High-temperature and high-pressure film covering process for OPP and PET material soft film with gum
The high-temperature and high-pressure lamination process with a composite functional agent addresses adhesive aging and corona issues in soft films, ensuring durability and quality in packaging and electronic applications.
Patent Information
- Application Number
- CN202411062289.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing soft film lamination processes face issues with pressure-sensitive adhesive aging, hardening, and viscosity loss due to ultraviolet exposure, and quality degradation from corona phenomena caused by static electricity, leading to reduced durability and product appearance.
A high-temperature and high-pressure lamination process incorporating a composite functional agent with ultraviolet absorption and antistatic properties, prepared by specific chemical reactions, is applied to OPP and PET films, enhancing durability and reducing surface resistance.
The process effectively prevents adhesive aging and corona-induced degradation, maintaining film quality and extending product life, suitable for packaging, advertising, and electrical applications.
Smart Images

Figure BDA0004978297860000031 
Figure BDA0004978297860000032 
Figure BDA0004978297860000041
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of soft film lamination, and in particular, relates to a high-temperature and high-pressure lamination process for soft films made of adhesive-backed OPP and PET materials. Background Art
[0002] With the continuous development of economy and the increasingly fierce market competition, consumers' requirements for product quality and appearance are also increasing. Therefore, modern enterprises and brands pay more and more attention to the packaging and display effects of products. Soft film lamination technology plays an important role in the modern packaging and printing industry because it can improve the surface gloss of products, enhance the wear resistance of products, and make them waterproof and moisture-proof.
[0003] OPP (oriented polypropylene) and PET (polyethylene terephthalate) are the two most commonly used materials in modern soft film lamination technology. OPP film occupies an important position in the packaging field due to its high transparency, good stiffness and tensile strength, as well as excellent moisture resistance, oil resistance, chemical resistance and other properties, while PET film is widely used in the fields of screen protection films for electronic products due to its high wear resistance, electrical insulation, flame retardancy and heat aging resistance.
[0004] The main disadvantage of the soft film lamination process at this stage is that over time, the soft film and the pressure-sensitive adhesive in the soft film lamination layer may age, harden or lose viscosity due to the influence of ultraviolet rays, and in severe cases, may cause large pieces of the film to fall off. This not only greatly affects the appearance of the product, but also shortens the service life of the product. In the prior art, ultraviolet absorbers are mixed in the pressure-sensitive adhesive. However, the relative molecular mass of the ultraviolet absorbers in the prior art is low. During the soft film lamination process, surface migration and volatilization often occur. Reducing the concentration of the ultraviolet absorber will lead to a weakened protective effect, and the durability is poor during long-term use. In addition, the soft film used in the field of electronic products may produce corona phenomenon and lead to quality degradation due to long-term contact with static electricity. Therefore, a certain antistatic ability is required. These are all deficiencies in the prior art and need to be solved urgently. Summary of the invention
[0005] The purpose of the present invention is to provide a high-temperature and high-pressure lamination process for soft films made of OPP and PET materials with adhesive backing, by mixing a composite functional agent in a pressure-sensitive adhesive and utilizing the ultraviolet absorption ability of the composite functional agent, the problem of the pressure-sensitive adhesive aging, hardening and losing viscosity due to ultraviolet irradiation is solved, and the antistatic ability of the composite functional agent is utilized to solve the problem of quality degradation caused by the corona phenomenon generated by the soft film due to long-term contact with static electricity.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A high-temperature and high-pressure laminating process for a soft film of OPP or PET material with adhesive backing, comprising the following steps:
[0008] Step 1: Clean, dry, heat treat and shear the prepared OPP / PET soft film;
[0009] Step 2: Mix the pressure-sensitive adhesive and the composite functional agent and evenly apply them on the surface of the substrate;
[0010] Step 3: Place the OPP / PET soft film on the film feeding device of the laminating machine and heat-press it to make the soft film fit tightly to the substrate;
[0011] Step 4: Cold cure the soft film after hot pressing.
[0012] Furthermore, in the first step, the temperature condition of the heat treatment is 150-160° C., and the time condition of the heat treatment is 30-45 min.
[0013] Furthermore, in the second step, the mass ratio of the composite functional agent to the pressure-sensitive adhesive is 0.5-2.5:100.
[0014] Furthermore, in the third step, the running speed of the laminating machine is 4-8 m / min, the temperature condition of the hot pressing treatment is 180-200° C., the pressure of the hot pressing treatment is 3-4 MPa, and the time condition of the hot pressing treatment is 60-75 s.
[0015] Furthermore, the temperature condition for cold treatment curing in the fourth step is 25-30°C.
[0016] Furthermore, the composite functional agent is prepared by the following steps:
[0017] Step 1: 2,4-dihydroxybenzophenone, triethylamine and tetrahydrofuran were mixed in a three-necked flask, magnetic stirring was turned on, and a tetrahydrofuran solution of 2-methyl-4-pyridinecarbonyl chloride was added dropwise to the three-necked flask using a high-pressure dropping pump under ice-water bath conditions. After the addition was completed, the mixture was reacted at 0°C for 5 hours. After the reaction was completed, saturated sodium bicarbonate was added to the three-necked flask for washing. After washing, the organic layer was separated using a separatory funnel, and the intermediate 1 was obtained by rotary evaporation;
[0018] The reaction process is as follows:
[0019]
[0020] Step 2: Mix the intermediate 1, acetonitrile and 4-bromobutyric acid in a three-necked flask, install a thermometer, start magnetic stirring, and react at 20°C for 24 hours. After the reaction is completed, rotary evaporate to obtain the intermediate 2;
[0021] The reaction process is as follows:
[0022]
[0023] Step 3: Mix chitosan oligosaccharides, triethylamine, dimethyl sulfoxide, and PyBop in a three-necked flask, install a thermometer, turn on the magnetic stirring, and slowly add the dimethyl sulfoxide solution of intermediate 2 to the three-necked flask with a high-pressure dropping pump. After the addition is completed, react at a temperature of 30°C for 4 hours. After the reaction is completed, precipitate the product with acetone, filter the precipitated product, wash the precipitate with ultrapure water, and obtain the composite functional agent after drying.
[0024] The reaction process is as follows:
[0025]
[0026] Further, the tetrahydrofuran solution of 2-methyl-4-pyridinecarbonyl chloride in step 1 is prepared from 0.1 mol 2-methyl-4-pyridinecarbonyl chloride and 40 g tetrahydrofuran, and the amount ratio of 2,4-dihydroxybenzophenone, triethylamine, tetrahydrofuran, and 2-methyl-4-pyridinecarbonyl chloride tetrahydrofuran solution used in step 1 is 0.1-0.11 mol: 0.1 mol: 80-100 g: 55.6 g.
[0027] Furthermore, the usage ratio of the intermediate 1, acetonitrile and 4-bromobutyric acid used in step 2 is 0.04 mol:80-100 g:0.04-0.045 mol.
[0028] Furthermore, the dimethyl sulfoxide solution of intermediate 2 in step 3 is prepared from 0.03 mol intermediate 2 and 20 g dimethyl sulfoxide, and the amount ratio of chitosan oligosaccharide, triethylamine, dimethyl sulfoxide, PyBop, and dimethyl sulfoxide solution of intermediate 2 used in step 3 is 20 g: 0.03 mol: 130-150 g: 0.1 g: 35.2 g.
[0029] Beneficial effects of the present invention:
[0030] 1) The present invention provides a high-temperature and high-pressure lamination process for soft films of OPP and PET materials with adhesive backing. The process effectively solves the problem of aging, hardening and degumming of the pressure-sensitive adhesive due to long-term exposure to ultraviolet light, and the problem of corona phenomenon caused by long-term contact of the soft film with an electrostatic environment, resulting in quality degradation. The amount of the composite functional agent added is small, which will not affect the effect of the pressure-sensitive adhesive. The process can be widely used in the packaging industry, advertising light billboards, and electrical appliance housings.
[0031] 2) The present invention uses 2,4-dihydroxybenzophenone and 2-methyl-4-pyridinecarbonyl chloride as raw materials and triethylamine as an acid-binding agent to obtain an intermediate 1 through an esterification reaction, and then uses the intermediate 1 and 4-bromobutyric acid to react with a quaternary ammonium salt to obtain a quaternary ammonium salt intermediate 2 having a -COOH structure, and finally reacts the -COOH of the intermediate 2 with the -NH 2Under the catalysis of PyBop, an N-acylation reaction occurs to obtain a macromolecular composite functional agent with a quaternary ammonium salt structure. The benzophenone compound has good ultraviolet light absorption capacity because it can undergo keto / enol isomerization with the ortho-hydroxyl group under ultraviolet light irradiation. In the present invention, the intermediate 2 and chitosan oligosaccharide are combined in a grafting manner to obtain a composite functional agent. The composite functional agent obtained in this manner retains the ultraviolet light absorption capacity and has good compatibility with polymer materials (pressure-sensitive adhesives), and the durability is greatly improved. In addition, the composite functional agent also has a quaternary ammonium salt structure. After being blended with the base resin (pressure-sensitive adhesive), this type of polymer quaternary ammonium salt compound can be evenly and finely dispersed into linear or mesh-shaped "conductive channels", releasing the static charge in the system, effectively reducing the surface resistance of the blend, and having permanent antistatic properties. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A composite functional agent is prepared by the following steps:
[0035] Step 1: 0.1 mol 2,4-dihydroxybenzophenone, 0.1 mol triethylamine and 80 g tetrahydrofuran are mixed in a container, magnetic stirring is turned on, and 55.6 g 2-methyl-4-pyridinecarbonyl chloride tetrahydrofuran solution is added dropwise to the container under ice-water bath conditions. After the addition is completed, the mixture is reacted at 0°C for 5 hours. After the reaction is completed, saturated sodium bicarbonate is added to the container for washing. After washing, the organic layer is separated with a separatory funnel, and the intermediate 1 is obtained by rotary evaporation. The 2-methyl-4-pyridinecarbonyl chloride tetrahydrofuran solution in the step is prepared from 0.1 mol 2-methyl-4-pyridinecarbonyl chloride and 40 g tetrahydrofuran;
[0036] Step 2: 0.04 mol intermediate 1, 80 g acetonitrile and 0.04 mol 4-bromobutyric acid were mixed in a container, a thermometer was installed, magnetic stirring was turned on, and the reaction was carried out at a temperature of 20°C for 24 hours. After the reaction was completed, intermediate 2 was obtained by rotary evaporation;
[0037] Step 3: Mix 20g of chitosan oligosaccharide, 0.03mol triethylamine, 130g of dimethyl sulfoxide, and 0.1g of PyBop in a container, install a thermometer, turn on magnetic stirring, and slowly add 35.2g of dimethyl sulfoxide solution of intermediate 2 to the container. After the addition is completed, react at a temperature of 30°C for 4h. After the reaction is completed, precipitate the product with acetone, filter the precipitated product, wash the precipitate with ultrapure water, and obtain the composite functional agent after drying.
[0038] Example 2
[0039] A composite functional agent is prepared by the following steps:
[0040] Step 1: 0.105 mol 2,4-dihydroxybenzophenone, 0.1 mol triethylamine and 90 g tetrahydrofuran are mixed in a container, magnetic stirring is turned on, and 55.6 g 2-methyl-4-pyridinecarbonyl chloride tetrahydrofuran solution is added dropwise to the container under ice-water bath conditions. After the addition is complete, the mixture is reacted at 0°C for 5 hours. After the reaction is complete, saturated sodium bicarbonate is added to the container for washing. After washing, the organic layer is separated with a separatory funnel, and the intermediate 1 is obtained by rotary evaporation. The tetrahydrofuran solution of 2-methyl-4-pyridinecarbonyl chloride in the step is prepared from 0.1 mol 2-methyl-4-pyridinecarbonyl chloride and 40 g tetrahydrofuran;
[0041] Step 2: 0.04 mol intermediate 1, 90 g acetonitrile and 0.0425 mol 4-bromobutyric acid were mixed in a container, a thermometer was installed, magnetic stirring was started, and the reaction was carried out at 20°C for 24 h. After the reaction was completed, intermediate 2 was obtained by rotary evaporation;
[0042] Step 3: Mix 20g of chitosan oligosaccharide, 0.03mol triethylamine, 140g of dimethyl sulfoxide, and 0.1g of PyBop in a container, install a thermometer, turn on the magnetic stirring, and slowly add 35.2g of dimethyl sulfoxide solution of intermediate 2 to the container. After the addition is completed, react at a temperature of 30°C for 4h. After the reaction is completed, precipitate the product with acetone, filter the precipitated product, wash the precipitate with ultrapure water, and obtain the composite functional agent after drying.
[0043] Example 3
[0044] A composite functional agent is prepared by the following steps:
[0045] Step 1: 0.11 mol 2,4-dihydroxybenzophenone, 0.1 mol triethylamine and 100 g tetrahydrofuran are mixed in a container, magnetic stirring is turned on, and 55.6 g 2-methyl-4-pyridinecarbonyl chloride tetrahydrofuran solution is added dropwise to the container under ice-water bath conditions. After the addition is complete, the mixture is reacted at 0°C for 5 hours. After the reaction is complete, saturated sodium bicarbonate is added to the container for washing. After washing, the organic layer is separated with a separatory funnel, and the intermediate 1 is obtained by rotary evaporation. The tetrahydrofuran solution of 2-methyl-4-pyridinecarbonyl chloride in the step is prepared from 0.1 mol 2-methyl-4-pyridinecarbonyl chloride and 40 g tetrahydrofuran;
[0046] Step 2: 0.04 mol intermediate 1, 100 g acetonitrile and 0.045 mol 4-bromobutyric acid were mixed in a container, a thermometer was installed, magnetic stirring was turned on, and the reaction was carried out at 20°C for 24 h. After the reaction was completed, intermediate 2 was obtained by rotary evaporation;
[0047] Step 3: Mix 20g of chitosan oligosaccharide, 0.03mol triethylamine, 150g of dimethyl sulfoxide, and 0.1g of PyBop in a container, install a thermometer, turn on magnetic stirring, and slowly add 35.2g of dimethyl sulfoxide solution of intermediate 2 to the container. After the addition is completed, react at a temperature of 30°C for 4h. After the reaction is completed, precipitate the product with acetone, filter the precipitated product, wash the precipitate with ultrapure water, and obtain the composite functional agent after drying.
[0048] Comparative Example 1
[0049] This comparative example is an anti-ultraviolet additive sold by Shanghai Canghong Industrial Co., Ltd.
[0050] The composite functional agent obtained in Examples 1-3 and the anti-ultraviolet additive sold by Shanghai Canghong Industrial Co., Ltd. were mixed with epoxy resin in a ratio of 8-92, and then cured to obtain epoxy resin boards. Four epoxy resin boards were placed in an ultraviolet light environment and irradiated for 24 hours. The color difference of the epoxy resin boards before and after irradiation was tested with the instrument QUV-Spray according to the standard ASTMG154-06, and the yellowness index was calculated according to the standard ASTME313-05. After irradiation with ultraviolet light for 72 hours, the test was performed again and the results were recorded to obtain Table 1:
[0051] project UV irradiation for 24 hours UV irradiation for 72 hours Example 1 1.24 5.21 Example 2 1.21 5.12 Example 3 1.23 5.26 Comparative Example 1 5.49 13.17
[0052] It can be seen from Table 1 that the epoxy resin cured board with the composite functional agent obtained in Examples 1-3 is superior to the epoxy resin cured board with the UV absorber of Comparative Example 1 in both short-term and long-term UV resistance, indicating that the composite functional agent prepared in the present invention has good compatibility with polymer materials, excellent UV resistance, and strong durability.
[0053] Example 4
[0054] A method for preparing a high-temperature and high-pressure laminating process of a soft film of OPP or PET material with adhesive backing, comprising the following steps:
[0055] Step 1: clean the prepared OPP soft film, dry it, heat treat it at 150°C for 30 minutes, and shear it;
[0056] Step 2: Mix the pressure-sensitive adhesive and the composite functional agent obtained in Example 1 in a mass ratio of 100:0.5 and evenly apply the mixture on the surface of the substrate;
[0057] Step 3: Place the OPP soft film on the film feeding device of the laminating machine, set the running speed to 4m / min, and heat-press for 60s at 180℃ to make the soft film fit tightly to the substrate;
[0058] Step 4: Cool the soft film after hot pressing to 25°C for cold treatment and curing.
[0059] Example 5
[0060] A method for preparing a high-temperature and high-pressure laminating process of a soft film of OPP or PET material with adhesive backing, comprising the following steps:
[0061] Step 1: clean the prepared OPP soft film, dry it, heat treat it at 155°C for 37.5min, and shear it;
[0062] Step 2: Mix the pressure-sensitive adhesive and the composite functional agent obtained in Example 2 in a mass ratio of 100:1.5 and evenly apply the mixture on the surface of the substrate;
[0063] Step 3: Place the OPP soft film on the film feeding device of the laminating machine, set the running speed to 6m / min, and heat-press for 67.5s at 190℃ to make the soft film fit tightly to the substrate;
[0064] Step 4: Cool the soft film after hot pressing to 27.5℃ for cold treatment and curing.
[0065] Example 6
[0066] A method for preparing a high-temperature and high-pressure laminating process of a soft film of OPP or PET material with adhesive backing, comprising the following steps:
[0067] Step 1: clean the prepared PET soft film, dry it, heat treat it at 160°C for 45 minutes, and shear it;
[0068] Step 2: Mix the pressure-sensitive adhesive and the composite functional agent obtained in Example 3 in a mass ratio of 100:2.5 and evenly apply the mixture on the surface of the substrate;
[0069] Step 3: Place the PET soft film on the film feeding device of the laminating machine, set the running speed to 8m / min, and heat-press for 75s at 200℃ to make the soft film fit closely to the substrate;
[0070] Step 4: Cool the soft film after hot pressing to 30°C for cold treatment and curing.
[0071] Comparative Example 2
[0072] The second step in Example 6 is changed to "evenly apply the pressure-sensitive adhesive on the surface of the substrate", and the other steps remain unchanged.
[0073] Comparative Example 3
[0074] This comparative example is the PET coated light box sheet sold by Shanghai Huihui Advertising Co., Ltd.
[0075] Comparative Example 4
[0076] This comparative example is the OPP flat protective film sold by Liheng New Material Technology Co., Ltd.
[0077] The soft films of Examples 4-6 and Comparative Examples 2-4 were tested for volume resistivity according to GB / T1410-2006. The test results are shown in Table 2:
[0078]
[0079]
[0080] It can be seen from Table 2 that the resistivity of the soft film after coating in the process of Examples 4-6 in which the composite functional agent obtained in Examples 1-3 is added is much lower than that of Comparative Example 2 in which the composite functional agent is not added and the commercially available Comparative Examples 3-4, indicating that the step of adding the composite functional agent in the coating process of the present invention can effectively reduce the resistance of the material surface to achieve the purpose of releasing the static charge in the system, and can effectively solve the problem of quality degradation caused by the corona phenomenon caused by long-term contact with the electrostatic environment of the insulating material, and can be widely used in the packaging industry, advertising light billboards, electrical housings and other fields.
[0081] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A high temperature and high pressure laminating process for soft films of OPP and PET materials with adhesive backing, comprising the following steps: Step 1: Clean, dry, heat treat and shear the prepared OPP / PET soft film; Step 2: Mix the pressure-sensitive adhesive and the composite functional agent and evenly apply them on the surface of the substrate; Step 3: Place the OPP / PET soft film on the film feeding device of the laminating machine, and heat and press it to make the soft film fit tightly to the substrate; Step 4: Cold cure the soft film after hot pressing; in, The composite functional agent is prepared by the following steps: Step 1, 2,4-dihydroxybenzophenone, triethylamine and tetrahydrofuran are mixed in a container, and a tetrahydrofuran solution of 2-methyl-4-pyridinecarbonyl chloride is added to the container under an ice-water bath condition, and then reacted at a temperature of 0° C. for 5 hours to obtain intermediate 1; Step 2: Mix the intermediate 1, acetonitrile and 4-bromobutyric acid in a container, and react at 20°C for 24 hours to obtain the intermediate 2; Step 3: Add chitosan oligosaccharide, triethylamine, dimethyl sulfoxide and PyBop into a container, add the dimethyl sulfoxide solution of intermediate 2 into the container, and then react at a temperature of 30° C. for 4 hours to obtain the composite functional agent.
2. According to claim 1, a high temperature and high pressure laminating process for soft films of OPP and PET materials with adhesive backing, characterized in that: The temperature condition of the heat treatment in the first step is 150-160° C., and the time condition of the heat treatment is 30-45 min.
3. The high temperature and high pressure laminating process of a soft film of OPP or PET with adhesive backing according to claim 1, characterized in that: In the second step, the mass ratio of the composite functional agent to the pressure-sensitive adhesive is 0.5-2.5:
100.
4. The high temperature and high pressure laminating process of a soft film of OPP or PET with adhesive backing according to claim 1, characterized in that: In the third step, the running speed of the laminating machine is 4-8 m / min, the temperature condition of the hot pressing treatment is 180-200° C., the pressure of the hot pressing treatment is 3-4 MPa, and the time condition of the hot pressing treatment is 60-75 s.
5. The high temperature and high pressure laminating process of OPP and PET soft films with adhesive backing according to claim 1, characterized in that: The temperature condition for cold treatment curing in the fourth step is 25-30°C.
6. The high temperature and high pressure laminating process of OPP and PET soft films with adhesive backing according to claim 1, characterized in that: The tetrahydrofuran solution of 2-methyl-4-pyridinecarbonyl chloride in step 1 is prepared from 0.1 mol of 2-methyl-4-pyridinecarbonyl chloride and 40 g of tetrahydrofuran.
7. The high temperature and high pressure laminating process of OPP and PET soft films with adhesive backing according to claim 1, characterized in that: The amount ratio of 2,4-dihydroxybenzophenone, triethylamine, tetrahydrofuran, and tetrahydrofuran solution of 2-methyl-4-pyridinecarbonyl chloride used in step 1 is 0.1-0.11 mol: 0.1 mol: 80-100 g: 55.6 g.
8. The high temperature and high pressure laminating process of OPP and PET soft films with adhesive backing according to claim 1, characterized in that: The amount ratio of the intermediate 1, acetonitrile and 4-bromobutyric acid used in step 2 is 0.04 mol: 80-100 g: 0.04-0.045 mol.
9. The high temperature and high pressure laminating process of OPP and PET soft films with adhesive backing according to claim 1, characterized in that: The dimethyl sulfoxide solution of intermediate 2 in step 3 is prepared from 0.03 mol of intermediate 2 and 20 g of dimethyl sulfoxide.
10. The high temperature and high pressure laminating process of OPP and PET soft films with adhesive backing according to claim 1, characterized in that: The amount ratio of chitosan oligosaccharide, triethylamine, dimethyl sulfoxide, PyBop, and dimethyl sulfoxide solution of intermediate 2 used in step 3 is 20g: 0.03mol: 130-150g: 0.1g: 35.2g.