Polymerization reaction technology and application of crosslinkable polymer
In the preparation of antireflective coatings, the polymerization reaction was solved by using 2,4-hexabutylphenol or 2,6-di-tert-butyl-4-methylphenol as regulators and polymerization under circulation pump conditions The problems of narrow molecular weight distribution and high conversion rate have achieved safe, environmentally friendly and low-cost crosslinkable polymer preparation, suitable for anti-reflective coatings.
Patent Information
- Application Number
- CN202411348212.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, in the crosslinkable organic polymer required for the preparation of antireflective coatings, the method of narrow molecular weight distribution, high conversion rate, safe, environmentally friendly, low cost, odorless and discolored is difficult to achieve, and the molecular weight PDI is large and heavy. Poor presentation.
A preparation method is adopted, including mixing the initiator, regulator, monomer and solvent, performing polymerization reaction under circulating pump conditions, using 2,4-dimethyl-6-tert-butylphenol or 2 ,6-di-tert-butyl-4-methylphenol is used as a regulator to circulate the reaction liquid through a circulation pump to control the polymerization conditions to obtain a crosslinkable polymer.
The molecular weight PDI of the crosslinkable polymer is achieved, without odor and discoloration, which improves the monomer conversion rate and polymer reproducibility, reduces costs, and meets the application needs of anti-reflective coatings.
Smart Images

Figure CN119081003A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a polymerization reaction technology and application of a cross-linkable polymer. Background Art
[0002] Anti-reflection coating (ARC) is a material that is spin-coated on the interface between photoresist and Si substrate to absorb the reflected light from photolithography. Anti-reflection coatings mainly include: bottom anti-reflection coating, top anti-reflection coating, developable bottom anti-reflection coating, spin-coated Si-containing anti-reflection coating, carbon coating, etc.
[0003] The key components of bottom anti-reflective coating (BARC) materials include cross-linkable resin, thermal acid generator, surfactant and solvent. The polymerization reaction of cross-linkable resin is sensitive to temperature, and the auto-acceleration phenomenon in the polymerization process makes it difficult to achieve precise control of molecular weight and dispersion.
[0004] In order to prepare the cross-linkable organic polymer contained in the low PDI anti-reflective coating composition, researchers have adopted traditional free radical polymerization, anionic polymerization, active free radical polymerization and other approaches. For the free radical polymerization of the organic polymer, the main termination mode is diradical disproportionation termination, which makes it difficult to control the molecular weight and molecular weight distribution of the polymer product. In addition, during the polymerization process, as the viscosity of the system increases, there will be a gel effect, making the molecular weight distribution even more difficult to control.
[0005] The effective method widely used at present is active free radical polymerization. Among them, nitroxide free radical polymerization (NMRP) is essentially a phenomenon of suspended animation polymerization between nitroxide compounds and monomer free radicals during the polymerization process, so that the amount of small molecular free radicals can be better controlled and not terminated by double radicals, avoiding the reaction stopping under the condition of low molecular weight. In this way, the chain segments can be continuously lengthened, so that products with larger molecular weight can be obtained. At the same time, since the combination in the suspended animation state will also break due to the increase in temperature, the generated free radicals will be released again, which can well control the rate of free radical reaction, thereby reducing the molecular weight distribution range in controlling the overall rate of free radical reaction, and at the same time, a larger molecular weight can be produced. Although the nitroxide polymerization system is simple, the product does not require complex post-processing technology, and its control effect is better. However, since this type of polymerization must use a nitroxide reagent, the versatility of the reaction is poor, and it is mainly used in the synthesis of styrene polymers, and is not applicable in the synthesis of cross-linkable organic polymers required for anti-reflective coating compositions.
[0006] Atom transfer radical polymerization (ATRP) uses simple organic halides as initiators and transition metal complexes as halogen atom carriers. Through redox reactions, a reversible dynamic equilibrium is established between active species and dormant species, thereby achieving control over the polymerization reaction. As a polymerization method derived from active polymerization, this method not only enables the relative molecular mass and distribution of the polymer to be precisely controlled, but also can adjust the microstructure of the polymer to obtain block polymers or grafted polymers, etc., and therefore has received more attention. However, the initiators and corresponding high-efficiency catalysts required are expensive, and the amount of catalyst used is too large, which can easily cause environmental pollution, and the subsequent catalyst recovery is difficult. The residue in the polymer can easily cause polymer aging and other side reactions, affecting the application of polymers in the field of anti-reflective coatings.
[0007] Reversible addition-fragmentation chain transfer radical polymerization (RAFT) is a process in which a special chain transfer agent with a high chain transfer constant is added to a conventional free radical polymerization system, so that the growth free radical and the chain transfer agent undergo degenerate transfer, thereby reducing the concentration of free radicals and making it possible to achieve active free radical polymerization. A dithioester derivative SC(Z)SR is usually added as a chain transfer agent. During the polymerization, it forms a dormant intermediate (SC(Z)S-Pn) with the growth chain free radical Pn·, which limits the irreversible diradical termination side reaction between the growth chain free radicals and enables the polymerization reaction to be effectively controlled. This dormant intermediate can cleave itself and release a new active free radical R· from the corresponding sulfur atom, which combines with the monomer to form a growth chain. The rate of addition or cleavage is much faster than the rate of chain growth. The dithioester derivative quickly transfers between the active free radical and the dormant free radical, narrowing the molecular weight distribution, thereby making the polymerization exhibit controllable / "active" characteristics. The biggest advantage of RAFT is that it is applicable to a wide range of monomers, which is very beneficial to the polymerization of olefin monomers containing special functional groups. No expensive reagents are needed, and impurities or residual reagents are not difficult to remove from the polymer product. Not only is the molecular weight distribution narrow, but the molecular design capability is also strong, and it can be used to prepare block, graft, and star copolymers. However, most of its regulators are dithioester derivatives, which may increase the toxicity of the polymer, and the preparation process of dithioester is relatively complicated. It may also give the polymer a certain color and odor, which affects the light absorption characteristics of the polymer, making it difficult to apply to anti-reflective coatings.
[0008] Patent application CN101544709A uses a vulcanization accelerator, diisopropyl xanthate disulfide, as a regulating agent. Although this solves the odor problem, the discoloration problem remains unsolved.
[0009] Patent application CN115197344A uses phenol with a carbon-nitrogen double bond at the ortho position as a regulator to prepare polyvinyl alcohol. The polymerization has good controllability and low cost, and can synthesize polymers with high molecular weight, low toxicity and high safety. However, the conversion rate is low. Prolonging the time can increase the conversion rate, but the PDI increases accordingly.
[0010] Patent application CN113185648A uses methacrylate monomers as comonomers, cobalt complexes as catalysts, adds solvents and initiators to form a reaction system, uses catalytic chain transfer polymerization to synthesize sulfur-free ω-terminated vinyl polymer dispersants, and then conducts sulfur-free RAFT emulsion polymerization to prepare cationic polymer hybrid pigments. The reaction conditions are mild, and the resulting polymer is colorless and odorless, but a cobalt complex is introduced.
[0011] Patent application CN110891980B provides a radical polymerization control agent of anthracene or naphthalene structure with the ability to inhibit radical polymerization, which, in the dark, captures free radicals generated by heat or decomposition and acts as a radical polymerization inhibitor of polymerizable compounds; however, during polymerization, by initiating polymerization while irradiating light of a certain wavelength, the radical polymerization inhibition effect is lost, thereby being able to easily initiate radical polymerization of free radical polymerizable compounds without increasing the amount of free radical polymerization initiator. However, this method requires light control, and the operation is relatively inconvenient.
[0012] Patent CN108948243B regulates the polymerization process under light conditions by the combined action of iodine compounds and Schiff base additives to obtain high molecular weight and low dispersity polymers under light conditions. The upper limit of the maximum molecular weight obtained by this method is higher and the distribution is narrower, but iodine is introduced and light control is also required.
[0013] Patent CN113913075A discloses a cross-linkable polymer and anti-reflective coating composition and a preparation method thereof, but this method has problems such as large molecular weight PDI and poor molecular weight reproducibility.
[0014] Therefore, there is still an urgent need for a cross-linkable organic polymer with low PDI (narrow molecular weight distribution), high conversion rate, safety, environmental protection, low cost, no odor and discoloration, and simple preparation method and a preparation method thereof. Summary of the invention
[0015] In order to solve the above technical problems, the present invention provides the following technical solutions.
[0016] In a first aspect, the present invention provides a method for preparing the cross-linkable polymer.
[0017] A method for preparing the cross-linkable polymer comprises the following steps:
[0018] (1) Material mixing: mixing an initiator, a regulator, a monomer and a solvent to obtain a mixture A; the monomer comprises a monomer represented by formula (II) and an acrylate monomer;
[0019] The structure of the monomer shown in formula (II) is:
[0020]
[0021] in,
[0022] R 1 Selected from substituted or unsubstituted C2~C 10 substituted or unsubstituted C2 alkenyl, substituted or unsubstituted C3 alkenyl, substituted or unsubstituted C4 alkenyl, substituted or unsubstituted C5 alkenyl, substituted or unsubstituted C6 alkenyl, substituted or unsubstituted C7 alkenyl, substituted or unsubstituted C8 alkenyl, substituted or unsubstituted C9 alkenyl, substituted or unsubstituted C 10 alkenyl);
[0023] R 2 With R 3 Each is independently selected from H, substituted or unsubstituted C1-C6 alkyl (e.g., substituted or unsubstituted C1 alkyl, substituted or unsubstituted C2 alkyl, substituted or unsubstituted C3 alkyl, substituted or unsubstituted C4 alkyl, substituted or unsubstituted C5 alkyl, substituted or unsubstituted C6 alkyl), substituted or unsubstituted C6-C 20 substituted or unsubstituted C6 aryl, substituted or unsubstituted C7 aryl, substituted or unsubstituted C8 aryl, substituted or unsubstituted C9 aryl, substituted or unsubstituted C 10 Aryl, substituted or unsubstituted C 11 Aryl, substituted or unsubstituted C 12 Aryl, substituted or unsubstituted C 13 Aryl, substituted or unsubstituted C 14 Aryl, substituted or unsubstituted C 15 Aryl, substituted or unsubstituted C 16 Aryl, substituted or unsubstituted C 17 Aryl, substituted or unsubstituted C 18 Aryl, substituted or unsubstituted C 19 Aryl, substituted or unsubstituted C 20 aryl);
[0024] The acrylic acid ester monomer is a substituted or unsubstituted alkyl acrylate or a substituted or unsubstituted alkyl methacrylate;
[0025] The regulating agent is a compound represented by formula (I),
[0026]
[0027] in,
[0028] R 4 Selected from substituted or unsubstituted C1-C6 alkyl groups (e.g. substituted or unsubstituted C1 alkyl groups, substituted or unsubstituted C2 alkyl groups, substituted or unsubstituted C3 alkyl groups, substituted or unsubstituted C4 alkyl groups, substituted or unsubstituted C5 alkyl groups, substituted or unsubstituted C6 alkyl groups);
[0029] R 5 With R 6 Each is independently selected from H, substituted or unsubstituted C1-C6 alkyl (e.g., substituted or unsubstituted C1 alkyl, substituted or unsubstituted C2 alkyl, substituted or unsubstituted C3 alkyl, substituted or unsubstituted C4 alkyl, substituted or unsubstituted C5 alkyl, substituted or unsubstituted C6 alkyl), substituted or unsubstituted C2-C 10 substituted or unsubstituted C2 alkenyl, substituted or unsubstituted C3 alkenyl, substituted or unsubstituted C4 alkenyl, substituted or unsubstituted C5 alkenyl, substituted or unsubstituted C6 alkenyl, substituted or unsubstituted C7 alkenyl, substituted or unsubstituted C8 alkenyl, substituted or unsubstituted C9 alkenyl, substituted or unsubstituted C 10 alkenyl);
[0030] (2) Polymerization reaction: removing oxygen from the mixture A obtained in step (1), introducing an inert gas or nitrogen, and performing a polymerization reaction at a certain temperature to obtain the cross-linkable polymer.
[0031] In some embodiments, R 1 is selected from the group consisting of substituted or unsubstituted vinyl, allyl, 1-butenyl, 2-butenyl, isobutenyl, 1-pentenyl, 2-pentenyl, 3-methyl-1-butenyl, 2-methyl-2-butenyl, 2,3-dimethyl-2-butenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 1-heptenyl, 2-heptenyl, 3-heptenyl, 1-octenyl, 2-octenyl, 3-octenyl, 1-nonenyl, 2-nonenyl, 3-nonenyl, decenyl, 1-dienyl, 2-dienyl and -3-dienyl.
[0032] In some embodiments, R 4Selected from substituted or unsubstituted C1-C6 straight chain alkyl groups (for example: substituted or unsubstituted C1 straight chain alkyl groups, substituted or unsubstituted C2 straight chain alkyl groups, substituted or unsubstituted C3 straight chain alkyl groups, substituted or unsubstituted C4 straight chain alkyl groups, substituted or unsubstituted C5 straight chain alkyl groups, substituted or unsubstituted C6 straight chain alkyl groups).
[0033] In some embodiments, R 4 Selected from substituted or unsubstituted C1~C6 branched alkyl groups (for example: substituted or unsubstituted C1 branched alkyl groups, substituted or unsubstituted C2 branched alkyl groups, substituted or unsubstituted C3 branched alkyl groups, substituted or unsubstituted C4 branched alkyl groups, substituted or unsubstituted C5 branched alkyl groups, substituted or unsubstituted C6 branched alkyl groups).
[0034] In some embodiments, R 2 With R 3 Each is independently selected from H, substituted or unsubstituted C1-C6 straight chain alkyl (for example: substituted or unsubstituted C1 straight chain alkyl, substituted or unsubstituted C2 straight chain alkyl, substituted or unsubstituted C3 straight chain alkyl, substituted or unsubstituted C4 straight chain alkyl, substituted or unsubstituted C5 straight chain alkyl, substituted or unsubstituted C6 straight chain alkyl).
[0035] In some embodiments, R 2 With R 3 Each is independently selected from H, substituted or unsubstituted C1-C6 branched alkyl (for example: substituted or unsubstituted C1 branched alkyl, substituted or unsubstituted C2 branched alkyl, substituted or unsubstituted C3 branched alkyl, substituted or unsubstituted C4 branched alkyl, substituted or unsubstituted C5 branched alkyl, substituted or unsubstituted C6 branched alkyl).
[0036] In some embodiments, R 2 With R 3Each is independently selected from H, substituted or unsubstituted groups: methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (i-Pr, i-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl propyl, -CH(CH3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1- Butyl (-CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)C H(CH3)CH2CH3), 4-methyl-2-pentyl (-CH(CH3)CH2CH(CH3)2), 3-methyl-3-pentyl (-C(CH3)(CH2CH3)2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 or octyl (-(CH2)7CH3).
[0037] In some embodiments, R 4 Selected from the following substituted or unsubstituted groups: methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (i-Pr, i-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl,
[0038] -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl,
[0039] -CH(CH3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl (-CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH 2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH(CH3)CH2CH3), 4-methyl-2-pentyl (-CH(CH3)CH2CH(CH3)2), 3-methyl-3-pentyl (-C(CH3)(CH2CH3)2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 or octyl (-(CH2)7CH3).
[0040] In some embodiments, R 5 With R 6 each independently selected from H, substituted or unsubstituted C1-C6 straight-chain alkyl (e.g., substituted or unsubstituted C1 straight-chain alkyl, substituted or unsubstituted C2 straight-chain alkyl, substituted or unsubstituted C3 straight-chain alkyl, substituted or unsubstituted C4 straight-chain alkyl, substituted or unsubstituted C5 straight-chain alkyl, substituted or unsubstituted C6 straight-chain alkyl), substituted or unsubstituted C1-C6 branched-chain alkyl (e.g., substituted or unsubstituted C1 branched-chain alkyl, substituted or unsubstituted C2 branched-chain alkyl, substituted or unsubstituted C3 branched-chain alkyl, substituted or unsubstituted C4 branched-chain alkyl, substituted or unsubstituted C5 branched-chain alkyl, substituted or unsubstituted C6 branched-chain alkyl), substituted or unsubstituted C2-C 10substituted or unsubstituted alkenyl groups (e.g., substituted or unsubstituted vinyl, allyl, 1-butenyl, 2-butenyl, isobutenyl, 1-pentenyl, 2-pentenyl, 3-methyl-1-butenyl, 2-methyl-2-butenyl, 2,3-dimethyl-2-butenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 1-heptenyl, 2-heptenyl, 3-heptenyl, 1-octenyl, 2-octenyl, 3-octenyl, 1-nonenyl, 2-nonenyl, 3-nonenyl, decenyl, 1-dienyl, 2-dienyl, and -3-dienyl).
[0041] In some embodiments, R 5 With R 6Each is independently selected from H, substituted or unsubstituted methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (i-Pr, i-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl, -CH(CH3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH 3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl (-CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(C H3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH(CH3)CH2CH3), 4-methyl-2-pentyl (-CH(CH3)CH2CH(CH3)2), 3-methyl-3-pentyl (-C(CH3)(CH2CH3)2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH 7CH3), vinyl, allyl, 1-butenyl, 2-butenyl, isobutenyl, 1-pentenyl, 2-pentenyl, 3-methyl-1-butenyl, 2-methyl-2-butenyl, 2,3-dimethyl-2-butenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 1-heptenyl, 2-heptenyl, 3-heptenyl, 1-octenyl, 2-octenyl, 3-octenyl, 1-nonenyl, 2-nonenyl, 3-nonenyl, decenyl, 1-dienyl, 2-dienyl and -3-dienyl.
[0042] In some embodiments, the mixing method of step (1) includes: dissolving the monomer in a solvent, adding an initiator and a regulator, and stirring evenly.
[0043] In some embodiments, the substituted C2 to C 10 Alkenyl, substituted C1-C6 alkyl and substituted C6-C 20 The substitution in the aryl group independently means that at least one hydrogen atom is replaced by one or more of C1-C5 alkyl (for example: C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl), C1-C6 alkoxy (for example: C1 alkoxy, C2 alkoxy, C3 alkoxy, C4 alkoxy, C5 alkoxy, C6 alkoxy) and phenyl.
[0044] In some embodiments, the alkyl group in the substituted or unsubstituted alkyl acrylate and the substituted or unsubstituted alkyl methacrylate has 1 to 8 carbon atoms (eg, 1, 2, 3, 4, 5, 6, 7 or 8).
[0045] In some embodiments, the substitution in the substituted alkyl acrylate and the substituted alkyl methacrylate each independently represents that at least one H atom is replaced by one or more of a hydroxyl group and an amino group.
[0046] In some embodiments, the acrylic acid ester monomer includes at least one of alkyl acrylate and methyl methacrylate.
[0047] In some embodiments, the R 4 wherein the substituted C1-C6 alkyl group, the R 5 The substituted C1-C6 alkyl or substituted C2-C 10 The alkenyl group, the R 6 The substituted C1-C6 alkyl or substituted C2-C 10 The substitutions in the alkenyl group each independently represent that at least one hydrogen atom is replaced by one or more selected from C1 to C5 alkyl groups (eg, C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl).
[0048] In some preferred embodiments, the R 4 is selected from substituted or unsubstituted C1-C3 alkyl; R 5 With R 6 Each is independently selected from H, substituted or unsubstituted C1-C3 alkyl, and substituted or unsubstituted C2-C4 alkenyl.
[0049] In some embodiments, the R 4 wherein the substituted C1-C3 alkyl group, the R 5 wherein the substituted C1-C3 alkyl or substituted C2-C4 alkenyl, the R 6The substitution in the substituted C1-C3 alkyl or substituted C2-C4 alkenyl each independently means that at least one hydrogen atom is replaced by one or more selected from C1-C5 alkyl.
[0050] In some embodiments, the monomers are methyl methacrylate and N-(methoxymethyl)methacrylamide.
[0051] In some embodiments, the initiator includes at least one of an azo-based free radical initiator and a peroxide-based free radical initiator.
[0052] In some embodiments, the azo free radical initiator includes at least one of 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobismethoxyisoheptanenitrile.
[0053] In some embodiments, the peroxide-based free radical initiator includes at least one of diisopropyl peroxydicarbonate, bis(2-ethylhexyl) per(oxy)dicarbonate, diethoxyethyl peroxydicarbonate, tert-butyl peroxyneodecanoate, α-cumyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, acetylcyclohexylsulfoperoxide, diisobutyryl peroxide, and 2,4,4-trimethylpentyl-2-peroxyphenoxyacetate.
[0054] In some preferred embodiments, the regulator includes at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol.
[0055] In some embodiments, the solvent includes at least one of tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol methyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide and N-methylpyrrolidone.
[0056] In some preferred embodiments, the solvent is selected from at least one of tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and propylene glycol propyl ether acetate.
[0057] In some embodiments, the mass ratio of the initiator to the regulator is 2: 1-10: 1. In some embodiments, the mass ratio of the initiator to the regulator is 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1 or 10: 1. In some embodiments, the mass ratio of the initiator to the regulator is 2: 1, 5: 1 or 10: 1.
[0058] In some embodiments, the mass ratio of the monomer to the regulating agent is 50: 1-1000: 1. In some embodiments, the mass ratio of the monomer to the regulating agent is 50: 1, 55: 1, 60: 1, 65: 1, 70: 1, 75: 1, 80: 1, 90: 1, 95: 1, 96: 1, 97: 1, 98: 1, 99: 1, 100: 1, 110: 1, 120: 1, 130: 1, 140: 1, 150: 1, 200: 1, 250: 1, 300: 1, 350: 1, 400: 1, 450: 1, 500: 1, 550: 1, 600: 1, 650: 1, 700: 1, 750: 1, 800: 1, 850: 1, 900: 1, 950: 1 or 1000: 1. In some embodiments, the feed mass ratio of the monomer to the regulating agent is 98: 1-400: 1. In some embodiments, the feed mass ratio of the monomer to the regulating agent is 98: 1-100: 1.
[0059] In some embodiments, the feed mass of the monomer represented by formula (II) accounts for 5wt%-80wt% of the total feed mass of the monomer represented by formula (II) and the acrylate monomer. In some embodiments, the feed mass of the monomer represented by formula (II) accounts for 5wt%, 10wt%, 15wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 30wt%, 31wt%, 31.5wt%, 31.9wt%, 32wt%, 33wt%, 34wt%, 35wt% of the total feed mass of the monomer represented by formula (II) and the acrylate monomer. %, 40wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt%, 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt%, 60wt%, 65wt%, 70wt%, 71wt%, 72wt%, 73wt%, 74wt%, 75wt%, 76wt%, 77wt%, 77wt%, 78wt%, 79wt% or 80wt%. In some embodiments, the feed mass of the monomer represented by formula (II) accounts for 15wt%-76wt% of the total feed mass of the monomer represented by formula (II) and the acrylate monomer.
[0060] In some embodiments, the volume of the solvent for each 1g of the monomer is 2.0ml-10.0ml. In some embodiments, the volume of the solvent for each 1g of the monomer is 2.0ml, 3.0ml, 4.0ml, 5.0ml, 5.1ml, 5.2ml, 5.3ml, 5.4ml, 5.5ml, 6.0ml, 6.5ml, 7.0ml, 7.5ml, 8.0ml, 8.5ml, 9.0ml, 9.5ml or 10.0ml. In some embodiments, the volume of the solvent for each 1g of the monomer is 2ml-5.3ml.
[0061] In some embodiments, the polymerization reaction is carried out in a device equipped with a reaction container, a circulation pipe and a circulation pump, both ends of the circulation pipe are connected to the reaction container, and the circulation pump is arranged between the two ends of the circulation pipe. The polymerization reaction is carried out under the condition that the circulation pump is used to circulate the mixture A between the reaction container and the circulation pipe.
[0062] In some embodiments, the circulation residence time of the circulating pump is set to 30 seconds-300 seconds. In some embodiments, the circulation residence time of the circulating pump is set to 30 seconds, 40 seconds, 50 seconds, 60 seconds, 70 seconds, 80 seconds, 90 seconds, 100 seconds, 150 seconds, 200 seconds, 250 seconds or 300 seconds. In some embodiments, the circulation residence time of the circulating pump is set to 60 seconds.
[0063] In some embodiments, the circulation ratio of the circulation pump is 1:15-1:50. In some embodiments, the circulation ratio of the circulation pump is 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45 or 1:50. In some embodiments, the circulation ratio of the circulation pump is 1:25.
[0064] In some embodiments, the certain temperature is 50° C.-90° C. In some embodiments, the certain temperature is 50° C., 55° C., 60° C., 65° C., 66° C., 67° C., 68° C., 69° C., 70° C., 71° C., 72° C., 73° C., 74° C., 75° C., 80° C., 85° C., or 90° C. In some embodiments, the certain temperature is 70° C.
[0065] In some embodiments, the temperature of the circulation conduit is 45° C.-85° C. In some embodiments, the temperature of the circulation conduit is 45° C., 50° C., 55° C., 60° C., 61° C., 62° C., 63° C., 64° C., 65° C., 66° C., 67° C., 68° C., 69° C., 70° C., 75° C., 80° C., or 85° C. In some embodiments, the temperature of the circulation conduit is 65° C.
[0066] In some embodiments, the reaction time of the polymerization reaction is 4 hours to 8 hours. In some embodiments, the reaction time of the polymerization reaction is 4 hours, 5 hours, 6 hours, 7 hours or 8 hours. In some embodiments, the reaction time of the polymerization reaction is 7 hours.
[0067] In some embodiments, the inert gas includes at least one of helium, neon, argon, krypton, and xenon.
[0068] In some embodiments, the acrylic acid ester monomer is methyl methacrylate, and the monomer represented by formula (II) is represented by formula (A):
[0069]
[0070] In some embodiments, the acrylic acid ester monomer is methyl methacrylate, and the monomer represented by formula (II) is represented by formula (A): The regulating agent is at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol. In some embodiments, the acrylic acid ester monomer is methyl methacrylate, and the monomer represented by formula (II) is represented by formula (A): The regulating agent is at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol; and the initiator is azobisisobutyronitrile.
[0071] In some embodiments, the acrylic acid ester monomer is methyl methacrylate, and the monomer represented by formula (II) is represented by formula (A): The regulating agent is at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol; the initiator is azobisisobutyronitrile; and the solvent is propylene glycol methyl ether acetate.
[0072] In some embodiments, the acrylic acid ester monomer is methyl methacrylate, and the monomer represented by formula (II) is represented by formula (A): The regulating agent is at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol; the initiator is azobisisobutyronitrile; the solvent is propylene glycol methyl ether acetate; the feed mass of the monomer represented by formula (II) accounts for 15wt% of the total feed mass of the monomer represented by formula (II) and the acrylate monomer.
[0073] In some embodiments, the acrylic acid ester monomer is methyl methacrylate, and the monomer represented by formula (II) is represented by formula (A): The regulating agent is at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol; the initiator is azobisisobutyronitrile; the solvent is tetrahydrofuran; the feed mass of the monomer represented by formula (II) accounts for 20wt%-50wt% of the total feed mass of the monomer represented by formula (II) and the acrylate monomer.
[0074] In some embodiments, the acrylic acid ester monomer is methyl methacrylate, and the monomer represented by formula (II) is represented by formula (A): The regulating agent is at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol; the initiator is azobisisobutyronitrile; the solvent is tetrahydrofuran; the feed mass of the monomer represented by formula (II) accounts for 24wt%-47wt% of the total feed mass of the monomer represented by formula (II) and the acrylate monomer.
[0075] In some embodiments, in the step (2), after the polymerization reaction is completed, post-treatment is also included, and the post-treatment includes: obtaining a reaction solution after the polymerization reaction is completed, mixing the reaction solution with n-hexane to produce precipitation, centrifuging or filtering to obtain a solid, and drying the solid.
[0076] In some embodiments, the volume ratio of the reaction solution to n-hexane is 1:1-1:5. In some embodiments, the volume ratio of the reaction solution to n-hexane is 1:1, 1:2, 1:3, 1:4 or 1:5.
[0077] In some embodiments, the weight average molecular weight (Mw) of the crosslinkable polymer is ≤30,000 Da. In some embodiments, the weight average molecular weight (Mw) of the crosslinkable polymer is ≤25,000 Da. In some embodiments, the weight average molecular weight (Mw) of the crosslinkable polymer is 20,000 Da-25,000 Da. In some embodiments, the weight average molecular weight (Mw) of the crosslinkable polymer is 20,000 Da, 21,000 Da, 22,000 Da, 23,000 Da, 24,000 Da or 25,000 Da.
[0078] In some embodiments, the molecular weight of the cross-linkable polymer has a PDI of ≤ 1.5. In some embodiments, the molecular weight of the cross-linkable polymer has a PDI of 1.4-1.5.
[0079] The repeating unit arrangement state of the cross-linkable polymer prepared by the preparation method is random copolymerization.
[0080] In a second aspect, the present invention provides a cross-linkable polymer.
[0081] A cross-linkable polymer prepared according to the preparation method of the first aspect.
[0082] In some embodiments, the cross-linkable polymer includes a monomer unit formed by a structure represented by formula (II) and an acrylate monomer unit.
[0083]
[0084] in,
[0085] R 1 Selected from substituted or unsubstituted C2~C 10 substituted or unsubstituted C2 alkenyl, substituted or unsubstituted C3 alkenyl, substituted or unsubstituted C4 alkenyl, substituted or unsubstituted C5 alkenyl, substituted or unsubstituted C6 alkenyl, substituted or unsubstituted C7 alkenyl, substituted or unsubstituted C8 alkenyl, substituted or unsubstituted C9 alkenyl, substituted or unsubstituted C 10 alkenyl);
[0086] R 2 With R 3 Each is independently selected from H, substituted or unsubstituted C1-C6 alkyl (e.g., substituted or unsubstituted C1 alkyl, substituted or unsubstituted C2 alkyl, substituted or unsubstituted C3 alkyl, substituted or unsubstituted C4 alkyl, substituted or unsubstituted C5 alkyl, substituted or unsubstituted C6 alkyl), substituted or unsubstituted C6-C 20 substituted or unsubstituted C6 aryl, substituted or unsubstituted C7 aryl, substituted or unsubstituted C8 aryl, substituted or unsubstituted C9 aryl, substituted or unsubstituted C 10 Aryl, substituted or unsubstituted C 11 Aryl, substituted or unsubstituted C 12 Aryl, substituted or unsubstituted C 13 Aryl, substituted or unsubstituted C 14 Aryl, substituted or unsubstituted C 15 Aryl, substituted or unsubstituted C 16 Aryl, substituted or unsubstituted C 17 Aryl, substituted or unsubstituted C 18 Aryl, substituted or unsubstituted C 19 Aryl, substituted or unsubstituted C 20 aryl);
[0087] In some embodiments, the substituted C2 to C 10 Alkenyl, substituted C1-C6 alkyl and substituted C6-C 20The substitution in the aryl group independently means that at least one hydrogen atom is replaced by one or more of C1-C5 alkyl (for example: C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl), C1-C6 alkoxy (for example: C1 alkoxy, C2 alkoxy, C3 alkoxy, C4 alkoxy, C5 alkoxy, C6 alkoxy), and phenyl.
[0088] In some embodiments, the acrylic acid ester monomer unit is a substituted or unsubstituted alkyl acrylate or a substituted or unsubstituted alkyl methacrylate.
[0089] In some embodiments, the alkyl group in the substituted or unsubstituted alkyl acrylate and the substituted or unsubstituted alkyl methacrylate has 1 to 8 carbon atoms (eg, 1, 2, 3, 4, 5, 6, 7 or 8).
[0090] In some embodiments, the substitution in the substituted alkyl acrylate and the substituted alkyl methacrylate each independently represents that at least one H atom is replaced by one or more of a hydroxyl group and an amino group.
[0091] In some embodiments, the content of the monomer unit formed by the structure shown in the formula (II) is 5wt%-80wt% based on the total mass of the crosslinkable polymer. In some embodiments, the content of the monomer unit formed by the structure shown in the formula (II) is 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt% or 80wt% based on the total mass of the crosslinkable polymer. In some embodiments, the content of the monomer unit formed by the structure shown in the formula (II) is 15wt% based on the total mass of the crosslinkable polymer.
[0092] In some embodiments, the acrylic acid ester monomer unit is methyl methacrylate.
[0093] In some embodiments, the monomer unit formed by the structure represented by formula (II) is:
[0094] In some embodiments, the acrylic acid ester monomer unit is methyl methacrylate, and the monomer unit formed by the structure represented by formula (II) is:
[0095] In a third aspect, the present invention provides a cross-linkable polymer prepared according to the preparation method of the first aspect or a use of the cross-linkable polymer of the second aspect.
[0096] A use of the cross-linkable polymer prepared according to the preparation method of the first aspect or the cross-linkable polymer of the second aspect in preparing an anti-reflective coating composition.
[0097] In a fourth aspect, the present invention provides an anti-reflective coating composition.
[0098] An anti-reflective coating composition comprises: a cross-linkable polymer prepared according to the preparation method of the first aspect or the cross-linkable polymer of the second aspect.
[0099] In some embodiments, the anti-reflective coating composition further includes a thermal acid generator, a surfactant, and a solvent.
[0100] Beneficial Effects
[0101] Compared with the prior art, the present invention has the following beneficial effects:
[0102] (1) Compared with the polymerization reaction without adding a regulating agent, the use of the regulating agent provided by the present invention is more conducive to reducing the PDI of the obtained cross-linkable polymer, which has an unexpected technical effect.
[0103] (2) Compared with the polymerization reaction without the circulation pump, the reaction under the condition of circulating the reaction liquid by the circulation pump of the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, which has an unexpected technical effect.
[0104] (3) Compared with the use of a para-unsubstituted structure regulator, the use of the regulator provided by the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, which has an unexpected technical effect.
[0105] (4) Compared with the use of a para-non-alkyl structured regulating agent, the use of the regulating agent provided by the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, and has an unexpected technical effect.
[0106] (5) Compared with the use of diphenolic regulators with a para-non-alkyl structure, the use of the regulator provided by the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, which has an unexpected technical effect.
[0107] (6) The cross-linkable polymer obtained by the preparation method provided by the present invention has a small molecular weight PDI (narrow molecular weight distribution), no odor and no discoloration, and has unexpected technical effects.
[0108] (7) Among the control agents provided by the present invention, at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol is preferably used as the control agent of the present invention, which is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer.
[0109] (8) The preparation method provided by the present invention has high monomer conversion rate, is safe, environmentally friendly, low cost, has good reproducibility of weight average molecular weight and molecular weight PDI, and has unexpected technical effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] Figure 1 It is a simplified structural schematic diagram of the reaction device of Example 1-Example 2, Comparative Example 1, Comparative Example 3-Comparative Example 5 of the present invention.
[0111] In the accompanying drawings, 1 is a reaction container; 2 is a circulation pump; and 3 is a circulation pipeline.
[0112] Terminology
[0113] In the description of the present invention, “plurality” means two or more than two, unless otherwise clearly and specifically defined.
[0114] The term "room temperature" means ambient temperature, referring to a temperature between about 10°C and about 30°C, or between about 20°C and 30°C, or about 25°C.
[0115] The term "wt%" means percent by mass.
[0116] The term "plurality" means two or more.
[0117] The term "circulation residence time" means the time that the material resides in the circulation conduit; that is, the time it leaves the reaction vessel.
[0118] The term "circulation ratio" means the ratio of the volume of material in the circulation pipe to the volume of material in the reaction vessel.
[0119] The term "Da" means Dalton.
[0120] In the present invention, PDI represents polymer dispersibility index, which is calculated by the formula PDI=polymer weight average molecular weight (Mw, also called weight average molecular weight) divided by polymer number average molecular weight (Mn, also called number average molecular weight).
[0121] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0122] In the following, all numbers disclosed herein are approximate, regardless of whether the word "about" or "approximately" is used. The value of each number may vary by 1%, 2%, 5%, 7%, 8%, 10%, 15% or 20%. Whenever a number with a value of N is disclosed, any number with a value of N+ / -1%, N+ / -2%, N+ / -3%, N+ / -5%, N+ / -7%, N+ / -8%, N+ / -10%, N+ / -15% or N+ / -20% will be explicitly disclosed, where "+ / -" means plus or minus.
[0123] The terms "optional", "optional" or "optionally" mean that the subsequently described event or circumstance may but need not occur.
[0124] The "C1-C 10 "Includes C1-C 10 Any integer point value in, such as C1, C2, C3, C4, C5, C6, C7, C8, C9, or C 10 . "C6-C 12 ”, “C3-C 10 ”, “C3-C 12 ”, “C4-C 12 ”, “C3-C 10 ”, “C6-C 20 " and so on, that is, "C6-C 12 "Includes C6-C 12 Any integer point value in, such as C6, C7, C8, C9, C 10 , C 11 , C 12 .
[0125] "Alkyl" is a hydrocarbon containing normal carbon atoms, secondary carbon atoms, tertiary carbon atoms, or ring carbon atoms. For example, an alkyl group can have 1 to 10 carbon atoms (i.e., C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl, C8 alkyl, C9 alkyl, or C 10alkyl), 1 to 8 carbon atoms (i.e., C1-C8 alkyl), or 1 to 6 carbon atoms (i.e., C1-C6 alkyl). Examples of suitable alkyl groups include, but are not limited to, methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (i-Pr, i-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl, -CH (CH3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl ( -CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH (CH3)CH2CH3), 4-methyl-2-pentyl (-CH(CH3)CH2CH(CH3)2), 3-methyl-3-pentyl (-C(CH3)(CH2CH3)2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 or octyl (-(CH2)7CH3).
[0126] An "alkenyl group" is a group containing at least one unsaturated site, i.e., a carbon-carbon sp 2 For example, an alkenyl group can have 2 to 10 carbon atoms (C2-C 10 alkenyl), 2 to 12 carbon atoms (C2-C 12 alkenyl, such as C2 alkenyl, C3 alkenyl, C4 alkenyl, C5 alkenyl, C6 alkenyl, C7 alkenyl, C8 alkenyl, C9 alkenyl, C 10 Alkenyl, C 11 Alkenyl or C 12Examples of suitable alkenyl groups include, but are not limited to, ethylene or vinyl (-CH=CH), allyl (-CHCH=CH), cyclopentenyl (-C5H7) and 5-hexenyl (-CHCHCHCHCH=CH), propenyl, isopropenyl, butenyl, isobutenyl, pentenyl, butadienyl, pentenyl, isopentenyl, pentadienyl, hexenyl, isohexenyl, hexadienyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, tridecenyl, tetradecenyl or pentadecenyl, etc.
[0127] "Aryl" means an aromatic hydrocarbon group derived by removing one hydrogen atom from a single carbon atom of a parent aromatic ring system. For example, an aryl group can have 6 to 20 carbon atoms (e.g., C6 aryl, C7 aryl, C8 aryl, C9 aryl, C 10 Aryl, C 11 Aryl, C 12 Aryl, C 13 Aryl, C 14 Aryl, C 15 Aryl, C 16 Aryl, C 17 Aryl, C 18 Aryl, C 19 Aryl or C 20 The aryl group may be 6 to 14 carbon atoms or 6 to 10 carbon atoms. Typical aryl groups include, but are not limited to, groups derived from benzene (e.g., phenyl), substituted benzene, naphthyl, anthracenyl, tetrahydronaphthyl, phenanthrenyl, fluorenyl or biphenyl or the like.
[0128] Examples of alkoxy groups include, but are not limited to, methoxy (MeO, -OCH3), ethoxy (EtO, -OCH2CH3), 1-propoxy (n-PrO, n-propoxy, -OCH2CH2CH3), 2-propoxy (i-PrO, i-propoxy, -OCH(CH3)2), 1-butoxy (n-BuO, n-butoxy, -OCH2CH2CH2CH3), 2-methyl-1-propoxy (i-BuO, i-butoxy, -OCH2CH(CH3)2), 2-butoxy (s-BuO, s-butoxy, -OCH(CH3)CH2CH3), 2-methyl-2-propoxy (t-BuO, t-butoxy, -OC(CH3)3), and the like.
[0129] The term "substituted" refers to alkyl, aryl, arylalkyl, heterocyclyl, heteroaryl, carbocyclyl, etc., for example, "substituted C1-C 10 Alkyl", "substituted C6-C 20 Aryl", "substituted arylalkyl", "substituted C1-C 20"Heterocycle" and "substituted carbocyclyl" refer to C1-C2-1, C1-C3-1, C1-C4-1, C1-C6-1, C1-C7-1, C1-C8-1, C1-C9-1, C1-C1 ... 10 Alkyl, C6-C 20 Aryl, Arylalkyl, C1-C 20 Heterocyclic, carbocyclic. Unless otherwise indicated, a substituted group may have a substituent at each substitutable position of the group. When more than one position in the given structural formula can be substituted by one or more substituents selected from a specific group, the substituents may be the same or different at each position.
[0130] The term "unsubstituted" means that the designated group bears no substituents.
[0131] The term "jk atoms" or "jk-membered" means that the cyclic group is composed of jk ring atoms, and the ring atoms include carbon atoms and / or heteroatoms such as O, N, S, and P; j and k are each independently any non-zero natural number, and k>j; "jk" includes j, k, and any natural number between the two. For example, "3-8 atoms" or "3-8-membered", "3-6 atoms" or "3-6-membered", "5-10 atoms" or "5-10-membered", "5-6 atoms" or "5-6-membered" means that the cyclic group is composed of 3-8 (i.e., 3, 4, 5, 6, 7, or 8), 3-6 (i.e., 3, 4, 5, or 6), 5-10 (i.e., 5, 6, 7, 8, 9, or 10), or 5-6 (i.e., 5 or 6) ring atoms, and the ring atoms include carbon atoms and / or heteroatoms such as O, N, S, and P. For another example, piperidinyl is a 6-atom heterocyclic group or a 6-membered heterocyclic group, and pyridinyl is a 6-atom heteroaryl group or a 6-membered heteroaryl group.
[0132] The term "jk pieces", "jk yuan" or "C j -C k " wherein j and k are independently any non-zero natural numbers, and k>j; for example, "1-4" means 1, 2, 3 or 4, "4-6 yuan" means 4 yuan, 5 yuan or 6 yuan; "C3-C6" means C3, C4, C5 or C6. And so on. DETAILED DESCRIPTION
[0133] In order to enable those skilled in the art to better understand the technical solution of the present invention, some non-limiting embodiments are further disclosed below to further describe the present invention in detail.
[0134] The reagents used in the present invention can be purchased from the market or prepared by the method described in the present invention.
[0135] The structure of N-(methoxymethyl)methacrylamide is: The structure of methyl methacrylate is:
[0136] Example 1: Preparation of cross-linkable polymer
[0137] In the reaction apparatus (see Figure 1 ), monomer N-(methoxymethyl)methacrylamide (2.6 g) and monomer methyl methacrylate
[0138] (2.3g) was dissolved in 10ml tetrahydrofuran, and azobisisobutyronitrile (500mg) and a regulator 2,4-dimethyl-6-tert-butylphenol (50mg) were added and stirred evenly. The mixture was deoxygenated (deoxygenated by vacuuming), sealed after passing nitrogen, and the circulating pump was turned on. The polymerization reaction was carried out at 70°C, the material circulation residence time (the time the material stayed in the circulation pipeline) was 60 seconds, the circulation ratio (the ratio of the volume of the material in the circulation pipeline to the volume of the material in the reaction container) was 1:25, the circulation pipeline temperature was 65°C, and the reaction was carried out for 7 hours. After the polymerization reaction was completed, a reaction solution was obtained, and the reaction solution was mixed with n-hexane (volume ratio was 1:1), precipitation occurred, centrifuged, and a solid was obtained, and the solid was dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw, also called weight average molecular weight) of the obtained crosslinkable polymer is 20,000 Da, the PDI (polymer dispersibility index) is 1.5, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the arrangement state of the repeating units of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer: colorless; the odor of the obtained crosslinkable polymer: odorless.
[0139] The operation of Example 1 was repeated many times, and the weight average molecular weight of the obtained cross-linkable polymer was in the range of 2.0±0.1 Da, and the PDI was in the range of 1.4-1.5, with good reproducibility.
[0140] Example 2: Preparation of cross-linkable polymer
[0141] In the reaction apparatus (see Figure 1 ), monomer N-(methoxymethyl)methacrylamide (3.8 g) and monomer methyl methacrylate
[0142] (1.2g) was dissolved in 10ml tetrahydrofuran, and azobisisobutyronitrile (250mg) and a regulator 2,4-dimethyl-6-tert-butylphenol (50mg) were added and stirred evenly. The mixture was deoxygenated (deoxygenated by vacuuming), sealed after passing nitrogen, and the circulating pump was turned on. The polymerization reaction was carried out at 70°C, the material circulation residence time (the time the material stayed in the circulation pipeline) was 60 seconds, the circulation ratio (the ratio of the volume of the material in the circulation pipeline to the volume of the material in the reaction container) was 1:25, the circulation pipeline temperature was 65°C, and the reaction was carried out for 7 hours. After the polymerization reaction was completed, a reaction solution was obtained, and the reaction solution was mixed with n-hexane (volume ratio of 1:1), precipitation occurred, centrifuged, and a solid was obtained. The solid was dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 25,000 Da, the PDI (polymer dispersibility index) is 1.4, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the arrangement state of the repeating units of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer is colorless; the odor of the obtained crosslinkable polymer is odorless.
[0143] The operation of Example 2 was repeated many times, and the weight average molecular weight of the obtained cross-linkable polymer was in the range of 2.5±0.1 Da, and the PDI was in the range of 1.4-1.5, with good reproducibility.
[0144] Example 3: Preparation of cross-linkable polymer
[0145] In the reaction apparatus (see Figure 1 ), dissolving monomer methyl methacrylate (51g) and monomer N-(methoxymethyl)methacrylamide (9g) in solvent propylene glycol methyl ether acetate (240ml), adding azobisisobutyronitrile (300mg) and regulating agent 2,4-dimethyl-6-tert-butylphenol (0.15g), stirring evenly, removing oxygen (removing oxygen by vacuumizing), passing nitrogen and sealing, turning on the circulation pump, and carrying out polymerization reaction at 70°C, the material circulation residence time (the time the material stays in the circulation pipeline) is 60 seconds, the circulation ratio (the ratio of the material volume in the circulation pipeline to the material volume in the reaction container) is 1:25, the circulation pipeline temperature is 65°C, reacting for 7 hours, and obtaining a reaction solution after the polymerization reaction is completed. The reaction solution is mixed with n-hexane (volume ratio is 1:1), precipitation occurs, centrifugation is performed to obtain a solid, and the solid is dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 24,000 Da, the PDI (polymer dispersibility index) is 1.4, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the repeating unit arrangement state of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer is colorless; the odor of the obtained crosslinkable polymer is odorless.
[0146] The operation of Example 3 was repeated many times, and the weight average molecular weight of the obtained cross-linkable polymer was in the range of 2.4±0.1 Da, and the PDI was in the range of 1.4-1.5, with good reproducibility.
[0147] Example 4: Preparation of cross-linkable polymer
[0148] In the reaction apparatus (see Figure 1 ), dissolve monomer methyl methacrylate (51g) and monomer N-(methoxymethyl) methacrylamide (9g) in solvent propylene glycol methyl ether acetate (240ml), add azobisisobutyronitrile (300mg) and regulating agent 2,6-di-tert-butyl-4-methylphenol (0.15g), stir evenly, remove oxygen (vacuum removal of oxygen), pass nitrogen and seal, turn on the circulation pump, and carry out polymerization reaction at 70°C, the material circulation residence time (the time the material stays in the circulation pipeline) is 60 seconds, the circulation ratio is 1:25, the circulation pipeline temperature is 65°C, and the reaction is carried out for 7 hours. After the polymerization reaction, a reaction solution is obtained, the reaction solution is mixed with n-hexane (volume ratio is 1:1), precipitation occurs, centrifugation is performed to obtain a solid, and the solid is dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 25,000 Da, the PDI is 1.5, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the arrangement state of the repeating units of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer is colorless; the odor of the obtained crosslinkable polymer is odorless.
[0149] The operation of Example 4 was repeated many times, and the weight average molecular weight of the obtained cross-linkable polymer was in the range of 25000±0.1 Da, and the PDI was in the range of 1.4-1.5, with good reproducibility.
[0150] Comparative Example 1: No Regulator
[0151] In the reaction apparatus (see Figure 1), dissolve the monomer methyl methacrylate (51g) and the monomer N-methoxymethyl acrylamide (9g) in the solvent propylene glycol methyl ether acetate (240ml), add azobisisobutyronitrile (300mg), stir evenly, deoxygenate, seal after nitrogen, open the circulation pump, and carry out polymerization reaction at 70°C. The material circulation residence time (the time the material stays in the circulation pipeline) is 60 seconds, the circulation ratio is 1:25, the circulation pipeline temperature is 65°C, and the reaction is carried out for 7 hours. After the polymerization reaction is completed, a reaction liquid is obtained, and the reaction liquid is mixed with n-hexane (volume ratio is 1:1), precipitation occurs, centrifugation is performed, and a solid is obtained. The solid is dried to obtain a crosslinkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 24,000 Da, the PDI is 2.7, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the arrangement state of the repeating units of the obtained crosslinkable polymer is random copolymerization. Color of the obtained cross-linkable polymer: colorless; Odor of the obtained cross-linkable polymer: odorless.
[0152] Conclusion: Compared with the polymerization reaction without adding a regulating agent, the use of the regulating agent provided by the present invention is more conducive to reducing the PDI of the obtained cross-linkable polymer, which has an unexpected technical effect.
[0153] Comparative Example 2: No Circulation Operation
[0154] In a four-necked bottle, the monomer methyl methacrylate (51g) and the monomer N-(methoxymethyl) methacrylamide (9g) were dissolved in the solvent propylene glycol methyl ether acetate (240ml), and azobisisobutyronitrile (300mg) and the regulator 2,4-dimethyl-6-tert-butylphenol (0.15g) were added, stirred evenly, deoxygenated (deoxygenated by vacuuming), sealed after passing nitrogen, reacted at 70°C, reacted for 7 hours, and obtained a reaction liquid after the polymerization reaction was completed. The reaction liquid was mixed with n-hexane (volume ratio of 1:1), precipitated, centrifuged, obtained a solid, and dried the solid to obtain a crosslinkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 27,000 Da, the PDI is 1.8, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the repeating unit arrangement state of the obtained crosslinkable polymer is random copolymerization. Color of the obtained cross-linkable polymer: colorless; Odor of the obtained cross-linkable polymer: odorless.
[0155] Conclusion: Compared with the polymerization reaction without the circulation pump, the reaction under the condition of circulating the reaction liquid by the circulation pump in the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, which has unexpected technical effects.
[0156] Comparative Example 3: Using a para-unsubstituted structure regulator
[0157] In the reaction apparatus (see Figure 1 ), dissolving monomer methyl methacrylate (51g) and monomer N-(methoxymethyl)methacrylamide (9g) in solvent propylene glycol methyl ether acetate (240ml), adding azobisisobutyronitrile (300mg) and regulating agent 2,6-di-tert-butylphenol (0.15g), stirring evenly, removing oxygen (removing oxygen by vacuumizing), sealing after passing nitrogen, turning on the circulation pump, and carrying out polymerization reaction at 70°C, the material circulation residence time (the time the material stays in the circulation pipeline) is 60 seconds, the circulation ratio is 1:25, the circulation pipeline temperature is 65°C, and the reaction is carried out for 7 hours. After the polymerization reaction, a reaction solution is obtained, the reaction solution is mixed with n-hexane (volume ratio is 1:1), precipitation occurs, centrifugation is performed, a solid is obtained, and the solid is dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 26,000 Da, the PDI is 2.5, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the repeating unit arrangement state of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer is colorless; the odor of the obtained crosslinkable polymer is odorless.
[0158] Conclusion: Compared with the use of a para-unsubstituted structure regulator, the use of the regulator provided by the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, and has an unexpected technical effect.
[0159] Comparative Example 4: Using a para-non-alkyl structure regulator
[0160] In the reaction apparatus (see Figure 1), dissolving monomer methyl methacrylate (51g) and monomer N-(methoxymethyl) methacrylamide (9g) in solvent propylene glycol methyl ether acetate (240ml), adding azobisisobutyronitrile (300mg) and regulating agent 4-methoxyphenol (also known as hydroquinone monomethyl ether) (0.15g), stirring evenly, removing oxygen (vacuuming to remove oxygen), passing nitrogen and sealing, turning on the circulation pump, and carrying out polymerization reaction at 70°C, the material circulation residence time (the time the material stays in the circulation pipeline) is 60 seconds, the circulation ratio is 1:25, the circulation pipeline temperature is 65°C, and the reaction is carried out for 7 hours. After the polymerization reaction, a reaction solution is obtained, the reaction solution is mixed with n-hexane (volume ratio is 1:1), precipitation occurs, centrifugation is performed to obtain a solid, and the solid is dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 26,000 Da, the PDI is 2.5, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the repeating unit arrangement state of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer is colorless; the odor of the obtained crosslinkable polymer is odorless.
[0161] Conclusion: Compared with the use of a para-non-alkyl structured regulator, the use of the regulator provided by the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, and has an unexpected technical effect.
[0162] Comparative Example 5: Using a diphenolic regulator with a para-non-alkyl structure
[0163] In the reaction apparatus (see Figure 1 ), dissolve monomer methyl methacrylate (51g) and monomer N-(methoxymethyl) methacrylamide (9g) in solvent propylene glycol methyl ether acetate (240ml), add azobisisobutyronitrile (300mg) and regulating agent hydroquinone (0.15g), stir evenly, remove oxygen (vacuum removal of oxygen), seal after passing nitrogen, turn on the circulation pump, and carry out polymerization reaction at 70°C, the material circulation residence time (the time the material stays in the circulation pipeline) is 60 seconds, the circulation ratio is 1:25, the circulation pipeline temperature is 65°C, and the reaction is carried out for 7 hours. After the polymerization reaction, a reaction solution is obtained, the reaction solution is mixed with n-hexane (volume ratio is 1:1), precipitation occurs, centrifugation is performed, a solid is obtained, and the solid is dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 28,000 Da, the PDI is 2.6, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the repeating unit arrangement state of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer is colorless; the odor of the obtained crosslinkable polymer is odorless.
[0164] Conclusion: Compared with the use of diphenolic regulators with a para-non-alkyl structure, the use of the regulator provided by the present invention is more conducive to reducing the molecular weight PDI of the obtained cross-linkable polymer, and has an unexpected technical effect.
[0165] Comparative Example 6: Reference CN113913075A Example 3
[0166] Dissolve the monomer N-(methoxymethyl) methacrylamide (3.8g) and the monomer methyl methacrylate (1.2g) in 10ml tetrahydrofuran, add azobisisobutyronitrile (250mg) and the regulator 2,4-dimethyl-6-tert-butylphenol (50mg), and stir evenly. Heat to reflux and react for 24 hours. The generated polymer is precipitated with n-hexane and heated and dried in a drying oven to obtain the desired polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 28,000 Da, the PDI (polymer dispersibility index) is 1.9, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the repeating unit arrangement state of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer: colorless; the odor of the obtained crosslinkable polymer: odorless.
[0167] The operation of Comparative Example 6 was repeated several times, and the weight average molecular weight of the obtained cross-linkable polymer fluctuated within the range of 28±0.3 Da, and the PDI fluctuated within the range of 1.7-2.1, with poor reproducibility.
[0168] Comparative Example 7: Referring to Example 3 of CN113913075A, a circulating pump is used and no regulating agent is added
[0169] In the reaction apparatus (see Figure 1), dissolve the monomer N-(methoxymethyl) methacrylamide (3.8g) and the monomer methyl methacrylate (1.2g) in 10ml tetrahydrofuran, add azobisisobutyronitrile (250mg), and stir evenly. Remove oxygen (deoxygen by vacuuming), seal after passing nitrogen, turn on the circulation pump, and carry out polymerization at 70°C. The material circulation residence time (the time the material stays in the circulation pipeline) is 60 seconds, the circulation ratio (the ratio of the volume of the material in the circulation pipeline to the volume of the material in the reaction container) is 1:25, the circulation pipeline temperature is 65°C, and the reaction is carried out for 7 hours. After the polymerization reaction is completed, a reaction solution is obtained, and the reaction solution is mixed with n-hexane (volume ratio is 1:1), precipitation occurs, centrifugation is performed, and a solid is obtained. The solid is dried to obtain a cross-linkable polymer. The weight average molecular weight (Mw) of the obtained crosslinkable polymer is 29,000 Da, the PDI (polymer dispersibility index) is 2.5, the conversion rate of the monomer methyl methacrylate is ≥95%, and the conversion rate of the monomer N-(methoxymethyl) methacrylamide is ≥95%; the repeating unit arrangement state of the obtained crosslinkable polymer is random copolymerization. The color of the obtained crosslinkable polymer is colorless; the odor of the obtained crosslinkable polymer is odorless.
[0170] The operation of Comparative Example 7 was repeated many times, and the weight average molecular weight of the obtained cross-linkable polymer fluctuated within the range of 29±0.3 Da, and the PDI fluctuated within the range of 2.2-2.8, with poor reproducibility.
[0171] The method of the present invention has been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein within the content, spirit and scope of the present invention to implement and apply the technology of the present invention. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention.
Claims
1. A method for preparing the cross-linkable polymer, characterized in that: The following steps are involved: (1) Material mixing: mixing an initiator, a regulator, a monomer and a solvent to obtain a mixture A; the monomer comprises a monomer represented by formula (II) and an acrylate monomer; The structure of the monomer shown in formula (II) is: in, R 1 Selected from substituted or unsubstituted C2~C 10 The alkenyl group; R 2 With R 3 are independently selected from H, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C 20 The aromatic group; The acrylic acid ester monomer is a substituted or unsubstituted alkyl acrylate or a substituted or unsubstituted alkyl methacrylate; The regulating agent is a compound represented by formula (I), in, R 4 A substituted or unsubstituted C1-C6 alkyl group; R 5 With R 6 are independently selected from H, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C 10 The alkenyl group; (2) Polymerization reaction: removing oxygen from the mixture A obtained in step (1), introducing an inert gas or nitrogen, and performing a polymerization reaction at a certain temperature to obtain the cross-linkable polymer.
2. The preparation method according to claim 1, wherein the substituted C2 to C 10 Alkenyl, substituted C1-C6 alkyl and substituted C6-C 20 The substitution in the aryl group independently means that at least one hydrogen atom is replaced by one or more of a C1-C5 alkyl group, a C1-C6 alkoxy group and a phenyl group; and / or The carbon number of the alkyl group in the substituted or unsubstituted alkyl acrylate and the substituted or unsubstituted alkyl methacrylate is 1 to 8; and / or The substitution in the substituted alkyl acrylate and the substituted alkyl methacrylate independently means that at least one H atom is replaced by one or more of hydroxyl group and amino group; and / or The acrylic acid ester monomer comprises at least one of alkyl acrylate and methyl methacrylate; and / or The R 4 wherein the substituted C1-C6 alkyl group, the R 5 The substituted C1-C6 alkyl or substituted C2-C 10 The alkenyl group, the R 6 The substituted C1-C6 alkyl or substituted C2-C 10 The substitutions in the alkenyl groups independently represent that at least one hydrogen atom is replaced by one or more alkyl groups selected from C1 to C5; and / or Preferably, the R 4 is selected from substituted or unsubstituted C1-C3 alkyl; R 5 With R 6Each is independently selected from H, substituted or unsubstituted C1-C3 alkyl, substituted or unsubstituted C2-C4 alkenyl; and / or Optionally, the R 4 wherein the substituted C1-C3 alkyl group, the R 5 wherein the substituted C1-C3 alkyl or substituted C2-C4 alkenyl, the R 6 The substitution in the substituted C1-C3 alkyl or substituted C2-C4 alkenyl each independently means that at least one hydrogen atom is replaced by one or more selected from C1-C5 alkyl.
3. The preparation method according to any one of claims 1 to 2, wherein the monomers are methyl methacrylate and N-(methoxymethyl)methacrylamide.
4. The preparation method according to any one of claims 1 to 3, wherein the initiator comprises at least one of an azo free radical initiator and a peroxide free radical initiator; and / or The azo free radical initiator includes at least one of 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobismethoxyisoheptanenitrile; and / or The peroxide-based free radical initiator includes at least one of diisopropyl peroxydicarbonate, bis(2-ethylhexyl) per(oxy)dicarbonate, diethoxyethyl peroxydicarbonate, tert-butyl peroxyneodecanoate, α-cumyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, acetylcyclohexylsulfoperoxide, diisobutyryl peroxide, and 2,4,4-trimethylpentyl-2-peroxyphenoxyacetate; and / or Preferably, the regulating agent includes at least one of 2,4-dimethyl-6-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol; and / or The solvent comprises at least one of tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol methyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide and N-methylpyrrolidone; and / or Preferably, the solvent is selected from at least one of tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate and propylene glycol propyl ether acetate; and / or Optionally, the feed mass ratio of the initiator to the regulator is 2:1-10:1 or 2:1; and / or Optionally, the mass ratio of the monomer to the regulator is 50:1-1000:1 or 98:1-400:1; and / or Optionally, the feed weight of the monomer represented by formula (II) accounts for 5wt%-80wt% of the total feed weight of the monomer represented by formula (II) and the acrylate monomer; and / or Optionally, the volume of the solvent charged per 1 g of the monomer is 2.0 ml-10.0 ml.
5. The preparation method according to any one of claims 1 to 4, wherein the polymerization reaction is carried out in a device provided with a reaction vessel, a circulation pipeline and a circulation pump, the two ends of the circulation pipeline are connected to the reaction vessel, the circulation pump is arranged between the two ends of the circulation pipeline, and the polymerization reaction is carried out under the condition that the circulation pump is used to circulate the mixture A between the reaction vessel and the circulation pipeline; and / or The circulation residence time of the circulation pump is set to 30 seconds to 300 seconds or 60 seconds; and / or The circulation ratio of the circulation pump is 1:15-1:50 or 1:25; and / or The certain temperature is 50°C-90°C or 70°C; and / or The temperature of the circulation pipeline is 45°C-85°C or 65°C; and / or The reaction time of the polymerization reaction is 4 hours to 8 hours or 7 hours.
6. The preparation method according to any one of claims 1 to 5, wherein in step (2), after the polymerization reaction is completed, a post-treatment is further included, wherein the post-treatment includes: After the polymerization reaction is completed, a reaction solution is obtained, the reaction solution is mixed with n-hexane, a precipitate is generated, and the solid is obtained by centrifugation or filtration, and the solid is dried.
7. The preparation method according to any one of claims 1 to 6, wherein the weight average molecular weight (Mw) of the cross-linkable polymer is ≤30,000 Da or the weight average molecular weight (Mw) of the cross-linkable polymer is 20,000 Da-25,000 Da; and / or Optionally, the molecular weight of the cross-linkable polymer has a PDI ≤ 1.
5.
8. The cross-linkable polymer prepared according to the preparation method according to any one of claims 1 to 7.
9. Use of the cross-linkable polymer prepared by the preparation method according to any one of claims 1 to 7 or the cross-linkable polymer according to claim 8 in preparing an anti-reflective coating composition.
10. An anti-reflective coating composition, characterized in that: include: The cross-linkable polymer prepared by the preparation method according to any one of claims 1 to 7 or the cross-linkable polymer according to claim 8.
Citation Information
Patent Citations
Recirculation loop reactor bulk polymerization process
CN101712729A
Anti-reflection coating composition and cross-linkable polymer
CN113913075A
Narrow-distribution polymer resin and preparation method thereof
CN116217777A
Polycarboxylate superplasticizer cyclic polymerization reaction device
CN212651825U
Production of polyester
JP1995278278A