Multi-mode, multi-band and multi-stage anti-counterfeiting device and preparation method thereof

By using the combination of indium tin oxide coated glass, thermally responsive photonic crystal gel layer and carbon-carbon double-bond modified glass layer in optical anti-counterfeiting technology, multi-band changes from visible light to long-wave infrared band are achieved, and the existing technology is solved The limitations of medium single or secondary anti-counterfeiting have achieved multi-modal, multi-band and three-level anti-counterfeiting effects, significantly improving the security and recognition of anti-counterfeiting devices.

CN119078394APending Publication Date: 2024-12-06WUHAN XINGUANG TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411318555.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing optical anti-counterfeiting technology only realizes single or secondary anti-counterfeiting in the visible light band, which cannot meet higher-level security needs, and is limited by reflection and fluorescence modes, multi-modal, multi-band and third-level anti-counterfeiting cannot be achieved.

Method used

Multimodal, multi-band and multi-stage anti-counterfeiting devices consisting of indium tin oxide coated glass, thermally responsive photonic crystal gel layer and carbon-carbon double-bond modified glass layer are used to achieve multi-modal, multi-band from visible light to long-wave infrared band through temperature stimulation. Band changes and achieve multi-stage anti-counterfeiting effects in reflection, emission and transmission modes.

Benefits of technology

It realizes multi-band changes from visible light to long-wave infrared bands, has three-level anti-counterfeiting effects, and each band changes independently and does not interfere with each other, which significantly improves the security and recognition of anti-counterfeiting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119078394A_ABST
    Figure CN119078394A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of optical anti-counterfeiting, in particular to a multi-mode, multi-band and multi-stage anti-counterfeiting device and a preparation method thereof, and the multi-mode, multi-band and multi-stage anti-counterfeiting device sequentially comprises indium tin oxide coated glass, a thermal response photonic crystal gel layer and a carbon-carbon double bond modified glass layer from outside to inside. Compared with the existing anti-counterfeiting technology, the multi-mode, multi-band and multi-level anti-counterfeiting device has the advantages that multi-band from visible light to long-wave infrared band and multi-level anti-counterfeiting in reflection, emission and transmission mode change can be realized, and most importantly, three-level anti-counterfeiting is realized. The change of the emission mode does not influence the color change of the visible light wave band, and each wave band changes independently and does not interfere with each other.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical anti-counterfeiting, and in particular to a multi-modal, multi-band and multi-level anti-counterfeiting device and a preparation method thereof. Background Art

[0002] In today's global society, counterfeiting has become a widely discussed and concerned issue. The harmful effects of counterfeit and substandard products on human health, socio-economic activities, and national security have caused deep concern in academia and industry. Therefore, effective anti-counterfeiting strategies are particularly critical. They not only help to protect the legitimate rights and interests of consumers, but also help to create an honest market environment, thereby promoting the realization of sustainable development goals and maintaining social stability. In this complex and urgent context, it is particularly important to deeply explore and promote the effectiveness and efficiency of anti-counterfeiting strategies.

[0003] Optical anti-counterfeiting technology can be realized by using luminescent materials, optically variable devices and responsive photonic crystals. It has the characteristics of good concealment, low imitation and high recognition, and has attracted widespread attention. Responsive photonic crystals can adjust their structural parameters such as lattice spacing d, refractive index n and diffraction angle θ through external stimuli, thereby achieving controllable adjustment of optical properties, which provides great potential for enhancing security and authenticity verification. However, the common responsive photonic crystals reported so far usually only have a single security feature, such as color change, which cannot meet the anti-counterfeiting market's demand for higher levels of security. Recently, many researchers have begun to explore new methods to integrate luminescent materials with photonic crystal structural colors to improve the anti-counterfeiting effect of products. Although these current technologies provide ideas for the design of new anti-counterfeiting materials, they are still limited to the visible light band and only achieve primary and secondary anti-counterfeiting in reflection mode and fluorescence mode.

[0004] Therefore, how to propose an optical anti-counterfeiting technology that can achieve multi-modal response, multi-band changes and third-level anti-counterfeiting (arbitration anti-counterfeiting) has become a problem that needs to be solved urgently. Summary of the invention

[0005] One of the purposes of the present invention is to provide a multi-modal, multi-band and multi-level anti-counterfeiting device that can achieve multi-band from visible light to long-wave infrared bands, and multi-level anti-counterfeiting in reflection, emission and transmission mode changes.

[0006] The second object of the present invention is to provide a method for preparing a multi-modal, multi-band and multi-level anti-counterfeiting device, which is simple and easy to control.

[0007] The solution adopted by the present invention to achieve one of the purposes is: a multi-modal, multi-band and multi-level anti-counterfeiting device, which includes, from the outside to the inside, indium tin oxide coated glass, a thermally responsive photonic crystal gel layer and a carbon-carbon double bond modified glass layer.

[0008] Preferably, when the anti-counterfeiting device is in reflection mode, the temperature in the visible light band will cause the color of the photonic crystal to change, which can be used as a primary anti-counterfeiting device.

[0009] Preferably, the anti-counterfeiting device is in the emission mode, in the long-wave infrared band, and the infrared camera can identify the emissivity of the ITO-coated glass and the modified glass layer, thereby having a secondary anti-counterfeiting effect.

[0010] Preferably, in the transmission mode, the transmission spectrum of the anti-counterfeiting device changes due to temperature stimulation, and the spectrum is recorded and the transmittance (T lum ) and the transmittance (T sol ), and then calculate the light modulation capability (ΔT lum ) and the light modulation capability in the sunlight band (ΔT sol ,) has three-level anti-counterfeiting effect.

[0011] Preferably, the formula is T lum / sol =∫φ lum / sol T(λ)dλ / ∫φ lum / sol dλ calculates the light transmittance in different bands; using the public ΔT lum / sol =T lum / sol,20℃ -T lum / sol,40℃ Calculate the optical modulation capability ΔT of the corresponding band lum and ΔT sol , T(λ) represents the transmittance when the wavelength of incident light is λ;

[0012] φlum(λ) represents the standard visual efficiency function of the human eye;

[0013] φsol(λ) represents the standard solar spectrum irradiance.

[0014] The solution adopted by the present invention to achieve the second purpose is: a method for preparing the multi-modal, multi-band and multi-level anti-counterfeiting device, comprising the following steps:

[0015] (1) uniformly mixing monodispersed superparamagnetic nanocrystal cluster core-shell particles with polymerizable thermally responsive functional monomers, an initiator, a crosslinking agent, and a dispersing solvent to obtain a prepolymer solution;

[0016] (2) applying a prepolymer droplet onto a carbon-carbon double bond modified glass surface, initiating polymerization with ultraviolet light, and fixing the thermal responsive gel layer onto the surface of the carbon-carbon double bond modified glass layer by covalent bond grafting;

[0017] (3) placing the product in step (2) in water, performing solvent exchange, and finally encapsulating it with indium tin oxide (ITO) coated glass.

[0018] Preferably, in step (1), the superparamagnetic nanocrystal cluster core-shell particles are 80-300 nm Fe3O4@PVP, and the concentration of the superparamagnetic nanocrystal cluster core-shell particles in the prepolymer solution is 3.7-18.5 mg / mL.

[0019] Preferably, in step (1), the polymerizable thermoresponsive functional substance is N-isopropylacrylamide (NIPAM) or a mixture of NIPAM and a non-thermally responsive monomer, and the non-thermally responsive monomer is at least one of acrylic acid, acrylamide, methyl methacrylate, and hydroxyethyl methacrylate.

[0020] Preferably, in step (1), the initiator is 2-hydroxy-2-methylethylpropiophenone (HMPP), 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, or 2,2-diethoxyacetophenone, the dispersing solvent is ethylene glycol (EG) or dimethyl sulfoxide, the cross-linking agent is ethylene glycol dimethacrylate (EGDMA) or N,N'-methylenebisacrylamide, and the cross-linking agent is 0.5%-4% of the molar amount of the polymerizable thermally responsive functional monomer.

[0021] Preferably, in step (2), the carbon-carbon double bond modified glass is glass treated with piranha solution and then modified in a toluene solution of 3-(methacryloyloxy)propyltrimethoxysilane.

[0022] The advantages of the multi-modal, multi-band and multi-level anti-counterfeiting device of the present invention compared with the existing anti-counterfeiting technology are that it can achieve multi-band from visible light to long-wave infrared bands, and multi-level anti-counterfeiting in reflection, emission and transmission mode changes, and most importantly, it achieves three-level anti-counterfeiting.

[0023] The change of the emission mode of the multi-modal, multi-band and multi-level anti-counterfeiting device of the present invention does not affect the color change of the visible light band, and each band changes independently without interfering with each other. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a field emission scanning electron microscope image of the thermal responsive photonic crystal hydrogel film in Example 1;

[0025] Figure 2 (a) digital photos and (b) spectrograms of the thermally responsive photonic crystal hydrogel film at different temperatures in Example 1;

[0026] Figure 3 is the emission spectrum of the anti-counterfeiting device in Example 1;

[0027] Figure 4The transmission spectra and optical digital photos of the anti-counterfeiting device in Example 1 at different temperatures;

[0028] Figure 5 The transmittance and transmittance change of the anti-counterfeiting device in Example 1 at different temperatures;

[0029] Figure 6 Spectra of the thermally responsive photonic crystal hydrogel film at different temperatures in Example 2;

[0030] Figure 7 Spectra of the thermally responsive photonic crystal hydrogel film at different temperatures in Example 3;

[0031] Figure 8 (a) digital photos and (b) spectrograms of the thermally responsive photonic crystal hydrogel film at different temperatures in Example 4;

[0032] Fig. 9 (a) digital photos and (b) spectrograms of the thermally responsive photonic crystal hydrogel film in Example 5 at different temperatures. DETAILED DESCRIPTION

[0033] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0034] Example 1

[0035] (1) Dispersing superparamagnetic nanocrystal cluster core-shell particles into a prepolymer solution consisting of a thermally responsive functional monomer N-isopropylacrylamide (NIPAM), a crosslinking agent ethylene glycol dimethacrylate (EGDMA), a photoinitiator, and an ethylene glycol solvent to form a prepolymer solution. The concentration of the superparamagnetic nanocrystal cluster core-shell particles in the prepolymer solution is 11.1 mg / mL, and the concentration of EGDMA is 2% of the molar amount of the NIPAM monomer.

[0036] (2) The prepolymer droplets were coated on the carbon-carbon double bond modified glass, a 500 Gs magnetic field was applied, and UV curing was performed for 5 min to fix the thermal responsive photonic crystal gel layer on the carbon-carbon double bond modified glass layer by covalent bond grafting.

[0037] (3) placing the thermally responsive photonic crystal gel layer in step (2) in water for solvent exchange; and finally encapsulating it with indium tin oxide (ITO) coated glass.

[0038] Figure 1This is a field emission scanning electron microscope image of the thermally responsive photonic crystal hydrogel film in Example 1; it can be seen from the figure that the pores in the three-dimensional network structure formed by the gel are relatively large (3-10 μm), providing space for the large-volume expansion and contraction of the gel network. The Fe3O4@PVP CNCs colloidal nanoparticles are arranged in an ordered one-dimensional chain structure with equal spacing in the pores of the gel network, which conforms to the Bragg diffraction equation. By adjusting the lattice spacing d between the particles, its optical properties can be changed, which provides a basis for the design of primary anti-counterfeiting.

[0039] Figure 2 The (a) digital photo and (b) spectrum of the thermal responsive photonic crystal hydrogel film in Example 1 at different temperatures; it can be seen from the figure that when the temperature rises from 29.0℃ to 30.7℃, the color of the sample gradually changes from red to blue; the diffraction wavelength lmax gradually blue-shifts from 633nm to 437nm, and its change covers the entire visible light band. This shows that in the reflection mode, the visible light band (380~780nm) has a good first-level anti-counterfeiting effect.

[0040] Figure 3 This is the emission spectrum of the anti-counterfeiting device in Example 1; it can be seen from the figure that the front of the device has a lower emissivity because it is an ITO coating, while the back is ordinary glass, which has a higher emissivity. Therefore, in the emission mode, the long-wave infrared band (8-14μm), the device can be identified by an infrared camera, and has a secondary anti-counterfeiting effect.

[0041] Figure 4 The transmission spectra and optical digital photos of the anti-counterfeiting device in Example 1 at different temperatures are shown in the figure. It can be seen from the figure that at 20°C, the pattern below the device is visible; as the temperature rises to 40°C, PNIPAM undergoes a phase transition, the scattering effect is enhanced, and the device becomes opaque, so the pattern below cannot be observed.

[0042] Figure 5 The transmittance and transmittance change of the anti-counterfeiting device in Example 1 at 20°C and 40°C. It can be seen from the figure that at 20°C, the transmittance of the device in the visible light band (380-780nm) and the entire sunlight band (380-2500nm) are calculated to be 21.5% and 32.5% respectively, and at 40°C, the transmittance of the device in the visible light band (380-780nm) and the entire sunlight band (380-2500nm) are 0.9% and 1.5% respectively; according to the formula, the light modulation rate ΔT of the corresponding band can be obtained lum and ΔT solIn summary, the temperature stimulation causes the change of the device transmittance. Experts use a spectrometer to record its spectrum, and then use the calculation formula to obtain the modulation rate of the device for visible light waves and the entire solar light band. This is the third level of anti-counterfeiting.

[0043] Example 2

[0044] (1) Dispersing superparamagnetic nanocrystal cluster core-shell particles into a prepolymer solution consisting of a thermally responsive functional monomer N-isopropylacrylamide (NIPAM), a crosslinking agent ethylene glycol dimethacrylate (EGDMA), a photoinitiator, and an ethylene glycol solvent to form a prepolymer solution. The concentration of the superparamagnetic nanocrystal cluster core-shell particles in the prepolymer solution is 3.7 mg / mL, and the concentration of EGDMA is 2% of the molar amount of the NIPAM monomer.

[0045] (2) The prepolymer droplets were coated on the carbon-carbon double bond modified glass, a 500 Gs magnetic field was applied, and UV curing was performed for 5 min to fix the thermal responsive photonic crystal gel layer on the carbon-carbon double bond modified glass layer by covalent bond grafting.

[0046] (3) placing the thermally responsive photonic crystal gel layer in step (2) in water, performing solvent exchange, and finally encapsulating it with indium tin oxide (ITO) coated glass.

[0047] Figure 6 Spectra of the thermally responsive photonic crystal hydrogel film in Example 2 at different temperatures; it can be seen from the figure that as the temperature increases from 29.0°C to 30.5°C, the peak position of the reflection peak blue-shifts from 686nm to 496nm.

[0048] Example 3

[0049] (1) Dispersing superparamagnetic nanocrystal cluster core-shell particles into a prepolymer solution consisting of a thermally responsive functional monomer N-isopropylacrylamide (NIPAM), a crosslinking agent ethylene glycol dimethacrylate (EGDMA), a photoinitiator, and an ethylene glycol solvent to form a prepolymer solution. The concentration of the superparamagnetic nanocrystal cluster core-shell particles in the prepolymer solution is 18.5 mg / mL, and the concentration of EGDMA is 2% of the molar amount of the NIPAM monomer.

[0050] (2) The prepolymer droplets were coated on the carbon-carbon double bond modified glass, a 500 Gs magnetic field was applied, and UV curing was performed for 5 min to fix the thermal responsive photonic crystal gel layer on the carbon-carbon double bond modified glass layer by covalent bond grafting.

[0051] (3) placing the thermally responsive photonic crystal gel layer in step (2) in water, performing solvent exchange, and finally encapsulating it with indium tin oxide (ITO) coated glass.

[0052] Figure 7Spectra of the thermally responsive photonic crystal hydrogel film at different temperatures in Example 3; it can be seen from the figure that as the temperature increases from 29.0°C to 30.5°C, the peak position of the reflection peak blue-shifts from 646nm to 484nm.

[0053] Example 4

[0054] (1) Dispersing superparamagnetic nanocrystal cluster core-shell particles into a prepolymer solution consisting of a thermally responsive functional monomer N-isopropylacrylamide (NIPAM), a crosslinking agent ethylene glycol dimethacrylate (EGDMA), a photoinitiator, and an ethylene glycol solvent to form a prepolymer solution. The concentration of the superparamagnetic nanocrystal cluster core-shell particles in the prepolymer solution is 11.1 mg / mL, and the concentration of EGDMA is 0.5% of the molar amount of the NIPAM monomer.

[0055] (2) The prepolymer droplets were coated on the carbon-carbon double bond modified glass, a 500 Gs magnetic field was applied, and UV curing was performed for 5 min to fix the thermal responsive photonic crystal gel layer on the carbon-carbon double bond modified glass layer by covalent bond grafting.

[0056] (3) placing the thermally responsive photonic crystal gel layer in step (2) in water, performing solvent exchange, and finally encapsulating it with indium tin oxide (ITO) coated glass.

[0057] Figure 8 (a) Digital photographs and (b) spectrograms of the thermally responsive photonic crystal hydrogel film at different temperatures in Example 4; it can be seen from the figure that when the temperature increases from 26.5°C to 30.5°C, its color remains almost unchanged, and when the temperature continues to increase from 31.0 to 32.0°C, lmax blue-shifts from 715nm to 527nm.

[0058] Example 5

[0059] (1) Dispersing superparamagnetic nanocrystal cluster core-shell particles into a prepolymer solution consisting of a thermally responsive functional monomer N-isopropylacrylamide (NIPAM), a crosslinking agent ethylene glycol dimethacrylate (EGDMA), a photoinitiator, and an ethylene glycol solvent to form a prepolymer solution. The concentration of the superparamagnetic nanocrystal cluster core-shell particles in the prepolymer solution is 11.1 mg / mL, and the concentration of EGDMA is 4.0% of the molar amount of the NIPAM monomer.

[0060] (2) The prepolymer droplets were coated on the carbon-carbon double bond modified glass, a 500 Gs magnetic field was applied, and UV curing was performed for 5 min to fix the thermal responsive photonic crystal gel layer on the carbon-carbon double bond modified glass layer by covalent bond grafting.

[0061] (3) placing the thermally responsive photonic crystal gel layer in step (2) in water, performing solvent exchange, and finally encapsulating it with indium tin oxide (ITO) coated glass.

[0062] Fig. 9 (a) Digital photos and (b) spectrograms of the thermal responsive photonic crystal hydrogel film in Example 5 at different temperatures; when the temperature is 26.5°C, red can be observed by the naked eye, and the first-order diffraction peak of Bragg diffraction (606nm) is within the visible light range. As the temperature slowly rises to 30.0°C, the structural color changes to blue-purple, and the diffraction peak appears at 405nm. During the entire change process, the photonic crystal structural color shows a high saturation.

[0063] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.

Claims

1. A multi-modal, multi-band and multi-level anti-counterfeiting device, Features: From the outside to the inside, it includes indium tin oxide coated glass, a thermal responsive photonic crystal gel layer and a carbon-carbon double bond modified glass layer.

2. The multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 1, Features: When the anti-counterfeiting device is in reflection mode, the temperature in the visible light band will cause the color of the photonic crystal to change, which can be used as a primary anti-counterfeiting device.

3. The multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 1, Features: When the anti-counterfeiting device is in the emission mode, in the long-wave infrared band, the infrared camera can identify the emissivity of the ITO-coated glass and the modified glass layer, and has a secondary anti-counterfeiting effect.

4. The multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 1, Features: In the transmission mode, the transmission spectrum of the anti-counterfeiting device changes due to temperature stimulation. The spectrum is recorded and the transmittance T in the visible light band is calculated. lum and the transmittance T of the entire sunlight band sol , and then calculate the light modulation capability ΔT in the visible light band lum and the light modulation capability ΔT in the sunlight band sol , with three-level anti-counterfeiting effect.

5. The multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 4, Features: Using formula Calculate the light transmittance in different bands; use the formula ΔT lum / sol =T lum / sol,20℃ -T lum / sol,40℃ Calculate the optical modulation capability ΔT of the corresponding band lum , and ΔT sol , Wherein, T(λ) represents the transmittance when the wavelength of incident light is λ; represents the standard visual efficiency function of the human eye; Represents the standard solar spectrum irradiance.

6. A method for preparing a multi-modal, multi-band and multi-level anti-counterfeiting device as claimed in any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) uniformly mixing monodispersed superparamagnetic nanocrystal cluster core-shell particles with polymerizable thermally responsive functional monomers, an initiator, a crosslinking agent, and a dispersing solvent to obtain a prepolymer solution; (2) applying a prepolymer droplet onto a carbon-carbon double bond modified glass surface, initiating polymerization with ultraviolet light, and fixing a thermally responsive gel layer onto the surface of the carbon-carbon double bond modified glass layer; (3) placing the product in step (2) in water, performing solvent exchange, and finally encapsulating it with indium tin oxide coated glass to obtain the multi-modal, multi-band and multi-level anti-counterfeiting device.

7. The method for preparing the multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 6, Features: In the step (1), the superparamagnetic nanocrystal cluster core-shell particles are Fe 3 O 4 @PVP, the particle size range is 80-300nm, and the concentration of superparamagnetic nanocrystal core-shell particles in the prepolymer solution is 3.7-18.5mg / mL.

8. The method for preparing the multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 6, Features: In the step (1), the polymerizable thermally responsive functional monomer is N-isopropylacrylamide or a mixture of N-isopropylacrylamide and a non-thermally responsive monomer, and the non-thermally responsive monomer is at least one of acrylic acid, acrylamide, methyl methacrylate, and hydroxyethyl methacrylate.

9. The method for preparing the multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 6, Features: In the step (1), the initiator is at least one of 2-hydroxy-2-methylethylpropiophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, and 2,2-diethoxyacetophenone; the dispersing solvent is at least one of ethylene glycol and dimethyl sulfoxide; the crosslinking agent is at least one of ethylene glycol dimethacrylate and N,N'-methylenebisacrylamide; and the crosslinking agent is 0.5%-4% of the molar amount of the polymerizable thermally responsive functional monomer.

10. The method for preparing the multi-modal, multi-band and multi-level anti-counterfeiting device according to claim 6, Features: In the step (2), the carbon-carbon double bond modified glass is glass treated with piranha solution and then modified in a toluene solution of 3-(methacryloyloxy)propyltrimethoxysilane.

Citation Information

Patent Citations

  • Thermochromic photonic crystal film in body temperature region and preparation method thereof

    CN110734527A

  • Flexible photonic crystal material with temperature / voltage response discoloration and preparation method thereof

    CN113386437A

  • RECOMBINANT EXTRACELLULAR DOMAIN OF IgE Fc RECEPTOR SUBUNIT ALPHA, PHARMACEUTICAL COMPOSITION COMPRISING SAME AND METHOD FOR PREPARING SAME

    KR102038675B1

  • Optical Anti-counterfeiting element and manufacturing method therefor, and optical Anti-counterfeiting product

    WO2020010885A1