Hollow molecular sieve with AEL structure as well as preparation method and application of hollow molecular sieve
By preparing AEL structure hollow molecular sieve with micropores and mesopores, the diffusion restriction caused by the micropore structure of the molecular sieve is solved, the selectivity and activity of the catalyst is improved, the catalyst life is extended, and the catalyst is shown in the heterogeneous catalytic reaction. Excellent application value.
Patent Information
- Application Number
- CN202411074470.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-06
AI Technical Summary
The microporous structure of the molecular sieve leads to limited diffusion of substances, affecting the activity and selectivity of the catalyst, and the catalyst life is short, especially in heterogeneous catalytic reactions.
Using the preparation method of hollow molecular sieve with AEL structure, the nano molecular sieve is used as the parent body by post-treatment method, and organic amine is added for heating treatment to form hollow molecular sieve with microporous and mesoporous AEL structure to improve the selectivity and activity of the catalyst.
It improves the selectivity and activity of the catalyst, extends the life of the catalyst, and shows excellent application value in heterogeneous catalytic reactions, and has the advantages of simple operation steps, low cost and environmentally friendly.
Smart Images

Figure CN119080023A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of molecular sieve porous materials, and in particular to a hollow molecular sieve with an AEL structure and a preparation method and application thereof. Background Art
[0002] Molecular sieves, commonly known as zeolites or zeolite molecular sieves, are an important class of crystalline microporous materials. They are composed of SiO4 tetrahedrons and AlO4 tetrahedrons as basic structural units connected by bridging oxygen. Due to their regular pore structure, adjustable active sites, good hydrothermal stability, high specific surface area, large pore volume and other characteristics, they are widely used in many fields, such as adsorption and separation, heterogeneous catalysis, various carriers, ion exchange, host-guest chemistry, etc.
[0003] Among them, AlPO4-11 has Aluminophosphate molecular sieves with AEL (International Molecular Sieve Association designated code) cages and 10-membered ring one-dimensional pore structure (http: / / www.iza-structure.org / databases / ). Because of its uniform and regular pore structure, comparable to the molecular size, it has a huge specific surface area, good hydrothermal stability and weak acid catalytic activity, and can be used as an adsorbent and catalyst carrier.
[0004] However, the micropores of molecular sieves can also bring about the problem of limited material diffusion while selecting their shape. Designing and constructing aluminum phosphate molecular sieves with hollow structures can introduce more mesopores on the basis of the original micropores, improve the diffusion capacity of guest molecules, shorten the mass transfer path, and at the same time give them a large specific surface area, which can expose more active sites, improve the activity and selectivity of the catalyst, solve the problem of diffusion limitation, and increase the life of the catalyst. It has great application prospects in heterogeneous catalysis such as alkane isomerization reactions. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a hollow molecular sieve with an AEL structure and a preparation method and application thereof. By adopting a post-treatment method, a nano molecular sieve is first synthesized as a matrix, and then an organic amine is added for post-treatment. The prepared hollow molecular sieve with an AEL structure has both micropores and mesopores, and has the characteristics of large specific surface area, many exposed active sites, fast diffusion of guest molecules, high mass transfer rate, high mechanical strength, long catalyst life, etc., which can effectively improve the selectivity and activity of the catalyst in a multiphase catalytic reaction.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing a hollow molecular sieve with an AEL structure, comprising the following steps:
[0007] (1) adding an aluminum source, phosphoric acid and a heteroatom-containing compound to deionized water in sequence, adding propylene oxide after stirring in an ice bath, and then adding deionized water and hydrofluoric acid, stirring sufficiently for the first time and then aging to obtain an aged gel;
[0008] (2) immersing the aged gel in a mixed solution of deionized water and a template agent, stirring the mixture for a second time to obtain a hydrogel, drying the mixture for the first time to obtain a xerogel, and grinding the xerogel powder;
[0009] (3) performing a first crystallization on the dry gel powder, separating the solid product, drying the solid product, and grinding it to obtain the nano molecular sieve powder;
[0010] (4) mixing the organic amine solution with the nano molecular sieve powder, heating for a second crystallization, separating the solid product after the second crystallization, drying for a second time, and calcining to obtain the hollow molecular sieve with AEL structure.
[0011] Furthermore, in step (1), the aluminum source is one of crystalline aluminum chloride, pseudo-boehmite or aluminum isopropoxide; the phosphoric acid concentration is 10 to 99 wt%; the hydrofluoric acid concentration is 5 to 70 wt%; and the heteroatom-containing compound is a compound comprising one of Cu, Co, Fe, Mg, Ni, Si or Zn.
[0012] Furthermore, in step (1), the aging temperature is 50-120° C., and the aging time is 0.5-6 h.
[0013] Furthermore, in step (2), the molar ratio of M:Al2O3:P2O5:HF:PO:H2O in the hydrogel is 0-2.0:0.1-1.0:0.02-5.0:0.002-0.5:2.0-150.0:5.0-500; the molar ratio of M:Al2O3:P2O5:HF:PO:H2O in the dry gel is 0-2.0:0.1-1.0:0.02-5.0:0.002-0.5:2.0-150.0:5.0-50; wherein M represents one of the heteroatoms Cu, Co, Fe, Mg, Ni, Si or Zn.
[0014] Furthermore, in step (2), the template is one of di-n-butylamine, diisobutylamine, di-n-propylamine, diisopropylamine, and diethylamine; the molar ratio of the aged gel to deionized water is 1:1 to 200 based on dry gel; and the molar ratio of the aged gel to the template is 1:0.1 to 2.0 based on dry gel.
[0015] Furthermore, in step (3), the temperature of the first crystallization is 80 to 240° C., and the time of the first crystallization is 0.5 to 24 hours.
[0016] Furthermore, in step (4), the organic amine is one of diethylamine, di-n-butylamine, di-n-propylamine, and 1-ethyl-3-methylimidazole hydroxide; the concentration of the organic amine solution is 0.01 to 5 mol / L; and the mass ratio of the molecular sieve powder to the organic amine solution is 1:5.0 to 50.0.
[0017] Furthermore, in step (4), the temperature of the second crystallization is 80-250° C., and the time of the second crystallization is 0.5-36 h; the calcination is carried out under air conditions, the calcination temperature is 400-600° C., and the calcination time is 2-12 h.
[0018] The invention also provides a method for preparing a hollow molecular sieve with an AEL structure and a hollow molecular sieve with an AEL structure.
[0019] The present invention also provides an application of a hollow molecular sieve with an AEL structure in heterogeneous catalysis.
[0020] Compared with the prior art, the present invention has the following advantages and technical effects:
[0021] (1) The present invention uses nanomolecular sieve as a matrix template and performs post-treatment under hydrothermal conditions to prepare a hollow molecular sieve with an AEL structure. First, the nanomolecular sieve is synthesized by a dry gel conversion method, and then it is used as a matrix for post-treatment, and an organic amine is added for heat treatment, and finally a hollow molecular sieve with an AEL structure is prepared. In the preparation method provided by the present invention, the organic amine added during the post-treatment exhibits alkaline properties and plays an etching role. At the same time, the added amines also have a structural guiding effect on the AEL type, thereby playing a role of secondary crystallization. It has the advantages of simple operation steps, low cost, environmental friendliness, and easy industrial application.
[0022] (2) The hollow molecular sieve with AEL structure prepared by the present invention has both micropores and mesopores, and has the characteristics of large specific surface area, many exposed active sites, fast diffusion of guest molecules, high mass transfer rate, high mechanical strength, and long catalyst life. It can effectively improve the selectivity and activity of its catalyst and has excellent application value in the field of catalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0024] Figure 1 The XRD spectrum of the hollow molecular sieve with AEL structure synthesized in Example 1 of the present invention;
[0025] Figure 2 The nitrogen physical adsorption-desorption isotherm and BJH mesopore distribution of the hollow molecular sieve with AEL structure synthesized in Example 1 of the present invention;
[0026] Figure 3 This is a SEM image of the hollow molecular sieve with an AEL structure synthesized in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0032] The present invention provides a method for preparing a hollow molecular sieve with an AEL structure, which specifically comprises the following steps:
[0033] First, prepare the nano molecular sieve matrix template, which is achieved by steps (1)-(3):
[0034] (1) adding an aluminum source, phosphoric acid and a heteroatom-containing compound to deionized water in sequence, stirring in an ice bath, adding propylene oxide and stirring, and continuing to add deionized water and hydrofluoric acid. After the first stirring is sufficient, aging is performed at 50 to 120° C. for 0.5 to 6 hours to obtain an aged gel;
[0035] The aluminum source is one of crystalline aluminum chloride, pseudo-boehmite, and aluminum isopropoxide; the concentration of phosphoric acid is 10 to 99 wt %; the concentration of hydrofluoric acid is 5 to 70 wt %; and the heteroatom-containing compound is a compound including one of Cu, Co, Fe, Mg, Ni, Si or Zn.
[0036] The aging temperature is more preferably 60-100°C, and the aging time is 0.5-6h; the ice bath stirring time is 0.1-2h, and the ice bath stirring speed is 50-600r / min; the first stirring temperature is 15-30°C, the first stirring time is 0.5-4h, and the first stirring speed is 50-600r / min;
[0037] (2) immersing the aged gel in a mixed solution of deionized water and a template agent, stirring the mixture for a second time to obtain a hydrogel, drying the mixture for a first time at 60 to 120° C. for 2 to 12 hours to obtain a xerogel, and grinding the xerogel powder;
[0038] The template agent is one of di-n-butylamine, diisobutylamine, di-n-propylamine, diisopropylamine and diethylamine; the molar ratio of the aged gel to deionized water is 1:1-200 based on dry gel; the molar ratio of the aged gel to the template agent is 1:0.1-2.0 based on dry gel;
[0039] The temperature of the second stirring is 25-50° C., the time of the second stirring is 1-8 hours, and the rotation speed of the second stirring is 50-600 r / min; the temperature of the first drying is 60-120° C., and the drying time is 2-12 hours.
[0040] The molar ratio of M:Al2O3:P2O5:HF:PO:H2O in the hydrogel is 0-2.0:0.1-1.0:0.02-5.0:0.002-0.5:2.0-150.0:5.0-500; the molar ratio of M:Al2O3:P2O5:HF:PO:H2O in the xerogel is 0-2.0:0.1-1.0:0.02-5.0:0.002-0.5:2.0-150.0:5.0-50; wherein M represents one of the heteroatoms Cu, Co, Fe, Mg, Ni, Si or Zn;
[0041] (3) crystallizing the dry gel powder for the first time at 80 to 240° C. for 0.5 to 24 h, separating the solid product, and drying and grinding the solid product to obtain the nano molecular sieve powder;
[0042] The first crystallization temperature is more preferably 120-240°C.
[0043] Secondly, the nanomolecular sieve is used as a matrix template and post-treated under hydrothermal conditions to prepare a hollow molecular sieve with an AEL structure, such as step (4):
[0044] (4) adding an organic amine to the nano molecular sieve powder, heating at 80 to 250° C. for a second crystallization for 0.5 to 36 h, separating the solid product after the second crystallization, drying at 50 to 120° C. for a second time for 1 to 24 h, and then calcining at 400 to 600° C. for 2 to 12 h to obtain a hollow molecular sieve with an AEL structure;
[0045] (5) The organic amine is one of diethylamine (DEA), di-n-butylamine (DBA), di-n-propylamine (DPA), and 1-ethyl-3-methylimidazole hydroxide ([Emim]OH); and the temperature of the second crystallization is more preferably 120-200°C.
[0046] Example 1
[0047] Embodiment 1 of the present invention provides a method for preparing a hollow aluminum phosphate molecular sieve with an AEL structure, which specifically comprises the following steps:
[0048] First, a nano-aluminum phosphate molecular sieve matrix template is prepared by steps (1) to (3):
[0049] (1) 9.7 g of crystalline aluminum chloride and 2.4 g of 85% phosphoric acid were added to 28 g of deionized water in sequence, stirred at 100 r / min in an ice bath for 0.5 h, 18 mL of propylene oxide (PO) was added dropwise, 8.0 g of deionized water and 0.2 g of 40% hydrofluoric acid were added dropwise, stirred for the first time at 100 r / min at 20° C. for 2 h, and aged at 50° C. for 3 h to obtain an aged gel.
[0050] (2) The aged gel was immersed in a mixed solution of 8.0 g of deionized water and 1.0 g of di-n-butylamine, and stirred for a second time at 25°C and 100 r / min for 1 h to obtain aluminum phosphate hydrogel. The aluminum phosphate hydrogel was placed in a mold and dried at 120°C for 2 h to obtain aluminum phosphate xerogel. The aluminum phosphate xerogel powder was obtained by grinding. The molar ratio of Al2O3:P2O5:HF:PO:H2O in the xerogel was 1.0:0.5:0.05:4.0:5.0.
[0051] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the first crystallization was carried out at 110° C. for 6 h before the dry gel powder was taken out. The reactor was cooled, and the product was washed with deionized water for 3 times. The final white solid was dried and ground to obtain nano aluminum phosphate molecular sieve powder.
[0052] Secondly, using the nano aluminum phosphate molecular sieve as a matrix template, post-treatment is performed under hydrothermal conditions to prepare a hollow aluminum phosphate molecular sieve having an AEL structure, as in step (4):
[0053] (4) Add 5.0 g of [Emim]OH aqueous solution (concentration of 0.05 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.20 g of nano aluminum phosphate molecular sieve powder, place in a 110°C oven for secondary crystallization for 6 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid at 100°C for 12 h. Then calcine in an air atmosphere at 400°C for 6 h to obtain an AEL structure hollow aluminum phosphate molecular sieve.
[0054] The AEL hollow aluminum phosphate molecular sieve prepared in Example 1 was characterized. Figures 1 to 3 shown.
[0055] First, the phase of the AEL structure hollow aluminum phosphate molecular sieve crystal prepared in Example 1 was investigated by X-ray powder diffraction (XRD) technology, and the type, purity and crystallinity of the prepared molecular sieve were identified by using the XRD diffraction angle position and intensity. Figure 1 As shown, compared with the PDF standard card of AEL aluminum phosphate molecular sieve configuration, the diffraction peaks are highly consistent, indicating that the prepared molecular sieve is a high-purity AEL topological structure, and the diffraction peaks are sharp, indicating high crystallinity. Among them, strong characteristic diffraction peaks of AEL structure aluminum phosphate molecular sieve appear at 2θ=8.09°, 9.43°, 13.20°, 15.70°, 20.49°, 21.12°, and 23.22°, corresponding to its (110), (020), (200), (130), (310), (002), and (240) crystal planes, respectively.
[0056] Secondly, nitrogen physical adsorption / desorption was used to measure the specific surface area and pore structure properties of the hollow aluminum phosphate molecular sieve with AEL structure synthesized in Example 1 of the present invention. Figure 2As shown by the nitrogen physical adsorption-desorption isotherm and BJH mesopore distribution of the hollow aluminophosphate molecular sieve with AEL structure synthesized in Example 1, according to the classification of IUPAC, the above material belongs to the typical type I+IV adsorption isotherm characteristics. The adsorption capacity increases rapidly with the slight change of relative pressure at 0.0 < P / P0 < 0.1, which is related to micropore filling; while at 0.1 < P / P0 < 0.9, it presents a plateau region, and the adsorption capacity changes slowly with the relative pressure, indicating a microporous structure with monolayer or quasi-monolayer adsorption; at 0.9 < P / P0 < 1.0, due to capillary condensation, an H4-type hysteresis loop appears, indicating that the material has mesoporous characteristics. This shows that the hollow aluminophosphate molecular sieve with AEL structure synthesized in Example 1 has both micropores and mesopores, and the specific surface area is 192m 2 / g. In addition, the results of the BJH mesopore distribution diagram are consistent with the nitrogen physical adsorption diagram, and mesopores exist in the range of 2 - 50 nm.
[0057] Figure 3 Figure 6 is an image of the hollow aluminophosphate molecular sieve with AEL structure synthesized in Example 1 of the present invention analyzed by scanning electron microscopy (SEM), and the scale bar is 4 μm. As Figure 3 shown, it can be observed that the hollow aluminophosphate molecular sieve with AEL structure synthesized in Example 1 is composed of nanoscale square crystals stacked together, with a rough surface, and the different light and dark contrasts show a hollow structure.
[0058] Example 2
[0059] The present invention provides a method for preparing a hollow aluminophosphosilicate molecular sieve with AEL structure, which specifically includes the following steps:
[0060] First, prepare a nanoscale aluminophosphosilicate molecular sieve mother template, which is realized by steps (1)-(3):
[0061] (1) Add 6.04 g of crystalline aluminum chloride, 0.10 g of tetraethyl orthosilicate (TEOS), and 2.4 g of 85% phosphoric acid by mass to 15 g of deionized water in turn. Stir at 200 r / min in an ice bath for 0.5 h, and dropwise add 17.5 mL of propylene oxide (PO). Dropwise add 8.0 g of deionized water and 0.17 g of 40% hydrofluoric acid by mass, and stir for the first time at 200 r / min at 20 °C for 2 h, and age at 80 °C for 2 h to obtain the aged gel.
[0062] (2) The aged gel was immersed in a mixed solution of 5.0 g of deionized water and 1.0 g of di-n-propylamine, and stirred for a second time at 200 r / min at 30°C for 1 h to obtain a silicoaluminophosphate hydrogel. The silicoaluminophosphate hydrogel was placed in a mold and dried for a first time at 90°C for 5 h to obtain a silicoaluminophosphate xerogel. The silicoaluminophosphate xerogel powder was obtained by grinding. The molar ratio of SiO2:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.01:1.0:0.8:0.07:6.0:8.0.
[0063] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 120° C. for 12 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano-silicoaluminophosphate molecular sieve powder.
[0064] Secondly, the nano-silicoaluminophosphate molecular sieve is used as a matrix template and post-treated under hydrothermal conditions to prepare a hollow silicoaluminophosphate molecular sieve having an AEL structure, as in step (4):
[0065] (4) Add 6.0 g of [Emim]OH aqueous solution (concentration of 0.10 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.3 g of nano-silicoaluminophosphate molecular sieve powder, place in a 120°C oven for secondary crystallization for 10 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 90°C for 12 h. Then calcine in an air atmosphere at 550°C for 12 h to obtain an AEL structure hollow silicoaluminophosphate molecular sieve.
[0066] Example 3
[0067] Example 3 of the present invention provides a method for preparing an AEL structure hollow magnesium aluminum phosphate molecular sieve, which specifically comprises the following steps:
[0068] First, a nano magnesium aluminum phosphate molecular sieve matrix template is prepared by steps (1) to (3):
[0069] (1) 5.1 g of aluminum isopropoxide, 0.10 g of magnesium chloride hexahydrate (MgCl2·6H2O) and 2.4 g of 85% phosphoric acid were added to 18 g of deionized water in sequence, and stirred at 300 r / min in an ice bath for 0.8 h. 17.5 mL of propylene oxide (PO) was added dropwise, and 8.0 g of deionized water and 0.17 g of 40% hydrofluoric acid were added dropwise. The mixture was stirred for the first time at 300 r / min at 25°C for 0.5 h, and aged at 90°C for 1 h to obtain an aged gel.
[0070] (2) The aged gel was immersed in a mixed solution of 8.0 g of deionized water and 1.0 g of diisopropylamine, and stirred for a second time at 30° C. and 300 r / min for 4 h to obtain a magnesium aluminum phosphate hydrogel. The magnesium aluminum phosphate hydrogel was placed in a mold and dried for a first time at 100° C. for 12 h to obtain a magnesium aluminum phosphate xerogel, which was ground to obtain a magnesium aluminum phosphate xerogel powder. The molar ratio of MgO:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.01:1.0:0.8:0.07:6.0:10.0.
[0071] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 150° C. for 10 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano magnesium aluminum phosphate molecular sieve powder.
[0072] Secondly, the nano magnesium aluminum phosphate molecular sieve is used as a matrix template and post-treated under hydrothermal conditions to prepare a hollow magnesium aluminum phosphate molecular sieve having an AEL structure, as in step (4):
[0073] (4) Add 7.0 g of [Emim]OH aqueous solution (concentration of 0.15 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, and then add 0.3 g of nano magnesium aluminum phosphate molecular sieve powder, place in a 150°C oven for secondary crystallization for 6 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 90°C for 12 h. Then calcine in an air atmosphere at 500°C for 8 h to obtain an AEL structure hollow magnesium aluminum phosphate molecular sieve.
[0074] Example 4
[0075] Example 4 of the present invention provides a method for preparing an AEL structure hollow cobalt aluminum phosphate molecular sieve, which specifically comprises the following steps:
[0076] First, a nano-cobalt aluminum phosphate molecular sieve matrix template is prepared by steps (1) to (3):
[0077] (1) 5.1 g of aluminum isopropoxide, 0.24 g of cobalt chloride hexahydrate (CoCl2·6H2O) and 2.4 g of 85% phosphoric acid were added to 13 g of deionized water in sequence, and stirred at 400 r / min in an ice bath for 0.5 h. 17.5 mL of propylene oxide (PO) was added dropwise, and 8.0 g of deionized water and 0.25 g of 40% hydrofluoric acid were added dropwise. The mixture was stirred at 400 r / min at 30°C for the first time for 1 h, and aged at 60°C for 3 h to obtain an aged gel.
[0078] (2) The aged gel was immersed in a mixed solution of 8.0 g of deionized water and 1.0 g of diisobutylamine, and stirred for a second time at 40°C and 400 r / min for 2 h to obtain cobalt aluminum phosphate hydrogel. The cobalt aluminum phosphate hydrogel was placed in a mold and dried for a first time at 110°C for 12 h to obtain cobalt aluminum phosphate xerogel, which was ground to obtain cobalt aluminum phosphate xerogel powder. The molar ratio of Co2O3:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.04:1.0:0.8:0.1:6.0:7.0.
[0079] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 200° C. for 24 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano-cobalt aluminum phosphate molecular sieve powder.
[0080] Secondly, using the nano-cobalt aluminum phosphate molecular sieve as a matrix template, post-treatment is performed under hydrothermal conditions to prepare a hollow cobalt aluminum phosphate molecular sieve having an AEL structure, as in step (4):
[0081] (4) Add 7.0 g of DBA solution (concentration of 0.15 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.3 g of nano cobalt aluminum phosphate molecular sieve powder, place in a 160° C. oven for secondary crystallization for 18 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 90° C. for 12 h. Then calcine at 550° C. in an air atmosphere for 4 h to obtain an AEL structure hollow cobalt aluminum phosphate molecular sieve.
[0082] Example 5
[0083] Example 5 of the present invention provides a method for preparing an AEL structure hollow aluminum zinc phosphate molecular sieve, which specifically comprises the following steps:
[0084] First, a nano zinc aluminum phosphate molecular sieve matrix template is prepared by steps (1) to (3):
[0085] (1) 5.1 g of aluminum isopropoxide, 0.45 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 2.4 g of 85% phosphoric acid were added to 15 g of deionized water in sequence, stirred at 500 r / min in an ice bath for 0.5 h, 17.5 mL of propylene oxide (PO) was added dropwise, 8.0 g of deionized water and 0.25 g of 40% hydrofluoric acid were added dropwise, stirred at 500 r / min at 30°C for the first time for 1 h, and aged at 80°C for 3 h to obtain an aged gel.
[0086] (2) The aged gel was immersed in a mixed solution of 8.0 g of deionized water and 1.0 g of diethylamine, and stirred for a second time at 40°C and 500 r / min for 2 h to obtain zinc aluminum phosphate hydrogel. The zinc aluminum phosphate hydrogel was placed in a mold and dried for a first time at 100°C for 12 h to obtain zinc aluminum phosphate xerogel, which was ground to obtain zinc aluminum phosphate xerogel powder. The molar ratio of ZnO:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.03:1.0:0.8:0.1:6.0:7.0.
[0087] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 200° C. for 12 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano zinc aluminum phosphate molecular sieve powder.
[0088] Secondly, using the nano zinc aluminum phosphate molecular sieve as a matrix template, post-treatment is performed under hydrothermal conditions to prepare a hollow zinc aluminum phosphate molecular sieve having an AEL structure, as in step (4):
[0089] (4) Add 5.0 g DEA solution (concentration of 0.20 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.3 g of nano zinc aluminum phosphate molecular sieve powder, place in a 160°C oven for secondary crystallization for 8 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 90°C for 12 h. Then calcine in an air atmosphere at 600°C for 4 h to obtain an AEL structure hollow zinc aluminum phosphate molecular sieve.
[0090] Example 6
[0091] Example 6 of the present invention provides a method for preparing an AEL structure hollow nickel aluminum phosphate molecular sieve, which specifically comprises the following steps:
[0092] First, prepare a nano nickel aluminum phosphate molecular sieve matrix template, which is achieved by steps (1)-(3):
[0093] (1) 4.82 g of crystalline aluminum chloride, 0.37 g of nickel acetate (NiC4H6O4·4H2O) and 2.4 g of 85% phosphoric acid were added to 15 g of deionized water in sequence, stirred at 200 r / min in an ice bath for 0.5 h, 17.5 mL of propylene oxide (PO) was added dropwise, 8.0 g of deionized water and 0.25 g of 40% hydrofluoric acid were added dropwise, stirred for the first time at 200 r / min at 30°C for 1 h, and aged at 60°C for 3 h to obtain an aged gel.
[0094] (2) The aged gel was immersed in a mixed solution of 8.0 g of deionized water and 1.0 g of diethylamine, and stirred for a second time at 200 r / min at 40°C for 2 h to obtain nickel aluminum phosphate hydrogel. The nickel aluminum phosphate hydrogel was placed in a mold and dried for a first time at 120°C for 6 h to obtain nickel aluminum phosphate xerogel. The nickel aluminum phosphate xerogel powder was obtained by grinding. The molar ratio of Ni2O3:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.06:0.8:0.8:0.1:6.0:7.0.
[0095] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 200° C. for 12 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano nickel aluminum phosphate molecular sieve powder.
[0096] Secondly, using the nano nickel aluminum phosphate molecular sieve as a matrix template, post-treatment is performed under hydrothermal conditions to prepare a hollow nickel aluminum phosphate molecular sieve having an AEL structure, as in step (4):
[0097] (4) Add 5.0 g of DEA solution (concentration of 0.30 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.3 g of nano nickel aluminum phosphate molecular sieve powder, place in a 180°C oven for secondary crystallization for 10 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 90°C for 12 h. Then calcine in an air atmosphere at 600°C for 4 h to obtain an AEL structure hollow nickel aluminum phosphate molecular sieve.
[0098] Example 7
[0099] Example 1 of the present invention provides a method for preparing an AEL structure hollow nickel aluminum phosphate molecular sieve, which specifically comprises the following steps:
[0100] First, prepare a nano nickel aluminum phosphate molecular sieve matrix template, which is achieved by steps (1)-(3):
[0101] (1) 5.43 g of crystalline aluminum chloride, 0.75 g of nickel acetate (NiC4H6O4·4H2O) and 2.4 g of 85% phosphoric acid were added to 18 g of deionized water in sequence, stirred at 200 r / min in an ice bath for 1 h, 26 mL of propylene oxide (PO) was added dropwise, 8.0 g of deionized water and 0.25 g of 40% hydrofluoric acid were added dropwise, stirred for the first time at 200 r / min at 30°C for 2 h, and aged at 60°C for 3 h to obtain an aged gel.
[0102] (2) The aged gel was immersed in a mixed solution of 8.0 g of deionized water and 1.0 g of diisobutylamine, and stirred for a second time at 200 r / min at 40°C for 2 h to obtain nickel aluminum phosphate hydrogel. The nickel aluminum phosphate hydrogel was placed in a mold and dried for a first time at 120°C for 6 h to obtain nickel aluminum phosphate xerogel. The nickel aluminum phosphate xerogel powder was obtained by grinding. The molar ratio of Ni2O3:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.12:0.9:0.8:0.1:9.0:10.0.
[0103] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 180° C. for 12 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano nickel aluminum phosphate molecular sieve powder.
[0104] Secondly, using the nano nickel aluminum phosphate molecular sieve as a matrix template, post-treatment is performed under hydrothermal conditions to prepare a hollow nickel aluminum phosphate molecular sieve having an AEL structure, as in step (4):
[0105] (4) Add 5.0g DPA solution (concentration of 0.30mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.3g of nano nickel aluminum phosphate molecular sieve powder, place in a 160°C oven for secondary crystallization for 10h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 90°C for 12h. Then calcine in an air atmosphere at 600°C for 4h to obtain AEL structure hollow nickel aluminum phosphate molecular sieve.
[0106] Example 8
[0107] Embodiment 8 of the present invention provides a method for preparing an AEL structure hollow silicoaluminophosphate molecular sieve, which specifically comprises the following steps:
[0108] First, a nano-silicoaluminophosphate molecular sieve matrix template is prepared by steps (1) to (3):
[0109] (1) 3.62 g of crystalline aluminum chloride, 0.045 g of white carbon black and 3.46 g of 85% phosphoric acid were added to 20 g of deionized water in sequence, stirred at 200 r / min in an ice bath for 0.1 h, 26 mL of propylene oxide (PO) was added dropwise, 1.0 g of deionized water and 0.45 g of 40% hydrofluoric acid were added dropwise, stirred at 200 r / min for the first time at 20°C for 2 h, and aged at 90°C for 1 h to obtain an aged gel.
[0110] (2) The aged gel was immersed in a mixed solution of 10.0 g of deionized water and 1.5 g of di-n-propylamine, and stirred for a second time at 200 r / min at 50°C for 6 h to obtain a silicoaluminophosphate hydrogel. The silicoaluminophosphate hydrogel was placed in a mold and dried for a first time at 100°C for 10 h to obtain a silicoaluminophosphate xerogel. The silicoaluminophosphate xerogel powder was obtained by grinding. The molar ratio of SiO2:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.025:1.0:2.0:0.30:15.0:20.0.
[0111] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 180° C. for 12 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano-silicoaluminophosphate molecular sieve powder.
[0112] Secondly, the nano-silicoaluminophosphate molecular sieve is used as a matrix template and post-treated under hydrothermal conditions to prepare a hollow silicoaluminophosphate molecular sieve having an AEL structure, as in step (4):
[0113] (4) Add 10.0 g of DEA solution (concentration of 1 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.3 g of nano-silicoaluminophosphate molecular sieve powder, place in a 180°C oven for secondary crystallization for 10 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 110°C for 12 h. Then calcine in an air atmosphere at 400°C for 12 h to obtain an AEL structure hollow silicoaluminophosphate molecular sieve.
[0114] Example 9
[0115] Example 9 of the present invention provides a method for preparing an AEL structure hollow aluminum iron phosphate molecular sieve, which specifically comprises the following steps:
[0116] First, prepare the nano-aluminum iron phosphate molecular sieve matrix template, which is achieved by steps (1)-(3):
[0117] (1) 3.06 g of aluminum isopropoxide, 0.30 g of ferric nitrate nonahydrate (Fe(NO3)3·9H2O) and 3.46 g of 85% phosphoric acid were added to 27 g of deionized water in sequence, stirred at 350 r / min in an ice bath for 0.1 h, 26 mL of propylene oxide (PO) was added dropwise, 1.0 g of deionized water and 0.45 g of 40% hydrofluoric acid were added dropwise, stirred at 350 r / min for the first time at 20°C for 2 h, and aged at 70°C for 3 h to obtain an aged gel.
[0118] (2) The aged gel was immersed in a mixed solution of 10.0 g of deionized water and 3 g of diisopropylamine, and stirred for a second time at 350 r / min at 50°C for 4 h to obtain aluminum iron phosphate hydrogel. The aluminum iron phosphate hydrogel was placed in a mold and dried for a first time at 80°C for 3 h to obtain aluminum iron phosphate xerogel, which was ground to obtain aluminum iron phosphate xerogel powder. The molar ratio of Fe2O3:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.05:1.0:2.0:0.30:15.0:25.0.
[0119] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 180° C. for 12 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano-aluminum iron phosphate molecular sieve powder.
[0120] Secondly, the nano-aluminum iron phosphate molecular sieve is used as a matrix template and post-treated under hydrothermal conditions to prepare a hollow aluminum iron phosphate molecular sieve with an AEL structure, as in step (4):
[0121] (4) Add 10.0 g of DPA solution (concentration of 0.8 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, then add 0.3 g of nano-aluminum iron phosphate molecular sieve powder, place in a 200°C oven for secondary crystallization for 15 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 100°C for 12 h. Then calcine at 600°C in an air atmosphere for 6 h to obtain an AEL structure hollow aluminum iron phosphate molecular sieve.
[0122] Example 10
[0123] Embodiment 10 of the present invention provides a method for preparing an AEL structure hollow magnesium aluminum phosphate molecular sieve, which specifically comprises the following steps:
[0124] First, a nano magnesium aluminum phosphate molecular sieve matrix template is prepared by steps (1) to (3):
[0125] (1) 5.1 g of aluminum isopropoxide, 0.32 g of magnesium chloride hexahydrate (MgCl2·6H2O) and 2.4 g of 85% phosphoric acid were added to 36 g of deionized water in sequence, stirred at 300 r / min in an ice bath for 0.5 h, 26 mL of propylene oxide (PO) was added dropwise, 8.0 g of deionized water and 0.17 g of 40% hydrofluoric acid were added dropwise, stirred for the first time at 300 r / min at 25°C for 0.5 h, and aged at 90°C for 1 h to obtain an aged gel.
[0126] (2) The aged gel was immersed in a mixed solution of 9.0 g of deionized water and 1.0 g of diethylamine, and stirred for a second time at 30° C. and 300 r / min for 4 h to obtain a magnesium aluminum phosphate hydrogel. The magnesium aluminum phosphate hydrogel was placed in a mold and dried for a first time at 90° C. for 12 h to obtain a magnesium aluminum phosphate xerogel, which was ground to obtain a magnesium aluminum phosphate xerogel powder. The molar ratio of MgO:Al2O3:P2O5:HF:PO:H2O in the xerogel was 0.03:1.0:0.8:0.07:9.0:20.0.
[0127] (3) 1.5 g of dry gel powder was added to a stainless steel reactor with a polytetrafluoroethylene liner, and the mixture was crystallized at 150° C. for 10 h. The reactor was cooled, and the product was washed three times with deionized water. The final white solid was dried and ground to obtain nano magnesium aluminum phosphate molecular sieve powder.
[0128] Secondly, the nano magnesium aluminum phosphate molecular sieve is used as a matrix template and post-treated under hydrothermal conditions to prepare a hollow magnesium aluminum phosphate molecular sieve having an AEL structure, as in step (4):
[0129] (4) Add 7.0 g of [Emim]OH aqueous solution (concentration of 0.5 mol / L) to a stainless steel reactor with a polytetrafluoroethylene liner, and then add 0.3 g of nano magnesium aluminum phosphate molecular sieve powder, place in a 180°C oven for secondary crystallization for 6 h, take out, cool the reactor, and wash the product with deionized water 3 times, and dry the final white solid for a second time at 90°C for 12 h. Then calcine in an air atmosphere at 500°C for 8 h to obtain an AEL structure hollow magnesium aluminum phosphate molecular sieve.
[0130] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a hollow molecular sieve with an AEL structure, characterized in that: The following steps are involved: (1) adding an aluminum source, phosphoric acid and a heteroatom-containing compound to deionized water in sequence, adding propylene oxide after stirring in an ice bath, and then adding deionized water and hydrofluoric acid, stirring sufficiently for the first time and then aging to obtain an aged gel; (2) immersing the aged gel in a mixed solution of deionized water and a template agent, stirring the mixture for a second time to obtain a hydrogel, drying the mixture for the first time to obtain a xerogel, and grinding the xerogel powder; (3) performing a first crystallization on the dry gel powder, separating the solid product, drying the solid product, and grinding it to obtain the nano molecular sieve powder; (4) mixing the organic amine solution with the nano molecular sieve powder, heating for a second crystallization, separating the solid product after the second crystallization, drying for a second time, and calcining to obtain the hollow molecular sieve with AEL structure.
2. The method for preparing the hollow molecular sieve with AEL structure according to claim 1, characterized in that: In step (1), the aluminum source is one of crystalline aluminum chloride, pseudo-boehmite or aluminum isopropoxide; the phosphoric acid concentration is 10-99wt%; the hydrofluoric acid concentration is 5-70wt%; and the heteroatom-containing compound is a compound including one of Cu, Co, Fe, Mg, Ni, Si or Zn.
3. The method for preparing the hollow molecular sieve with AEL structure according to claim 1, characterized in that: In step (1), the aging temperature is 50-120° C., and the aging time is 0.5-6 h.
4. The method for preparing the hollow molecular sieve with AEL structure according to claim 1, characterized in that: In step (2), the molar ratio of M: Al2O3: P2O5: HF: PO: H2O in the hydrogel is 0-2.0: 0.1-1.0: 0.02-5.0: 0.002-0.5: 2.0-150.0: 5.0-500; the molar ratio of M: Al2O3: P2O5: HF: PO: H2O in the xerogel is 0-2.0: 0.1-1.0: 0.02-5.0: 0.002-0.5: 2.0-150.0: 5.0-50; wherein M represents one of the heteroatoms Cu, Co, Fe, Mg, Ni, Si or Zn.
5. The method for preparing the hollow molecular sieve with AEL structure according to claim 1, characterized in that: In step (2), the template is one of di-n-butylamine, diisobutylamine, di-n-propylamine, diisopropylamine and diethylamine; the molar ratio of the aged gel to deionized water is 1:1-200 based on dry gel; the molar ratio of the aged gel to the template is 1:0.1-2.0 based on dry gel.
6. The method for preparing the hollow molecular sieve with AEL structure according to claim 1, characterized in that: In step (3), the temperature of the first crystallization is 80 to 240° C., and the time of the first crystallization is 0.5 to 24 hours.
7. The method for preparing the hollow molecular sieve with AEL structure according to claim 1, characterized in that: In step (4), the organic amine is one of diethylamine, di-n-butylamine, di-n-propylamine, and 1-ethyl-3-methylimidazole hydroxide; the concentration of the organic amine solution is 0.01-5 mol / L; and the mass ratio of the molecular sieve powder to the organic amine solution is 1:5.0-50.
0.
8. The method for preparing the hollow molecular sieve with AEL structure according to claim 1, characterized in that: In step (4), the temperature of the second crystallization is 80-250° C., and the time of the second crystallization is 0.5-36 hours; the calcination is carried out under air conditions, the calcination temperature is 400-600° C., and the calcination time is 2-12 hours.
9. A hollow molecular sieve with an AEL structure prepared by the method for preparing a hollow molecular sieve with an AEL structure as claimed in any one of claims 1 to 8.
10. Use of the hollow molecular sieve with the AEL structure as claimed in claim 9 in heterogeneous catalysis.