Method for efficiently extracting lithium element in lithium iron manganese phosphate positive electrode material by using ammonium persulfate

Through the leaching process of ammonium persulfate and water and multiple reaction steps, combined with ammonia water neutralization and pickling steps, the extraction efficiency and purity of lithium elements in lithium manganese iron phosphate positive electrode material has been successfully improved, and the low efficiency in the existing technology has been solved and environmental pollution problems have achieved efficient recycling and industrial application of lithium elements.

CN119080031APending Publication Date: 2024-12-06QUJING HUAXIANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411241533.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is inefficient when extracting lithium elements in lithium manganese iron phosphate positive electrode material, has a long reaction time, high energy consumption and environmental pollution, making it difficult to meet the needs of industrial production.

Method used

Using the leaching process of ammonium persulfate and water, the lithium element is gradually extracted through multiple reactions and filtration steps, and the impurities are removed by using ammonia water neutralization and pickling steps to finally prepare high-purity lithium hydroxide to achieve a full closed loop of lithium element. Recycle.

Benefits of technology

It has achieved efficient extraction of lithium elements in lithium manganese iron phosphate, with the extraction rate reaching more than 99.6%, and the loss rate is less than 3%. At the same time, environmental pollution is reduced and it is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080031A_ABST
    Figure CN119080031A_ABST
Patent Text Reader

Abstract

The invention discloses a method for efficiently extracting a lithium element in a lithium iron manganese phosphate positive electrode material by using ammonium persulfate, which specifically comprises the following steps: discharging a waste lithium iron manganese phosphate battery, disassembling, sorting and crushing to obtain lithium iron manganese phosphate positive electrode powder, adding ammonium persulfate into the positive electrode powder, and extracting lithium twice to obtain a lithium extraction solution and lithium extraction slag; the lithium extraction slag is continuously washed with water to obtain more lithium in the water washing liquid, the water washing liquid is refluxed for use in the process, and the lithium is enriched in the primary lithium extraction liquid. The primary lithium extraction liquid is neutralized by ammonia water to remove impurities, the neutralization liquid is subjected to barium hydroxide preparation to obtain lithium hydroxide, the primary lithium extraction liquid neutralization slag is further subjected to lithium extraction, lithium is extracted by means of ammonium persulfate leaching / pickling and the like, and the obtained lithium extraction liquid is mixed with the primary lithium extraction liquid to neutralize and remove impurities to prepare lithium hydroxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of resource utilization of solid wastes, and specifically relates to a method for efficiently extracting lithium elements from lithium iron manganese phosphate positive electrode materials by using ammonium persulfate. Background Art

[0002] my country is the world's largest producer and consumer of lithium batteries. It is estimated that by 2025, my country's lithium battery production will reach 1.45TWh. Lithium iron phosphate batteries have the advantages of long life, large capacity, and safe use, and are increasingly used in energy storage, electric vehicles, electronic information and other fields. As an upgraded version of lithium iron phosphate batteries, lithium iron manganese phosphate batteries have attracted much attention due to their high energy density, stable structure and low cost. Therefore, lithium iron manganese phosphate materials are expected to be mass-produced and applied in the future, so a large amount of waste lithium iron manganese phosphate positive electrode powder will be produced. Then the extraction and recycling of lithium elements will become a key factor restricting its further development.

[0003] Currently reported methods for recovering valuable metals from waste lithium iron phosphate batteries include pyrolysis, hydrolysis, solid-liquid combination, mechanochemical, electrochemical, and direct repair methods. These methods can achieve the extraction of lithium elements to a certain extent, but there are problems such as long reaction time, high energy consumption, and serious environmental pollution. However, when it comes to extracting lithium elements from lithium iron phosphate cathode materials containing complex components, the efficiency of these methods is often lower and it is difficult to meet the needs of industrial production. Therefore, developing an efficient, environmentally friendly, and industrially suitable method for extracting lithium elements from lithium iron phosphate cathode materials is of great significance for promoting the application of lithium iron phosphate materials and the development of the lithium-ion battery industry. Summary of the invention

[0004] The present invention provides a method for efficiently extracting lithium from lithium iron manganese phosphate positive electrode materials using ammonium persulfate. The present invention is achieved through the following technical steps: (1) After the waste lithium manganese iron phosphate batteries are discharged, they are disassembled, sorted and crushed to obtain lithium manganese iron phosphate positive electrode powder; (2) adding ammonium persulfate to the positive electrode powder of step (1) at a mass ratio of lithium manganese iron phosphate positive electrode powder to ammonium persulfate of 0.3-1.2:1, and then adding pure water at a liquid-to-solid ratio of 2-4:1, reacting at 20-60° C. for 30-90 min, and filtering to obtain a primary lithium extraction liquid and a primary lithium extraction slag; (3) adding ammonium persulfate to the primary lithium extraction slag obtained in step (2), wherein the amount of ammonium persulfate added is 0.3-0.7 times the mass of the primary lithium extraction slag, and then adding an appropriate amount of pure water at a liquid-solid ratio of 2-4:1, reacting at 20-60° C. for 30-90 min, filtering to obtain a secondary lithium extraction liquid and a secondary lithium extraction slag, and the secondary lithium extraction liquid is refluxed to the primary lithium extraction process for use; (4) The secondary lithium extraction slag is leached with pure water, the liquid-to-solid ratio during the leaching process is 2-4:1, and the reaction is carried out at 20-60°C for 30-90 min, and the tertiary lithium extraction liquid and the tertiary lithium extraction slag are obtained by filtration. The tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use; (5) The primary lithium extraction solution is treated with ammonia water to remove impurities, thereby obtaining a neutralized solution and a neutralized residue, and the neutralized solution is added with barium hydroxide to prepare lithium hydroxide; (6) further extracting lithium from the neutralized slag, adding ammonium persulfate at a mass ratio of 0.3-0.75:1, adding pure water at a liquid-solid ratio of 1.5-3.0:1, reacting at 20-60°C for 1-3 h to obtain a neutralized slag primary lithium extraction liquid and a primary lithium extraction slag, and mixing the neutralized slag primary lithium extraction liquid with the primary lithium extraction liquid after refluxing to remove impurities; (7) The neutralization slag primary lithium extraction slag is acid washed with 0.2-1% acid, with a liquid-to-solid ratio of 2-4:1, and reacted at 20-60°C for 1-3h to obtain a neutralization slag secondary lithium extraction liquid and a secondary lithium extraction slag, and the neutralization slag secondary lithium extraction liquid is refluxed to the neutralization slag primary lithium extraction process for use; (8) The slag is washed with pure water with a liquid-to-solid ratio of 2-4:1, reacted at 20-60°C for 30-90 min, filtered to obtain a neutralization slag tertiary lithium extraction liquid and tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use; (9) The neutralized slag obtained in step (8) is washed with pure water with a liquid-to-solid ratio of 3:1, reacted at 20°C for 30-90 min, filtered to obtain a neutralized slag tertiary lithium extraction liquid and a tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use.

[0005] The acid used in the pickling step in step (7) is nitric acid.

[0006] The concentration of the nitric acid is 0.2-1.0%.

[0007] Beneficial effects of the present invention: 1. Lithium iron manganese phosphate can be selectively leached with lithium element in the process of ammonium persulfate and water leaching system to achieve the purpose of resource recovery.

[0008] 2. The lithium iron manganese phosphate lithium extraction liquid is neutralized with ammonia water without introducing impurities, and lithium hydroxide is prepared from the neutralized liquid; the neutralized slag is further used to extract lithium, realizing a fully closed-loop recovery of lithium elements in lithium iron manganese phosphate; 3. During the lithium extraction process of lithium manganese iron phosphate, only ammonium persulfate and a small amount of nitric acid need to be added, and a single raw material is used. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 is a process flow chart of the present invention; DETAILED DESCRIPTION

[0010] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.

[0011] Embodiment 1: (1) After the waste lithium manganese iron phosphate batteries are discharged, they are disassembled, sorted and crushed to obtain lithium manganese iron phosphate positive electrode powder; (2) adding ammonium persulfate to the positive electrode powder of step (1) at a mass ratio of 0.3-1.2:1, and then adding pure water at a liquid-to-solid ratio of 3:1, reacting at 60° C. for 30 min, and filtering to obtain a primary lithium extraction solution and a primary lithium extraction slag; (3) adding ammonium persulfate to the primary lithium extraction slag obtained in step (2) at a mass ratio of 0.3-0.7:1 between the primary lithium extraction slag and ammonium persulfate, and then adding pure water at a liquid-solid ratio of 3:1, reacting at 60° C. for 30 min, filtering to obtain a secondary lithium extraction liquid and a secondary lithium extraction slag, and refluxing the secondary lithium extraction liquid to the primary lithium extraction process for use; (4) leaching the secondary lithium extraction slag obtained in step (3) with pure water at a liquid-to-solid ratio of 3:1, reacting at 60° C. for 30-90 min, filtering to obtain a tertiary lithium extraction liquid and a tertiary lithium extraction slag, and returning the tertiary lithium extraction liquid to the secondary lithium extraction process for use; (5) After steps (1) to (4), the extraction rate of Li in lithium manganese iron phosphate is ≥99.6%, the Fe loss is ≤3%, the P loss is ≤3%, and the Mn loss is ≤3%; (6) removing impurities from the primary lithium extraction solution obtained in step (2) with aqueous ammonia to obtain a neutralized solution and a neutralized residue, and adding barium hydroxide to the neutralized solution to prepare lithium hydroxide; (7) further extracting lithium from the neutralized slag obtained in step (6), adding 0.3-0.75 times the mass of ammonium persulfate of the neutralized slag, and then adding pure water to make the liquid-solid ratio 1.5:1, reacting at 60° C. for 1 h to obtain a neutralized slag primary lithium extraction liquid and a primary lithium extraction slag, and mixing the neutralized slag primary lithium extraction liquid with the primary lithium extraction liquid after refluxing to remove impurities; (8) washing the neutralized slag obtained in step (7) with 0.2-1.0% nitric acid at a liquid-to-solid ratio of 3:1, reacting at 20° C. for 1 h to obtain a neutralized slag secondary lithium extraction liquid and a secondary lithium extraction slag, and the neutralized slag secondary lithium extraction liquid is refluxed to the neutralized slag primary lithium extraction process for use; (9) The neutralized slag obtained in step (8) is washed with pure water with a liquid-to-solid ratio of 3:1, reacted at 20°C for 30-90 min, filtered to obtain a neutralized slag tertiary lithium extraction liquid and a tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use.

[0012] (10) In the entire process of steps (7) to (-9), the Li extraction rate is ≥99.7%, the Fe loss is ≤3%, the P loss is ≤2%, and the Mn loss is ≤3%; Example 2 (1) After the waste lithium manganese iron phosphate batteries are discharged, they are disassembled, sorted and crushed to obtain lithium manganese iron phosphate positive electrode powder; (2) adding ammonium persulfate in an amount equal to one times the mass of the lithium manganese iron phosphate positive electrode powder to step (1), and then adding pure water to make the liquid-to-solid ratio 3:1, reacting at 20-60° C. for 30-90 min, and filtering to obtain a primary lithium extraction liquid and a primary lithium extraction slag; (3) adding ammonium persulfate in an amount 0.5 times the mass of the primary lithium extraction slag to step (2), and then adding pure water so that the liquid-to-solid ratio is 3:1, reacting at 20-60° C. for 30-90 min, filtering to obtain a secondary lithium extraction liquid and a secondary lithium extraction slag, and refluxing the secondary lithium extraction liquid to the primary lithium extraction process for use; (4) leaching the secondary lithium extraction slag obtained in step (3) with pure water at a liquid-to-solid ratio of 3:1, reacting at 20-60° C. for 30-90 min, filtering to obtain a tertiary lithium extraction liquid and a tertiary lithium extraction slag, and refluxing the tertiary lithium extraction liquid into the secondary lithium extraction process for use; (5) In the entire process of steps (1) to (4), the Li extraction rate is ≥99.5%, the Fe loss is ≤3%, the P loss is ≤2%, and the Mn loss is ≤3%; (6) removing impurities from the primary lithium extraction solution obtained in step (2) with aqueous ammonia to obtain a neutralized solution and a neutralized residue, and adding barium hydroxide to the neutralized solution to prepare lithium hydroxide; (7) further extracting lithium from the neutralized slag obtained in step (6), adding ammonium persulfate in an amount 0.5 times the mass of the neutralized slag, and then adding pure water so that the liquid-to-solid ratio is 1.5:1, reacting at 20-60° C. for 30-90 min to obtain a neutralized slag primary lithium extraction liquid and a primary lithium extraction slag, and mixing the neutralized slag primary lithium extraction liquid with the primary lithium extraction liquid after refluxing to remove impurities; (8) washing the neutralized slag obtained in step (7) with 0.2-1.0% nitric acid at a liquid-to-solid ratio of 3:1, reacting at 20° C. for 1 h to obtain a neutralized slag secondary lithium extraction liquid and a secondary lithium extraction slag, and the neutralized slag secondary lithium extraction liquid is refluxed to the neutralized slag primary lithium extraction process for use; (9) The neutralized slag obtained in step (8) is washed with pure water with a liquid-to-solid ratio of 3:1, reacted at 20-60°C for 30-90 min, filtered to obtain a neutralized slag tertiary lithium extraction liquid and a tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use.

[0013] (10) In the entire process of steps (7) to (-9), the Li extraction rate is ≥99.5%, the Fe loss is ≤3%, the P loss is ≤2%, and the Mn loss is ≤4%; Example 3 (1) After the waste lithium manganese iron phosphate batteries are discharged, they are disassembled, sorted and crushed to obtain lithium manganese iron phosphate positive electrode powder; (2) adding ammonium persulfate to the mixture in step (1) at a mass ratio of lithium manganese iron phosphate positive electrode powder to ammonium persulfate of 0.3-1.2:1, and then adding pure water to make the liquid-solid ratio of 2-4:1, reacting at 60°C for 30 minutes, and filtering to obtain a primary lithium extraction liquid and a primary lithium extraction slag; (3) Adding ammonium persulfate to the first lithium extraction slag in step (2) at a mass ratio of 0.3-1.2:1 to ammonium persulfate, and then adding pure water to make the liquid-solid ratio 2-4:1, reacting at 60°C for 90 minutes, filtering to obtain a secondary lithium extraction liquid and a secondary lithium extraction slag. The secondary lithium extraction liquid is refluxed to the first lithium extraction process for use; (4) leaching the secondary lithium extraction slag obtained in step (3) with pure water at a liquid-to-solid ratio of 2-4:1, reacting at 60° C. for 90 min, filtering to obtain a tertiary lithium extraction liquid and a tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use; (5) In the entire process of steps (1) to (4), the Li extraction rate is ≥99.2%, the Fe loss is ≤2%, the P loss is ≤2%, and the Mn loss is ≤3%; (6) removing impurities from the primary lithium extraction solution obtained in step (2) with aqueous ammonia to obtain a neutralized solution and a neutralized residue, and adding barium hydroxide to the neutralized solution to prepare lithium hydroxide; (7) further extracting lithium from the neutralized slag obtained in step (6), adding ammonium persulfate 1-2 times the mass of the neutralized slag, and then adding pure water so that the liquid-to-solid ratio is 1-3:1, reacting at 60° C. for 90 minutes to obtain a neutralized slag primary lithium extraction liquid and a primary lithium extraction slag, and mixing the neutralized slag primary lithium extraction liquid with the primary lithium extraction liquid after refluxing to remove impurities; (8) washing the neutralized slag obtained in step (7) with 0.2-1.0% nitric acid at a liquid-to-solid ratio of 1-3:1, reacting at 20° C. for 1 h to obtain a neutralized slag secondary lithium extraction liquid and a secondary lithium extraction slag, and the neutralized slag secondary lithium extraction liquid is refluxed to the neutralized slag primary lithium extraction process for use; (9) The neutralized slag obtained in step (8) is washed with pure water with a liquid-to-solid ratio of 1-3:1, reacted at 60°C for 90 min, filtered to obtain a neutralized slag tertiary lithium extraction liquid and a tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use.

[0014] (10) In the entire process of steps (7) to (9), the Li extraction rate is ≥99.4%, the Fe loss is ≤3%, the P loss is ≤2%, and the Mn loss is ≤3%.

Claims

1. A method for efficiently extracting lithium from lithium iron manganese phosphate positive electrode material using ammonium persulfate, characterized in that The following steps are involved: (1) After the waste lithium manganese iron phosphate batteries are discharged, they are disassembled, sorted and crushed to obtain lithium manganese iron phosphate positive electrode powder; (2) adding ammonium persulfate to the positive electrode powder of step (1) at a mass ratio of lithium manganese iron phosphate positive electrode powder to ammonium persulfate of 0.3-1.2:1, and then adding pure water at a liquid-to-solid ratio of 2-4:1, reacting at 20-60° C. for 30-90 min, and filtering to obtain a primary lithium extraction liquid and a primary lithium extraction slag; (3) adding ammonium persulfate to the primary lithium extraction slag obtained in step (2), wherein the amount of ammonium persulfate added is 0.3-0.7 times the mass of the primary lithium extraction slag, and then adding an appropriate amount of pure water at a liquid-solid ratio of 2-4:1, reacting at 20-60° C. for 30-90 min, filtering to obtain a secondary lithium extraction liquid and a secondary lithium extraction slag, and the secondary lithium extraction liquid is refluxed to the primary lithium extraction process for use; (4) The secondary lithium extraction slag is leached with pure water, the liquid-to-solid ratio in the leaching process is 2-4:1, the reaction is carried out at 20-60°C for 30-90 minutes, and the tertiary lithium extraction liquid and the tertiary lithium extraction slag are obtained by filtration. The tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use; (5) The primary lithium extraction solution is treated with ammonia water to remove impurities, thereby obtaining a neutralized solution and a neutralized residue, and the neutralized solution is added with barium hydroxide to prepare lithium hydroxide; (6) further extracting lithium from the neutralized slag, adding ammonium persulfate at a mass ratio of 0.3-0.75:1, adding pure water at a liquid-solid ratio of 1.5-3.0:1, reacting at 20-60°C for 1-3 h to obtain a neutralized slag primary lithium extraction liquid and a primary lithium extraction slag, and mixing the neutralized slag primary lithium extraction liquid with the primary lithium extraction liquid after refluxing to remove impurities; (7) The neutralization slag primary lithium extraction slag is acid washed with 0.2-1% acid, with a liquid-to-solid ratio of 2-4:1, and reacted at 20-60°C for 1-3 h to obtain a neutralization slag secondary lithium extraction liquid and secondary lithium extraction slag, and the neutralization slag secondary lithium extraction liquid is refluxed to the neutralization slag primary lithium extraction process for use; (8) The slag is washed with pure water with a liquid-to-solid ratio of 2-4:1, reacted at 20-60°C for 30-90 min, filtered to obtain a neutralization slag tertiary lithium extraction liquid and tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use; (9) The neutralized slag obtained in step (8) is washed with pure water with a liquid-to-solid ratio of 3:1, reacted at 20°C for 30-90 min, filtered to obtain a neutralized slag tertiary lithium extraction liquid and a tertiary lithium extraction slag, and the tertiary lithium extraction liquid is refluxed to the secondary lithium extraction process for use.

2. The method for efficiently extracting lithium from lithium iron manganese phosphate positive electrode material using ammonium persulfate according to claim 1, characterized in that: The acid used in the pickling step in step (7) is nitric acid.

3. The method for efficiently extracting lithium from lithium iron manganese phosphate positive electrode material using ammonium persulfate according to claim 2, characterized in that: The concentration of the nitric acid is 0.2-1.0%.