A discloses a catalyst for efficiently catalyzing the conversion of synthesis gas into industrial fuels. The catalyst has a carrier of TiO2 and an active ingredient of Ru metal with a content of 0.1-5wt%. The preparation steps are Ru metal loading, drying, muffle furnace sintering, dilute ammonia water treatment, drying and reduction. The preparation process is relatively complicated and its application direction is catalytic synthesis gas.

[0006] Some existing catalysts may have a certain impact on the substituents on the benzene ring during the benzene ring hydrogenation process, for example:

[0007] CN 117776868 A discloses a ruthenium-carbon catalyst:

[0008]

[0009] Although the catalyst can achieve hydrogenation on the benzene ring, the functional groups on the ring are also affected, reducing the methyl formate group to a methanol group. In production, some processes often require the retention of the functional groups on the ring. For example, 1,4-cyclohexanecarboxylic acid can be used for peptic ulcer drugs and polyester resin modification, which has a wide range of usage scenarios and application value. If this catalyst is used, the methanol group on the ring needs to be oxidized twice, which increases the production steps and costs. Summary of the invention

[0010] In view of the problems existing in the prior art, the first aspect of the present invention proposes a preparation method for a phenyl derivative hydrogenation catalyst, comprising:

[0011] S1: The carrier is pretreated by acid immersion. After washing, the carrier is dispersed in water and o-chlorophenylglycine and ruthenium solution are added;

[0013] S2: slowly add palladium solution dropwise to maintain the solution pH at 7-8;

[0014] S3: After the dripping is completed, a reducing agent is added to the solution in step S2 for reduction, the pH of the solution is adjusted, and water is removed to obtain a catalyst;

[0015] S4: In an atmosphere of an inert and reducing mixed gas, the dehydrated solid of S3 is calcined and crushed.

[0016] In some specific embodiments of the preparation method of the first aspect, the carrier in step S1 is selected from silicon dioxide, aluminum oxide, and activated carbon.

[0017] In some specific embodiments of the preparation method of the first aspect, the acid in step S1 is selected from hydrochloric acid, nitric acid, and sulfuric acid.

[0018] In some specific embodiments of the preparation method of the first aspect, the mass fraction of the acid in step S1 is 0.5-1.5%, in some embodiments 0.5%, in some embodiments 0.6%, in some embodiments 0.7%, in some embodiments 0.8%, in some embodiments 0.9%, in some embodiments 1.0%, in some embodiments 1.1%, in some embodiments 1.2%, in some embodiments 1.3%, in some embodiments 1.4%, and in some embodiments 1.5%.

[0019] In some specific embodiments of the preparation method of the first aspect, the amount of o-chlorophenylglycine in step S1 is 1 to 3 mmol per 1 g of carrier, in some embodiments, the amount of o-chlorophenylglycine is 1 mmol per 1 g of carrier, in some embodiments, the amount of o-chlorophenylglycine is 2 mmol per 1 g of carrier, and in some embodiments, the amount of o-chlorophenylglycine is 3 mmol per 1 g of carrier.

[0020] In some specific embodiments of the preparation method of the first aspect, the specific surface area of ​​the carrier is 800 to 1400 m 2 / g, in some embodiments the carrier has a specific surface area of ​​800m 2 / g, in some embodiments the carrier has a specific surface area of ​​900m 2 / g, in some embodiments the carrier has a specific surface area of ​​1000m2 / g, in some embodiments the carrier has a specific surface area of ​​1100m 2 / g, in some embodiments the carrier has a specific surface area of ​​1200m 2 / g, in some embodiments the carrier has a specific surface area of ​​1300m 2 / g, in some embodiments the carrier has a specific surface area of ​​1400m 2 / g.

[0021] In some specific embodiments of the preparation method of the first aspect, the ruthenium solution in step S1 is selected from ruthenium chloride salt and ruthenium nitrate salt solution.

[0022] In some specific embodiments of the preparation method of the first aspect, the concentration of the ruthenium solution in step S1 is 0.15-0.19 mmol / mL, in some embodiments the concentration of the ruthenium solution is 0.15 mmol / mL, in some embodiments the concentration of the ruthenium solution is 0.16 mmol / mL, in some embodiments the concentration of the ruthenium solution is 0.17 mmol / mL, in some embodiments the concentration of the ruthenium solution is 0.18 mmol / mL, and in some embodiments the concentration of the ruthenium solution is 0.19 mmol / mL.

[0023] In some specific embodiments of the preparation method of the first aspect, the palladium solution in step S2 is selected from palladium chloride and palladium nitrate.

[0024] In some specific embodiments of the preparation method of the first aspect, the concentration of the palladium solution in step S2 is 0.30-0.35 mmol / mL, in some embodiments the concentration of the palladium solution is 0.30 mmol / mL, in some embodiments the concentration of the palladium solution is 0.31 mmol / mL, in some embodiments the concentration of the palladium solution is 0.32 mmol / mL, in some embodiments the concentration of the palladium solution is 0.33 mmol / mL, in some embodiments the concentration of the palladium solution is 0.34 mmol / mL, and in some embodiments the concentration of the palladium solution is 0.35 mmol / mL.

[0025] In some specific embodiments of the preparation method of the first aspect, the reducing agent in step S3 is selected from potassium borohydride, sodium borohydride, and lithium aluminum tetrahydride.

[0026] In some specific embodiments of the preparation method of the first aspect, the concentration of the reducing agent in step S3 is 2.0-3.0 mmol / mL, in some embodiments the concentration of the reducing agent is 2.0 mmol / mL, in some embodiments the concentration of the reducing agent is 2.2 mmol / mL, in some embodiments the concentration of the reducing agent is 2.4 mmol / mL, in some embodiments the concentration of the reducing agent is 2.6 mmol / mL, in some embodiments the concentration of the reducing agent is 2.8 mmol / mL, and in some embodiments the concentration of the reducing agent is 3.0 mmol / mL.

[0027] In some specific embodiments of the preparation method of the first aspect, the pH value adjusted in step S3 is 9-10.

[0028] In some specific embodiments of the preparation method of the first aspect, the inert gas in the step S4 is selected from nitrogen, argon, or a mixture thereof.

[0029] In some specific embodiments of the preparation method of the first aspect, the reducing gas in the step S4 is selected from hydrogen.

[0030] In some specific embodiments of the preparation method of the first aspect, the volume ratio of the inert gas to the reducing gas in the S4 step is (8-10):1, in some embodiments it is 8:1, in some embodiments it is 9:1, and in some embodiments it is 10:1.

[0031] In some specific embodiments of the preparation method of the first aspect, the calcination method in step S4 is:

[0032] 1. Raise the temperature to 180-220°C at any rate of 30-60°C per minute, 40-50°C per minute, or 45°C per minute, and maintain for 1-3 minutes;

[0033] 2. Raise the temperature to 750-850°C at a rate of 20-35°C / min, or 25-35°C / min, or 30°C / min, and maintain for 5-15 minutes;

[0034] 3. Slowly cool down to room temperature at a rate not higher than 10℃ / min.

[0035] In some specific embodiments of the preparation method of the first aspect, the diameter of the particles after pulverization in step S4 is

[0036] 0.08-0.12 mm, in some embodiments the diameter is 0.08 mm, in some embodiments the diameter is 0.09 mm, in some embodiments the diameter is 0.10 mm, in some embodiments the diameter is 0.11 mm, and in some embodiments the diameter is 0.12 mm.

[0037] The second aspect of the present invention provides a catalyst prepared by the method of the first aspect.

[0038] In some specific embodiments of the preparation method of the second aspect, the catalyst can be represented by the general formula aOch-bRu-cPd / SiO2, wherein Och represents o-chlorophenylglycine, a is the micromolar amount of o-chlorophenylglycine fed per gram of carrier SiO2, a is selected from 1 to 3, preferably 2, b is the micromolar amount of ruthenium metal loaded per gram of carrier SiO2, b is selected from 0.3 to 0.6, preferably 0.43, and c is the micromolar amount of palladium metal loaded per gram of carrier SiO2, c is selected from 0.4 to 0.6, preferably 0.53.

[0039] The third aspect of the present invention provides an application of the catalyst prepared in the second aspect in catalyzing the hydrogenation of phenyl derivatives.

[0040] In some applications of the catalyst provided in the third aspect, the phenyl derivative used as a substrate is selected from m-xylylenediamine, bisphenol A, 2,4-toluenediamine, 4,4'-diaminodiphenylmethane, 1,4-phthalic acid, and p-phenylenediamine.

[0041] The yield of the present invention

[0042] Among them, n b is the maximum theoretical molar yield of the target product; n a is the actual molar yield of the target product;

[0043] The yield of the present invention

[0044] Among them, n c is the molar amount of the reaction substrate consumed; n d is the initial molar amount of the reaction substrate;

[0045] Glycine ethyl ester (CAS: 120746-42-1); Glycine (CAS: 56-40-6);

[0046] O-chlorophenylglycine (CAS: 141196-64-7);

[0047] The present invention provides a selective catalyst for retaining substituents which can be expressed by the general formula aTemp-bRu-cPd / SiO2:

[0048] After the calcination process, the complexing positioning template agent is destroyed. The formula aTemp-bRu-cPd / SiO2 does not mean that the catalyst after calcination still retains the complexing positioning template agent. The formula Temp only represents the type of complexing positioning template agent used in the preparation process.

[0049] a is the molar amount of complexing template agent Temp added per 1g carrier SiO2, and the value range of a is 1mmol~3mmol;

[0050] Temp in the following examples or comparative examples is Ges, Gly, Och, respectively, Ges represents the use of glycine ethyl ester (CAS: 120746-42-1) as a complexing template, Gly represents the use of glycine (CAS: 56-40-6) as a complexing template, and Och represents the use of o-chlorophenylglycine (CAS: 141196-64-7) as a complexing template;

[0051] Wherein, b is the molar amount of ruthenium atoms loaded per 1g of carrier SiO2, and the value range of b is 0.3mmol~0.6mmol;

[0052] Wherein, c is the molar amount of palladium atoms loaded per 1g of carrier SiO2, and the value range of c is 0.4mmol~0.6mmol;

[0053] In the present invention, the room temperature is 5-40°C in some embodiments, 10-35°C in some embodiments, 15-30°C in some embodiments, 20-25°C in some embodiments, and 25°C in some embodiments.

[0054] The reagents used in the present invention are all purchased from the open legal market, such as Sinopharm Shanghai Test, Sigma, MacLean, Xilong and other companies, and have not been further purified.

[0055] Advantages of the present invention:

[0056] The present invention adopts SiO2 as a carrier, uses o-chlorophenylglycine to perform template positioning of ruthenium ions and palladium ions, reduces the positioned ruthenium and palladium metal ions, and calcines them in an atmosphere of an inert and reducing mixed gas, and loads the reduced ruthenium and palladium atoms on SiO2. The present invention develops a universal ruthenium / palladium-based SiO2-loaded catalyst, which is applied to a benzene ring hydrogenation catalyst with retained substituents. The catalyst can particularly selectively hydrogenate phenyl derivatives, retaining functional groups unchanged during the hydrogenation process, and achieves a conversion rate of multiple raw materials greater than 98% and a target product selectivity greater than 96% in an intermittent reactor by adjusting different process parameters, and the catalyst can be applied multiple times. DETAILED DESCRIPTION

[0057] The technical solution of the present invention is further described below, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.

[0058] Example 1

[0059] Step 1: Set the specific surface area to 1000-1200m 2 / g of 20g of silica carrier is immersed in 1% mass fraction of dilute hydrochloric acid solution and stirred for 20min. After the immersion, the carrier is filtered and washed with ultrapure water for 3 times. After filtration, the washed carrier is dispersed in 100ml of ultrapure water, 40mmol of o-chlorophenylglycine and 50ml of ruthenium chloride with a concentration of 0.173mmol / mL are added, and stirred at 200rpm for 10min.

[0060] Step 2: During the stirring process, 32 ml of palladium nitrate and sodium bicarbonate solution with a concentration of 0.33 mmol / mL were slowly added to the solution at the same time to maintain the pH of the solution at 7-8.

[0061] Step 3: After the addition, add 38 ml of potassium borohydride with a concentration of 2.5 mmol / mL to the above solution for reduction. Finally, adjust the pH of the solution to between 9 and 10, and evaporate under reduced pressure at 40°C for dehydration.

[0062] Step 4: In the presence of a mixed gas of N2 and H2 with a volume ratio of 9:1, the solid dehydrated in step 3 is calcined, the calcination temperature is increased to 200°C in 5 minutes, maintained for 1 minute, then increased to 800°C at a rate of 20°C / min, maintained for 10 minutes, and then slowly cooled to room temperature at a rate not higher than 10°C / min. After grinding into particles of about 0.1 mm, a catalyst for selective hydrogenation with retention of substituents is obtained, which is represented by the formula 2.0Och-0.43Ru-0.53Pd / SiO2, wherein Och represents o-chloropHenylglycine (CAS: 141196-64-7) in the preparation process.

[0063] Comparative Example 1:

[0064] The difference between Comparative Example 1 and Example 1 is that the o-chlorophenylglycine in step 1 is replaced with an equal molar amount of glycine to obtain a catalyst 2.0Gly-0.43Ru-0.53Pd / SiO2, wherein Gly represents the use of glycine as a complexing template in the preparation process. Comparative Example 2:

[0065] The difference between Comparative Example 2 and Example 1 is that the o-chlorophenylglycine in step 1 is replaced with an equimolar amount of glycine ethyl ester to obtain a catalyst 2.0Ges-0.43Ru-0.53Pd / SiO2, wherein Ges represents glycine ethyl ester used as the complexing template in the preparation process.

[0066] Comparative Example 3:

[0067] The difference between Comparative Example 3 and Example 1 is that in step S2, instead of palladium nitrate being added dropwise, an equimolar amount of nickel nitrate is added dropwise to obtain a catalyst 2.0Och-0.43Ru-0.53Ni / SiO2, wherein Och indicates that o-chlorophenylglycine (O-chloropHenylglycine) is used as the complexing template agent in the preparation process.

[0068] Comparative Example 4:

[0069] The difference between Comparative Example 4 and Example 1 is that potassium borohydride reduction is not used.

[0070] Comparative Example 5:

[0071] The difference between Comparative Example 5 and Example 1 is that ruthenium chloride is not added, and the catalyst 2.0Och-0.53Pd / SiO2 is obtained, wherein Och represents that the complexing template agent used in the preparation process is o-chlorophenylglycine (O-chloropHenylglycine).

[0072] Comparative Example 6:

[0073] The difference between Comparative Example 6 and Example 1 is that after palladium nitrate is added dropwise in step S2, platinum nitrate with a molar amount of 30% palladium nitrate is added dropwise to obtain a catalyst 2.0Och-0.43Ru-0.53Pd-0.16Pt / SiO2, wherein Och represents that the complexing template agent used in the preparation process is o-chlorophenylglycine (O-chloropHenylglycine);

[0074] Embodiment 2:

[0075] 735mmol of m-xylylenediamine and 1000ml of chloroform were added to an autoclave, and then 2wt% of the catalyst prepared in Example 1 (based on the mass of m-xylylenediamine) was added. The catalytic temperature was maintained between 150 and 160°C, and hydrogen was introduced at a pressure range of 4.0 to 4.5MPa. The catalytic reaction was carried out for 5.0h to obtain a hydrogenated mixed solution. The conversion rate of the raw material m-xylylenediamine was 99.1%, and the selectivity yield% of the target product 1,3-cyclohexylenediamine was 96.21%.

[0076] Embodiment 3:

[0077] 439mmol of bisphenol A and 600ml of chloroform were placed in an autoclave, and 3wt% of the catalyst prepared in Example 1 (based on the mass of bisphenol A) was added. The catalytic temperature was maintained between 150 and 160°C, and hydrogen was introduced at a pressure range of 3.0 to 3.5MPa. The catalytic reaction was carried out for 5.0h to obtain a hydrogenated mixed solution. The conversion rate of the raw material bisphenol A was 99.95%, and the selectivity yield% of the target product hydrogenated bisphenol A was 97.1%.

[0078] Embodiment 4:

[0079] 819.6 mmol of 2,4-toluenediamine and 1200 ml of tetrahydrofuran were added to an autoclave, and 1 wt% of the catalyst prepared in Example 1 (based on the mass of 2,4-toluenediamine) was added; the catalytic temperature was maintained between 130 and 140° C., hydrogen gas at a pressure of 4.0 MPa was introduced, and the catalytic reaction was carried out for 3 hours to obtain a hydrogenated mixed solution; the conversion rate of the raw material 2,4-toluenediamine was 99.91%, and the selectivity yield% of the target product 1-methyl-2,4-cyclohexanediamine was 98.40%;

[0080] Embodiment 5:

[0081] 505mmol of MDA (4,4'-diaminodiphenylmethane) and 800ml of tetrahydrofuran were added to an autoclave, and 3wt% of the catalyst prepared in Example 1 (based on the mass of 4,4'-diaminodiphenylmethane) was added; the catalytic temperature was maintained between 140 and 150°C, and hydrogen gas at a pressure of 4.5MPa was introduced for catalytic reaction for 3h to obtain a hydrogenated mixed solution; the conversion rate of the raw material 4,4'-diaminodiphenylmethane was 99.93%, and the selectivity yield% of the target product 4,4'-diaminodicyclohexylmethane was 98.64%;

[0082] Embodiment 6:

[0083] The catalysts prepared in Example 1 and Comparative Examples 1 to 6 were mixed with 603 mmol of 1,4-phthalic acid and 900 ml of chloroform, respectively, and added into an autoclave. 5 wt% of catalyst (based on the mass of 1,4-phthalic acid) was added. The catalytic temperature was 180° C., and hydrogen gas with a pressure of 5.0 MPa was introduced. The catalytic reaction was carried out for 12 h to obtain a hydrogenated mixed solution. The yield of the target product 1,4-cyclohexanedicarboxylic acid was % and the conversion rate of the raw material 1,4-phthalic acid was conv.%, and the results are shown in Table 1:

[0084] Table 1: Effect of catalysts of Example 1 and Comparative Examples 1 to 6 on selective hydrogenation of 1,4-phthalic acid

[0085] entry Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 conv.(%) 99.1 62.9% 41.3% 5.1% 52.1% 3.2% 15.3% yield(%) 95.2 1.5% 2.6% 0.2% 7.8% 4.3% 3.6%

[0086] In Table 1, the 1,4-phthalic acid conversion rate conv.% of the catalysts of Comparative Examples 1 and 2 is 62.9% and 41.3% respectively, and the yield % of the product 1,4-cyclohexanedicarboxylic acid is 1.5% and 2.6% respectively. The yield of 1,4-cyclohexanedimethanol in Comparative Examples 1 to 6 is much higher than that of 1,4-cyclohexanedicarboxylic acid, and the carboxyl group on the benzene ring is reduced to a methanol group by hydrogen. When the catalyst prepared in Example 1 is used for the reaction, the 1,4-phthalic acid conversion rate conv.% is 99.1%, and the yield % of 1,4-cyclohexanedicarboxylic acid is as high as 95.2%.

[0087] Embodiment 7:

[0088] 926mmol of p-phenylenediamine and 1000ml of chloroform were added to an autoclave, and the catalyst prepared in Example 1 was added; the amount of the catalyst was 4wt% of the raw material in the first autoclave, and 0.4wt% was added in the second autoclave; the catalytic temperature was 150°C, and hydrogen gas at a pressure of 4.5MPa was introduced. The catalytic reaction was carried out for 3.0-4.0h to obtain a hydrogenated solution; the catalyst was recycled 10 times, and the selectivity yield% of the target product 1,4-cyclohexanediamine and the conversion rate conv.% of the reactant p-phenylenediamine were detected by GC. The results are shown in Table 2:

[0089] Table 2: Catalyst activity test after multiple cycles

[0090] Cycle times First Kettle 2 3 4 5 6 7 8 9 10 conv.(%) 99.9% 97.9% 99.9% 98.9% 99.9% 99.9% 99.9% 99.9% 99.9% 99.9% yield(%) 97.8% 97.8% 97.8% 97.8% 97.8% 97.8% 97.8% 97.8% 97.8% 97.8%

[0091] It can be seen that for the catalyst 2.0Och-0.43Ru-0.53Pd / SiO2 prepared in Example 1 of the present invention, only 0.4wt% of catalyst needs to be added in each production cycle to maintain a high conversion rate conv.% and selectivity yield%.

[0092] Embodiment 8:

[0093] The feed of each component in Example 1 was adjusted to prepare catalysts with different a, b, and c values. The prepared catalysts were mixed with 1,4-phthalic acid and chloroform according to the method and feed amount of Example 6, added to an autoclave, heated, and pressurized with hydrogen to obtain a hydrogenated mixed solution. GC test, the selectivity (yield%) of the target product 1,4-cyclohexanedicarboxylic acid and the conversion rate (conv.%) of the raw material 1,4-phthalic acid are shown in Table 3:

[0094] Table 3: Performance of catalysts with different ratios

[0095]

[0096] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

Claims

1. A catalyst for the hydrogenation of phenyl derivatives, include: S1: The carrier is pretreated by acid immersion. After washing, the carrier is dispersed in water and o-chlorophenylglycine and ruthenium solution are added; S2: slowly add palladium solution dropwise to maintain the solution pH at 7-8; S3: After the dropwise addition, a reducing agent is added to the solution in step S2 for reduction, the pH of the solution is adjusted, and water is removed; S4: In an atmosphere of an inert and reducing mixed gas, the dehydrated solid of S3 is calcined and crushed.

2. The preparation of the catalyst according to claim 1, It is characterized in that The carrier of step S1 is selected from silicon dioxide, aluminum oxide, activated carbon, and / or the acid of step S1 is selected from hydrochloric acid, nitric acid, sulfuric acid, and / or the mass fraction of the acid of step S1 is 0.5-1.5%, preferably 1%, and / or the amount of o-chlorophenylglycine added to step S1 is 1-3 mmol per 1 g of carrier, preferably 2 mmol, and / or the specific surface area of ​​the carrier is 800-1400 m 2 / g, preferably 1000-1200m 2 / g.

3. The preparation of the catalyst according to any one of claims 1 or 2, It is characterized in that The ruthenium solution in step S1 is selected from ruthenium chloride salt and ruthenium nitrate salt solution, and / or the concentration of the ruthenium solution in step S1 is 0.15-0.19 mmol / mL, preferably 0.173 mmol / mL.

4. The preparation of the catalyst according to any one of claims 1 to 3, It is characterized in that The palladium solution in step S2 is selected from palladium chloride and palladium nitrate, and / or the concentration of the palladium solution in step S2 is 0.30-0.35 mmol / mL, preferably 0.33 mmol / mL.

5. The preparation of the catalyst according to any one of claims 1 to 4, It is characterized in that The reducing agent in step S3 is selected from potassium borohydride, sodium borohydride, lithium aluminum tetrahydride, and / or the concentration of the reducing agent in step S3 is 2.0-3.0 mmol / mL, preferably 2.5 mmol / mL, and / or the pH value adjusted in step S3 is 9-10.

6. The preparation of the catalyst according to any one of claims 1 to 5, It is characterized in that In the step S4, the inert gas is selected from nitrogen, argon or a mixture thereof, and / or, the reducing gas in the step S4 is selected from hydrogen, and / or, the volume ratio of the inert gas to the reducing gas in the step S4 is (8-10):1, preferably 9:1, and / or, the calcination method in the step S4 is to heat the temperature to 180-220°C at a rate of 30°C-60°C per minute, maintain for 1-3 minutes, then heat the temperature to 750-850°C at a rate of 20-35°C / min, maintain for 5-15 minutes, and then slowly cool to room temperature at a rate not higher than 10°C / min, and / or, the diameter of the particles after crushing is 0.08-0.12 mm, preferably 0.1 mm.

7. A catalyst prepared by the method according to any one of claims 1 to 6.

8. The catalyst according to claim 7, It is characterized in that Available general formula aOch-bRu-cPd / SiO 2 In other words, Och represents o-chlorophenylglycine, and a represents SiO per gram of carrier. 2 The micromolar amount of o-chlorophenylglycine fed, wherein a is selected from 1 to 3, preferably 2, and b is per gram of carrier SiO 2 The micromolar amount of ruthenium metal loaded, wherein b is selected from 0.3 to 0.6, preferably 0.43, and c is per gram of carrier SiO 2 The micromolar amount of palladium metal loaded, wherein c is selected from 0.4 to 0.6, preferably 0.

53.

9. Use of the catalyst according to any one of claims 7 or 8 in the hydrogenation of phenyl derivatives.

10. The use according to claim 9, wherein the phenyl derivative is selected from m-phenylenediamine, 2,4-toluenediamine, 1,4-phthalic acid, p-phenylenediamine, bisphenol A, and 4,4'-diaminodiphenylmethane.

Citation Information

Patent Citations

  • Low-content supported ruthenium-palladium bimetal hydrogenation catalyst and preparation method thereof

    CN103157468A

  • Ruthenium-silver / carbon catalyst as well as preparation method and application thereof

    CN116651445A

  • Supported Pd-based selective hydrogenation catalyst as well as preparation method and application thereof

    CN117654488A

  • Heterocyclic compound

    WO2013100027A1

Cited By

  • Continuous production method of 1, 3-cyclohexyl dimethylamine

    CN119874532A