Super-hydrophobic coating, preparation method thereof, super-hydrophobic coating and application
By using Diels-Alder bond polymer matrix, microcapsules and modified nanoparticles in superhydrophobic coatings, self-warning and self-repair of the coating is achieved, solving the problem of vulnerability of traditional coatings and improving the coating Durability and superhydrophobic properties.
Patent Information
- Application Number
- CN202411446861.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional superhydrophobic coatings are easily damaged under factors such as ultraviolet rays and wear, resulting in a decline in superhydrophobic performance and making it difficult to meet the actual application needs.
Using polymer matrix containing Diels-Alder bonds, microcapsules loaded with low surface energy substances and fluorescent dyes, and modified superhydrophobic nanoparticles, the damage detection and structural repair of the coating can be achieved through self-warning and self-repair mechanisms. .
It realizes self-warning of damage and superhydrophobic recovery of the coating, extends the durability and service life of the coating, and has significant development potential.
Smart Images

Figure CN119081529A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of super hydrophobic coatings, and in particular relates to a super hydrophobic coating and a preparation method thereof, a super hydrophobic coating and an application thereof. Background Art
[0002] Super-hydrophobic coating is a coating with special surface properties. The water contact angle of its solid coating is >150° and the rolling angle is <10°. Based on its unique properties, super-hydrophobic coatings have been widely used in many fields such as self-cleaning, oil-water separation, anti-icing, and anti-corrosion. However, in actual use, the surface of super-hydrophobic coatings is easily damaged. One is chemical damage caused by ultraviolet rays, and the other is wear and tear during service. Physical damage caused by collisions seriously affects the super-hydrophobic performance and service life of the coating. Therefore, traditional super-hydrophobic coatings have been difficult to meet the needs of practical applications. Summary of the invention
[0003] In view of the problem that current super-hydrophobic coatings cannot perform self-warning and self-repair of damage, a super-hydrophobic coating and a preparation method thereof, a super-hydrophobic coating and an application thereof are provided.
[0004] In some embodiments, a super hydrophobic coating is provided, comprising a polymer matrix containing Diels-Alder bonds and microcapsules and super hydrophobic nanoparticles dispersed in the polymer matrix.
[0005] The microcapsule comprises a core material and a capsule wall covering the core material;
[0006] The core material includes a low surface energy substance and a fluorescent dye;
[0007] The super hydrophobic nanoparticles are prepared by modifying hydrophobic nanoparticles using a modifier.
[0008] In some embodiments, the super hydrophobic coating satisfies one or more of the following characteristics:
[0009] (1) The low surface energy substance is one or more of fluorinated alkyl silanes such as 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, tridecafluorooctyltriethoxysilane, (3,3,3-trifluoropropyl)methyldiethoxysilane, etc.;
[0010] (2) The fluorescent dye is one or more of fluorescein isothiocyanate, 2',7'-dichlorofluorescein, 2',7'-difluorofluorescein, and crystal violet lactone, which are organic small molecules with fluorescent properties;
[0011] (3) The hydrophobic nanoparticles are one or more of nano-silicon dioxide, nano-titanium dioxide, nano-aluminum oxide and nano-zinc oxide;
[0012] (4) The modifier is one or more of methyltriethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, trimethylchlorosilane and polydimethylsiloxane;
[0013] (5) The raw materials for preparing the capsule wall of the microcapsule include polymer prepolymer, organic solvent containing ester group and benzene ring, urea, ammonium chloride, phenol organic matter, and maleic anhydride copolymer;
[0014] (6) The polymer matrix containing Diels-Alder bonds is one or more of polyurethane containing Diels-Alder bonds, epoxy resin containing Diels-Alder bonds, and acrylate containing Diels-Alder bonds;
[0015] (7) The mass ratio of the microcapsule, the super-hydrophobic nanoparticles and the polymer matrix containing Diels-Alder bonds is (0.05-0.5): (0.5-2): (1.5-2);
[0016] (8) The diameter of the microcapsule is 10 μm to 100 μm;
[0017] (9) The particle size of the super hydrophobic nanoparticles is 10 nm to 800 nm.
[0018] In some embodiments, the method for preparing the microcapsules comprises the steps of:
[0019] Mix urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water, and adjust the pH to 2-4 to obtain a first solution;
[0020] Mixing the fluorescent dye, the polymer prepolymer, the low surface energy substance and the organic solvent containing the ester group and the benzene ring to obtain a second solution;
[0021] The second solution is mixed with the first solution, a first reaction is carried out, formaldehyde is added, a second reaction is carried out, the mixture is washed with water, and the mixture is dried to obtain the microcapsules.
[0022] In some embodiments, the method for preparing the microcapsules satisfies one or more of the following characteristics:
[0023] (1) The mass ratio of urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water is (0.1~2): (0.01~0.2): (0.01~0.2): (1~5): (40~80);
[0024] (2) The mass ratio of fluorescent dye, polymer prepolymer, low surface energy substance, and organic solvent containing ester group and benzene ring is (0.02~0.05): (0.8~1): (10~20): (5~10);
[0025] (3) The volume ratio of the first solution to the second solution is (5-7):(2-3);
[0026] (4) Volume ratio of formaldehyde to the second solution (1-1.5):(10-15);
[0027] (5) performing the first reaction at a rotation speed of 400 rpm to 800 rpm for 10 min to 15 min;
[0028] (6) The second reaction is carried out for 4 to 5 hours.
[0029] In some embodiments, the method for preparing the super-hydrophobic nanoparticles comprises the following steps:
[0030] Dispersing hydrophobic nanoparticles in an alcohol solvent, adding a modifier, performing a third reaction, washing with alcohol, and drying to obtain super hydrophobic nanoparticles;
[0031] In some embodiments, the method for preparing superhydrophobic nanoparticles satisfies one or more of the following characteristics:
[0032] (1) In the step of dispersing the hydrophobic nanoparticles in the alcohol solvent, the final concentration of the hydrophobic nanoparticles is 0.05 g / mL to 0.25 g / mL;
[0033] (2) In the step of dispersing the hydrophobic nanoparticles in an alcohol solvent and adding a modifier, the final concentration of the modifier is 0.05 g / mL to 0.1 g / mL;
[0034] (3) The temperature for carrying out the third reaction is 20°C to 60°C;
[0035] (4) The third reaction is carried out for 5 to 15 hours;
[0036] (5) The third reaction is carried out at a rotation speed of 300 rpm to 800 rpm.
[0037] In some embodiments, the method for preparing the polymer matrix containing Diels-Alder bonds comprises: performing a cycloaddition reaction using raw materials including a furan-terminated polymer prepolymer containing double bonds and maleimide.
[0038] In some embodiments, a method for preparing a super hydrophobic coating is provided, wherein raw materials including microcapsules, super hydrophobic nanoparticles, and a polymer matrix containing Diels-Alder bonds are mixed to prepare the super hydrophobic coating.
[0039] In some embodiments, there is provided an application of the super-hydrophobic coating or the super-hydrophobic coating prepared by the preparation method in preparing a super-hydrophobic coating with self-warning and self-repairing functions.
[0040] In some embodiments, a super-hydrophobic coating with self-warning and self-repairing functions is provided, wherein the coating comprises the super-hydrophobic coating or is obtained by solidifying the raw materials of the super-hydrophobic coating prepared by the preparation method.
[0041] The super-hydrophobic coating prepared using the provided super-hydrophobic coating can achieve damage self-warning and self-repair. When the coating is damaged, an obvious fluorescent warning signal will appear in the damaged area, and the strength of the fluorescent signal also reflects the severity of the coating damage. At the same time, coating damage causes microcapsules to rupture, thereby releasing low surface energy substances, and the super-hydrophobicity of the coating can be effectively restored. After heat treatment, the DA bond will break and reconnect, thereby repairing the structural damage of the coating. The super-hydrophobic coating prepared by the present invention can not only warn of coating damage, but also can simultaneously restore the super-hydrophobicity and structural damage of the coating, effectively improving the durability and service life of the material, and has huge development potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions in the implementation methods and examples of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for use in the description of the implementation methods or examples. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0043] Figure 1 is a scanning electron microscope image of the microcapsules prepared in Example 1;
[0044] Figure 2 The scanning electron microscope image of the super hydrophobic nano-SiO2 prepared in Example 1;
[0045] Figure 3 is the water contact angle of the super-hydrophobic coating prepared in Example 1;
[0046] Figure 4 This is a microscopic image of the super-hydrophobic coating prepared in Example 2 after damage;
[0047] Figure 5 This is a microscopic image of the super-hydrophobic coating prepared in Example 2 after repair;
[0048] Figure 6 are the water contact angles of the coating prepared in Example 2 before damage, after damage, and after repair, wherein A is the water contact angle of the coating before damage, B is the water contact angle of the coating after damage, and C is the water contact angle of the coating after repair;
[0049] Figure 7 The fluorescence images of the coating prepared in Example 2 before and after repair, wherein A is the fluorescence image of the coating before repair after damage, and B is the fluorescence image of the coating after repair;
[0050] Figure 8 is the water contact angle of the coating in Comparative Example 1;
[0051] Fig. 9 The water contact angle of the super hydrophobic coating in Comparative Example 2 after being cut with a scalpel and repaired in an oven at 80°C for 3 h. DETAILED DESCRIPTION
[0052] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0053] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0054] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0055] In the present application, "plurality", "multiple", "multiple times", "multiples", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0056] The terms "combination thereof", "any combination thereof", "any combination thereof" and the like used in this application include all suitable combinations of any two or more of the listed items.
[0057] In this application, the "suitable" mentioned in "suitable combination", "suitable method", "any suitable method", etc. is based on the ability to implement the technical solution of this application, solve the technical problems of this application, and achieve the expected technical effects of this application.
[0058] In the present application, "preferred", "better", "more preferred" and "suitable" are only used to describe implementation methods or examples with better effects. It should be understood that they do not constitute limitations on the scope of protection of the present application.
[0059] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.
[0060] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0061] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0062] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0063] In the present application, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges included therein.
[0064] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0065] In the present application, % (w / w) and wt% both represent weight percentage, % (v / v) refers to volume percentage, and % (w / v) refers to mass volume percentage.
[0066] The "room temperature" in this application generally refers to 5°C to 30°C, preferably 25±5°C.
[0067] In one embodiment, a super hydrophobic coating is provided, comprising a polymer matrix containing Diels-Alder bonds and microcapsules and super hydrophobic nanoparticles dispersed in the polymer matrix.
[0068] The microcapsule comprises a core material and a capsule wall covering the core material;
[0069] The core material includes a low surface energy substance and a fluorescent dye;
[0070] Super hydrophobic nanoparticles are prepared by modifying hydrophobic nanoparticles using a modifier.
[0071] In one embodiment, the low surface energy substance is one or more fluorinated alkyl silanes such as 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, tridecafluorooctyltriethoxysilane, (3,3,3-trifluoropropyl)methyldiethoxysilane, etc.
[0072] In one embodiment, the fluorescent dye is any one of organic small molecules having fluorescent properties such as fluorescein isothiocyanate, 2',7'-dichlorofluorescein, 2',7'-difluorofluorescein, and crystal violet lactone.
[0073] In one embodiment, the hydrophobic nanoparticles are one or more of nano-silicon dioxide, nano-titanium dioxide, nano-aluminum oxide, and nano-zinc oxide.
[0074] In one embodiment, the modifier is one or more of methyltriethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, trimethylchlorosilane, and polydimethylsiloxane.
[0075] In one embodiment, the raw materials for preparing the capsule wall of the microcapsule include polymer prepolymer, organic solvent containing ester group and benzene ring, urea, ammonium chloride, phenol organic matter, and maleic anhydride copolymer.
[0076] In one embodiment, the polymer matrix containing Diels-Alder bonds is one or more of polyurethane containing Diels-Alder bonds, epoxy resin containing Diels-Alder bonds, and acrylate containing Diels-Alder bonds.
[0077] In one embodiment, in the superhydrophobic coating provided, the mass ratio of the microcapsules, the superhydrophobic nanoparticles and the polymer matrix containing Diels-Alder bonds is (0.05~0.5):(0.5~2):(1.5~2), for example, 0.05:0.5:1.5, 0.05:0.5:2, 0.05:2:1.5, 0.5:0.5:1.5, 0.5:2:1.5, 0.5:2:2, 0.3:1:1.5 or a range selected from any two of the foregoing ratios.
[0078] In one embodiment, the diameter of the microcapsule is 10 μm to 100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm or a range consisting of any two of the foregoing values.
[0079] In one embodiment, the particle size of the superhydrophobic nanoparticles is 10 nm to 800 nm, for example, 10 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm or a range selected from any two of the foregoing values.
[0080] In one embodiment, a method for preparing microcapsules in a super-hydrophobic coating is provided, comprising the steps of:
[0081] Mix urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water, and adjust the pH to 2-4 to obtain a first solution;
[0082] Mixing the fluorescent dye, the polymer prepolymer, the low surface energy substance and the organic solvent containing the ester group and the benzene ring to obtain a second solution;
[0083] The second solution is mixed with the first solution, a first reaction is carried out, formaldehyde is added, a second reaction is carried out, the mixture is washed with water, and the mixture is dried to obtain microcapsules loaded with low surface energy substances and fluorescent dyes.
[0084] In one embodiment, a method for preparing microcapsules in a super-hydrophobic coating is provided, comprising the steps of:
[0085] Mix urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water, and adjust the pH to 2-4 to obtain a first solution;
[0086] Mixing the fluorescent dye, the polymer prepolymer, the low surface energy substance and the organic solvent containing the ester group and the benzene ring to obtain a second solution;
[0087] The second solution is added to the first solution to carry out a first reaction, formaldehyde is added, a second reaction is carried out, the solution is washed with water, and the solution is dried to obtain microcapsules loaded with low surface energy substances and fluorescent dyes.
[0088] In one embodiment, in the method for preparing microcapsules, the mass ratio of urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water is (0.1-2): (0.01-0.2): (0.01-0.2): (1-5): (40-80), and the mass ratio of urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water can also be (0.9-1): (0.08-0.09): (0.07-0.08): (2.4-2.5): (50-60).
[0089] In one embodiment, in the method for preparing microcapsules, the mass ratio of the fluorescent dye, the polymer prepolymer, the low surface energy substance, and the organic solvent containing an ester group and a benzene ring is (0.02-0.05): (0.8-1): (10-20): (5-10).
[0090] In one embodiment, the polyurethane prepolymer in the raw material for preparing the capsule wall of the microcapsule includes any one of Desmodur L75 (purchased from Covestro AG), Desmodur L60 (purchased from Covestro AG), Elastospray L 100 (purchased from BASF AG), and Arcol PU 3000 (purchased from Arco Chemicals).
[0091] In one embodiment, in the raw materials for preparing the capsule wall of the microcapsule, the organic solvent containing an ester group and a benzene ring includes one or more of phenyl acetate and ethyl phenylacetate.
[0092] In one embodiment, the phenolic organic matter in the raw materials for preparing the capsule wall of the microcapsule includes one or more of phenol, resorcinol and catechol.
[0093] In one embodiment, in the raw materials for preparing the capsule wall of the microcapsule, the maleic anhydride copolymer includes one or more of vinyl maleic anhydride copolymer and styrene maleic anhydride copolymer.
[0094] In one embodiment, in the raw materials for preparing the capsule wall of the microcapsule, the average molecular weight of the vinyl maleic anhydride copolymer is 300,000-500,000, for example, 300,000, 400,000, or 500,000.
[0095] In one embodiment, in the method for preparing microcapsules, the volume ratio of the first solution to the second solution is (5-7): (2-3).
[0096] In one embodiment, in the method for preparing microcapsules, the volumes of formaldehyde and the second solution are (1-1.5):(10-15).
[0097] In one embodiment, in the method for preparing microcapsules, the first reaction is carried out at a rotation speed of 400 rpm to 800 rpm, for example, 400 rpm, 500 rpm, 600 rpm, 700 rpm, and 800 rpm.
[0098] The first reaction time is 10 min~15 min.
[0099] In one embodiment, in the method for preparing microcapsules, the second reaction is carried out for 4 hours to 5 hours.
[0100] In one embodiment, a method for preparing super-hydrophobic nanoparticles in a super-hydrophobic coating is provided, comprising the following steps:
[0101] The hydrophobic nanoparticles are dispersed in an alcohol solvent, a modifier is added, a third reaction is carried out, the solvent is washed with alcohol, and the solvent is dried to obtain super hydrophobic nanoparticles.
[0102] In one embodiment, in the method for preparing superhydrophobic nanoparticles, the hydrophobic nanoparticles are dispersed in an alcohol solvent step, and the final concentration of the hydrophobic nanoparticles is 0.05 g / mL to 0.25 g / mL, for example, 0.05 g / mL, 0.1 g / mL, 0.15 g / mL, 0.2 g / mL, 0.25 g / mL or a range selected from any two of the foregoing values.
[0103] In one embodiment, in the method for preparing super-hydrophobic nanoparticles, in the step of dispersing the hydrophobic nanoparticles in an alcohol solvent, the alcohol solvent includes one or more of ethanol and n-butanol.
[0104] In one embodiment, in the method for preparing superhydrophobic nanoparticles, the hydrophobic nanoparticles are dispersed in an alcohol solvent, and in the step of adding a modifier, the final concentration of the modifier is 0.05 g / mL to 0.1 g / mL, for example, 0.05 g / mL, 0.06 g / mL, 0.07 g / mL, 0.08 g / mL, 0.09 g / mL, 0.1 g / mL or a range selected from any two of the foregoing values.
[0105] In one embodiment, in the method for preparing superhydrophobic nanoparticles, the temperature for carrying out the third reaction is 20°C to 60°C, for example, 20°C, 30°C, 40°C, 50°C, 60°C or a range selected from any two of the foregoing values.
[0106] In one embodiment, in the method for preparing superhydrophobic nanoparticles, the time for the third reaction is 5 h to 15 h, for example, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h or a range selected from any two of the foregoing values.
[0107] In one embodiment, in the method for preparing superhydrophobic nanoparticles, the third reaction is carried out at a rotation speed of 300 rpm to 800 rpm, for example, 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm or a range selected from any two of the foregoing values.
[0108] In one embodiment, the preparation method of the polymer matrix containing Diels-Alder bonds in the super hydrophobic coating provided comprises: using a raw material including a furan-terminated polymer prepolymer containing a double bond and maleimide (as an olefin) to perform a cycloaddition reaction, and the reaction formula is simplified as follows: .
[0109] In one embodiment, the preparation method of the polymer matrix containing Diels-Alder bonds in the super-hydrophobic coating provided comprises: dissolving maleimide in a solvent, adding a furan-terminated polymer prepolymer, and performing a cycloaddition reaction to prepare a polymer matrix containing Diels-Alder bonds. The polymer matrix prepared by the furan and maleimide system contains abundant reversible DA bonds.
[0110] In one embodiment, in the method for preparing a polymer matrix containing Diels-Alder bonds, the mass ratio of maleimide, solvent and furan-terminated polymer prepolymer is (50-60): (5-10): (40-50).
[0111] In one embodiment, in the method for preparing a polymer matrix containing Diels-Alder bonds, in the step of dissolving maleimide in a solvent, the solvent comprises N,N-dimethylformamide.
[0112] In one embodiment, in the method for preparing a polymer matrix containing Diels-Alder bonds, maleimide is dissolved in a solvent, a furan-terminated polymer prepolymer is added, and a reaction step is performed at a reaction temperature of 60°C to 70°C.
[0113] In one embodiment, in the method for preparing a polymer matrix containing Diels-Alder bonds, maleimide is dissolved in a solvent, a furan-terminated polymer prepolymer is added, and a reaction step is performed, and the reaction time is 20 hours to 30 hours.
[0114] In one embodiment, the furan-terminated polymer prepolymer includes one or more of a furan-terminated polyurethane prepolymer, a furan-terminated epoxy prepolymer, and a furan-terminated acrylate prepolymer.
[0115] In one embodiment, the method for preparing a furan-terminated polyurethane prepolymer comprises the following steps: subjecting polyisocyanate, polyol and solvent to a fourth reaction in an inert gas atmosphere, adding furfurylamine, and subjecting the polyurethane prepolymer to a fifth reaction to prepare the furan-terminated polyurethane prepolymer.
[0116] In one embodiment, in the method for preparing a furan-terminated polyurethane prepolymer, the mass ratio of polyisocyanate, polyol, solvent, and furfurylamine is (8-10): (40-50): (5-10): (3-5).
[0117] In one embodiment, the polyisocyanate comprises 4,4-diisocyanate dicyclohexylmethane.
[0118] In one embodiment, the polyol comprises polypropylene glycol.
[0119] In one embodiment, the temperature for carrying out the fourth reaction is 70°C to 80°C.
[0120] In one embodiment, the fourth reaction is carried out for 10 min to 30 min.
[0121] In one embodiment, the fifth reaction is carried out at 20° C. to 30° C. for 2 h to 4 h, and then at 60° C. to 70° C. for 20 min to 60 min.
[0122] In one embodiment, the maleimide includes any one of N,N′-(4,4′-methylenediphenyl)bismaleimide, N,N′-cyclohexylmaleimide, N,N′-tetrahydrofuranmaleimide, N,N′-dimethylmaleimide, and N,N′-phenylmaleimide.
[0123] In one embodiment, a method for preparing a super hydrophobic coating is provided, wherein raw materials including microcapsules, super hydrophobic nanoparticles and a polymer matrix containing Diels-Alder bonds are mixed to prepare the super hydrophobic coating.
[0124] In one embodiment, there is provided an application of the super-hydrophobic coating or the super-hydrophobic coating prepared by the preparation method in preparing a super-hydrophobic coating with self-warning and self-repairing functions.
[0125] In one embodiment, a super-hydrophobic coating with self-warning and self-repairing functions is provided, wherein the coating comprises the super-hydrophobic coating or is obtained by solidifying the raw materials of the super-hydrophobic coating prepared by the preparation method.
[0126] In one embodiment, the super hydrophobic coating is uniformly dispersed in an organic solvent, coated on the surface of a substrate, and cured at 50-100° C. to evaporate the solvent and finally obtain a super hydrophobic coating.
[0127] In one embodiment, the super hydrophobic coating is uniformly dispersed in an organic solvent step, and the organic solvent is any one of ethanol, butyl acetate, ethyl acetate, and butyl butyrate.
[0128] The self-repair of super-hydrophobic coating is mainly reflected in two aspects, one is the repair of surface free energy, and the other is the repair of physical structure damage. By pre-embedding hydrophobic agents in the coating, after damage, these hydrophobic agents are released and migrate to the damaged area to achieve the recovery of surface free energy. The super-hydrophobic coating provided includes microcapsules loaded with low surface energy substances and fluorescent dyes, super-hydrophobic nanoparticles and polymer matrix containing Diels-Alder bonds. The core material of the microcapsules loaded with low surface energy substances and fluorescent dyes includes low surface energy substances and fluorescent dyes, and the polymer matrix containing Diels-Alder bonds contains abundant dynamic chemical bonds. The super-hydrophobic coating prepared by the super-hydrophobic coating provided has damage self-warning and self-repairing functions. When the surface of the super-hydrophobic coating is damaged, the damaged part will show a fluorescent signal, and release low surface energy substances to restore the super-hydrophobicity of the coating. After heat treatment, the chemical bonds inside the coating will undergo a process of first breaking and then reconnecting, further repairing the mechanical damage of the coating and achieving complete repair of the coating damage. It not only realizes the early warning of coating damage, but also can simultaneously repair the superhydrophobic properties and structural damage of the coating, improving the repair efficiency while significantly extending the service life of the superhydrophobic coating, and has broad development prospects.
[0129] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are illustrative, not restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.
[0130] The vinyl maleic anhydride copolymer used in the following examples and comparative examples has an average molecular weight of 400,000 and is purchased from Sigma-Aladdin Reagent Co., Ltd.; the polyurethane prepolymer is Desmodur L 75, purchased from Covestro AG; and the styrene-based maleic anhydride copolymer is purchased from Sigma-Aldrich, model SMA 1000.
[0131] Example 1
[0132] 1. Dissolve 0.9 g urea, 0.08 g ammonium chloride, and 0.07 g phenol in 50 mL (0.05 g / mL) aqueous solution of vinyl maleic anhydride copolymer, adjust the solution pH to 3.5, and transfer to a flask; evenly mix 0.03 g fluorescent dye, 0.8 g polyurethane prepolymer, 12 mL low surface energy material 1H,1H,2H,2H-perfluorooctyltriethoxysilane, and 10 mL phenyl acetate, add dropwise to the flask, and react at room temperature and 600 rpm for 15 min, add 2.5 g formaldehyde, and continue the reaction for 4 h; after the reaction is completed, the emulsion is continuously rinsed with deionized water, filtered, and dried in a vacuum freeze dryer for 24 h to achieve microcapsules.
[0133] 2. Dissolve 5 g of nano-silica in 100 mL of n-butanol, stir for 20 min, add 7 g of methyltriethoxysilane, react for 12 h at 25 °C and 400 rpm, wash with anhydrous ethanol three times, and finally dry it in a 60 °C oven for 12 h to obtain superhydrophobic nano-silica.
[0134] 3. 9.8 g of 4,4-diisocyanate dicyclohexylmethane, 40 g of polypropylene glycol, and 5 mL of N,N-dimethylformamide were placed in a flask and reacted at 75 °C and 500 rpm for 15 min under a nitrogen environment. After cooling, 3.85 g of furfurylamine was added and the reaction continued at 25 °C and 500 rpm for 3 h, and then at 65 °C for 30 min to obtain a furan-terminated polyurethane prepolymer. Then 7.3 g of N,N′-(4,4′-methylenediphenyl)bismaleimide was dissolved in 42 mL of N,N-dimethylformamide DMF and added to the furan-terminated polyurethane prepolymer, and reacted at 60 °C and 500 rpm for 24 h to finally obtain a polyurethane containing DA bonds.
[0135] 4. Disperse 0.5 g microcapsules, 1.5 g super-hydrophobic nano-silica, and 2 g polyurethane coating evenly in 40 mL of ethanol solution, spray the mixed solution evenly on the cleaned glass surface with a spray gun, and cure it in a 70 °C oven to evaporate the solvent to finally obtain a super-hydrophobic coating.
[0136] Figure 1 This is a scanning electron microscope image of the microcapsules prepared in Example 1. Figure 2 This is a scanning electron microscope image of the super-hydrophobic nano-SiO2 prepared in Example 1. Figure 3 The water contact angle of the superhydrophobic coating was measured by a contact angle meter (JC2000C1, Shanghai Zhongchen). Five different positions were taken for each sample and the average value was taken. Figure 1 It can be found that the microcapsules are spherical with a diameter of about 25 μm, ensuring sufficient internal space to load low surface energy substances and fluorescent dyes. Figure 2 It can be found that the shape of super-hydrophobic nano-SiO2 is relatively regular and the size is about 150 nm. Figure 3 It can be seen that the water contact angle of the coating is about 156.4°, indicating that the coating has superhydrophobic properties.
[0137] Example 2
[0138] 1. Dissolve 1 g urea, 0.09 g ammonium chloride, and 0.08 g phenol in 60 mL (0.04 g / mL) vinyl maleic anhydride copolymer aqueous solution, adjust the solution pH to 3.5, and transfer to a flask; evenly mix 0.04 g fluorescent dye, 1 g polyurethane prepolymer, 15 mL low surface energy material 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and 10 mL phenyl acetate, add dropwise to the flask, and react at room temperature and 800 rpm for 10 min, add 2.7 g formaldehyde, and continue the reaction for 4.5 h; after the reaction is completed, the emulsion is continuously rinsed with deionized water, filtered, and dried in an oven for 24 h to achieve microcapsules.
[0139] 2. Dissolve 8 g of nano-titanium dioxide in 100 mL of ethanol, stir for 20 min, add 8 g of dimethyldiethoxysilane, continue the reaction at 30 °C and 600 rpm for 8 h, and wash it with deionized water 3 times. Finally, place it in an oven at 80 °C and dry it for 10 h to obtain superhydrophobic nano-titanium dioxide.
[0140] 3. Place 10 g of 4,4-diisocyanate dicyclohexylmethane, 45 g of polypropylene glycol, and 7 mL of N,N-dimethylformamide in a flask and react at 70 °C and 600 rpm for 20 min under a nitrogen environment. After cooling, add 4 g of furfurylamine and continue to react at 25 °C and 600 rpm for 3 h, then keep at 60 °C for 30 min to obtain a furan-terminated polyurethane prepolymer. Then dissolve 7.5 g of N,N′-(4,4′-methylenediphenyl)bismaleimide in 45 mL of N,N-dimethylformamide DMF and add it to the furan-terminated polyurethane prepolymer. React at 65 °C and 600 rpm for 22 h to finally obtain a polyurethane containing DA bonds.
[0141] 4. Disperse 0.4 g microcapsules, 1.5 g super-hydrophobic nano-silica, and 1.5 g polyurethane coating evenly in 40 mL of ethanol solution, spray the mixed solution evenly on the cleaned glass surface with a spray gun, and cure it in a 60 °C oven to evaporate the solvent to finally obtain a super-hydrophobic coating.
[0142] Figure 4 This is a microscopic image of the super-hydrophobic coating prepared in Example 2 after damage. Figure 5 This is a microscopic image of the super-hydrophobic coating prepared in Example 2 after repair. Figure 6 The water contact angles of the intact coating, damaged coating, and repaired coating. Figure 7 Fluorescence images before and after coating restoration. Figure 4 It can be seen that there are obvious scratches on the damaged super-hydrophobic coating, and the scratch width is about 150 μm. If it is not repaired in time, the performance of the coating will be seriously affected. Figure 5 It can be seen that the coating was scratched with a scalpel and then placed in an oven at 100°C for 2 hours for repair. After the repair, the scratches on the surface of the coating disappeared, leaving only tiny traces of the coating repair, which fully demonstrates the excellent self-healing properties of the coating. Figure 6 It can be seen that the water contact angle of the complete coating is 154°, and the hydrophobic property is excellent; however, once the coating is damaged, the hydrophobic property drops sharply, which will inevitably cause the corrosion reaction to intensify; it is worth noting that the water contact angle of the repaired coating is still above 110°, which on the one hand indicates that the coating has a good hydrophobic effect, and on the other hand also indicates that the coating has excellent self-healing performance. Figure 7 It can be seen that the damaged coating shows obvious warning signals, while the warning signals disappear after the repair. Therefore, the fluorescent signal can be used to track the repair status of the coating.
[0143] Comparative Example 1
[0144] This comparative example provides a coating without super-hydrophobic nanoparticles and a preparation method thereof, which specifically comprises the following steps:
[0145] 1. Dissolve 0.8 g urea, 0.08 g ammonium chloride, and 0.07 g phenol in 55 mL (0.05 g / mL) aqueous solution of vinyl maleic anhydride copolymer, adjust the solution pH to 3.4, and transfer to a flask; evenly mix 0.02 g fluorescent dye, 0.9 g polyurethane prepolymer, 13 mL low surface energy material 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and 12 mL phenyl acetate, add dropwise to the flask, and react at room temperature and 500 rpm for 15 min, add 2.7 g formaldehyde, and continue the reaction for 4.5 h; after the reaction is completed, the emulsion is continuously rinsed with deionized water, filtered, and dried in a vacuum freeze dryer for 36 h to achieve microcapsules.
[0146] 3. Place 9.9 g of 4,4-diisocyanate dicyclohexylmethane, 41 g of polypropylene glycol, and 5 mL of N,N-dimethylformamide in a flask and react at 75 °C and 500 rpm for 15 min under a nitrogen environment. After cooling, add 3.9 g of furfurylamine and continue to react at 25 °C and 500 rpm for 3 h, then keep at 65 °C for 40 min to obtain a furan-terminated polyurethane prepolymer. Then dissolve 7.5 g of N,N′-(4,4′-methylenediphenyl)bismaleimide in 40 mL of N,N-dimethylformamide DMF and add it to the furan-terminated polyurethane prepolymer. React at 60 °C and 500 rpm for 24 h to finally obtain a polyurethane coating containing DA bonds.
[0147] 4. Disperse 0.4 g microcapsules and 1.8 g polyurethane coating evenly in 38 mL ethanol solution, spray the mixed solution evenly on the cleaned glass surface with a spray gun, and cure it in a 75 °C oven to evaporate the solvent to finally obtain a superhydrophobic coating.
[0148] Figure 8 The water contact angle of the polyurethane coating lacking superhydrophobic nanoparticles in Comparative Example 1 is shown. Figure 8 It can be seen that the water contact angle of the polyurethane coating is 72.7°, which does not have hydrophobic properties and does not meet the requirements of super-hydrophobic coatings. Therefore, the super-hydrophobic nanoparticles loaded in the microcapsules are a key link in achieving the super-hydrophobic properties of the coating.
[0149] Comparative Example 2
[0150] This comparative example provides a super-hydrophobic coating lacking a DA bond and a preparation method thereof, which specifically comprises the following steps:
[0151] 1 g urea, 0.08 g ammonium chloride, and 0.09 g phenol were dissolved in 55 mL (0.05 g / mL) styrene-maleic anhydride copolymer aqueous solution, the pH of the solution was adjusted to 3.5, and the solution was transferred to a flask; 0.05 g fluorescent dye, 0.9 g polyurethane prepolymer, 14 mL low surface energy material 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and 10 mL ethyl phenylacetate were evenly mixed, added dropwise to the flask, and reacted at room temperature and 900 rpm for 10 min, 2.6 g formaldehyde was added, and the reaction was continued for 4 h; after the reaction was completed, the emulsion was continuously rinsed with deionized water, filtered, and dried in an oven for 30 h to obtain microcapsules.
[0152] 2. Dissolve 9 g of nano-titanium dioxide in 110 mL of ethanol, stir for 20 min, add 8.5 g of dimethyldiethoxysilane, continue the reaction at 30 °C and 550 rpm for 8 h, wash it with deionized water 4 times, and finally place it in an oven at 80 °C and dry it for 12 h to obtain superhydrophobic nano-titanium dioxide.
[0153] 3. Take 3.5 g of bisphenol A diglycidyl ether, 1.3 g of polyetheramine, 0.5 g of microcapsules, and 1.2 g of super-hydrophobic nano-silica, mix them thoroughly under a magnetic stirrer at 600 rpm, and evenly disperse them in 45 mL of ethanol solution. Spray the mixed solution evenly on the cleaned glass surface with a spray gun, and cure it in an oven at 70 °C to evaporate the solvent to finally obtain a super-hydrophobic coating.
[0154] Fig. 9 The water contact angle of the superhydrophobic coating lacking DA bonds in Comparative Example 2 is shown after being scratched with a scalpel and repaired in an 80°C oven for 3 h. Fig. 9 It can be seen that the water contact angle of the repaired coating is about 75°, which still does not have super hydrophobic properties. On the contrary, the super hydrophobic coating containing DA bonds in Example 2 has a water contact angle of 112.9° after repair. In summary, the presence of DA bonds in microcapsules plays an important role in restoring the hydrophobic properties of the coating.
[0155] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0156] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description and drawings may be used to interpret the content of the claims.
Claims
1. A super hydrophobic coating, characterized in that, The invention comprises a polymer matrix containing Diels-Alder bonds and microcapsules and super-hydrophobic nanoparticles dispersed in the polymer matrix. The microcapsule comprises a core material and a capsule wall covering the core material; The core material includes a low surface energy substance and a fluorescent dye; The super hydrophobic nanoparticles are prepared by modifying hydrophobic nanoparticles using a modifier.
2. Super hydrophobic coating according to claim 1, characterised in that, Meet one or more of the following characteristics: (1) The low surface energy substance is one or more of fluorinated alkyl silanes such as 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, tridecafluorooctyltriethoxysilane, (3,3,3-trifluoropropyl)methyldiethoxysilane, etc.; (2) The fluorescent dye is one or more of fluorescein isothiocyanate, 2',7'-dichlorofluorescein, 2',7'-difluorofluorescein, and crystal violet lactone, which are organic small molecules with fluorescent properties; (3) The hydrophobic nanoparticles are one or more of nano-silicon dioxide, nano-titanium dioxide, nano-aluminum oxide and nano-zinc oxide; (4) The modifier is one or more of methyltriethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, trimethylchlorosilane and polydimethylsiloxane; (5) The raw materials for preparing the capsule wall of the microcapsule include polymer prepolymer, organic solvent containing ester group and benzene ring, urea, ammonium chloride, phenol organic matter, and maleic anhydride copolymer; (6) The polymer matrix containing Diels-Alder bonds is one or more of polyurethane containing Diels-Alder bonds, epoxy resin containing Diels-Alder bonds, and acrylate containing Diels-Alder bonds; (7) The mass ratio of the microcapsule, the super-hydrophobic nanoparticles and the polymer matrix containing Diels-Alder bonds is (0.05-0.5): (0.5-2): (1.5-2); (8) The diameter of the microcapsule is 10 μm to 100 μm; (9) The particle size of the super hydrophobic nanoparticles is 10 nm to 800 nm.
3. The super hydrophobic coating according to claim 1 or 2, characterized in that, The preparation method of the microcapsules comprises the steps of: Mix urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water, and adjust the pH to 2-4 to obtain a first solution; Mixing the fluorescent dye, the polymer prepolymer, the low surface energy substance and the organic solvent containing the ester group and the benzene ring to obtain a second solution; The second solution is mixed with the first solution, a first reaction is carried out, formaldehyde is added, a second reaction is carried out, the mixture is washed with water, and the mixture is dried to obtain the microcapsules.
4. The super hydrophobic coating according to claim 3, wherein The method for preparing the microcapsules satisfies one or more of the following characteristics: (1) The mass ratio of urea, ammonium chloride, phenolic organic matter, maleic anhydride copolymer and water is (0.1~2): (0.01~0.2): (0.01~0.2): (1~5): (40~80); (2) The mass ratio of fluorescent dye, polymer prepolymer, low surface energy substance, and organic solvent containing ester group and benzene ring is (0.02~0.05): (0.8~1): (10~20): (5~10); (3) The volume ratio of the first solution to the second solution is (5-7):(2-3); (4) Volume ratio of formaldehyde to the second solution (1-1.5):(10-15); (5) performing the first reaction at a rotation speed of 400 rpm to 800 rpm for 10 min to 15 min; (6) The second reaction is carried out for 4 to 5 hours.
5. according to the super hydrophobic coating described in any one of claims 1 to 4, it is characterised in that The preparation method of the super-hydrophobic nanoparticles comprises the following steps: The hydrophobic nanoparticles are dispersed in an alcohol solvent, a modifier is added, a third reaction is carried out, the solvent is washed with alcohol, and the solvent is dried to obtain super hydrophobic nanoparticles.
6. The super hydrophobic coating according to claim 5, wherein The method for preparing the super-hydrophobic nanoparticles satisfies one or more of the following characteristics: (1) In the step of dispersing the hydrophobic nanoparticles in the alcohol solvent, the final concentration of the hydrophobic nanoparticles is 0.05 g / mL to 0.25 g / mL; (2) In the step of dispersing the hydrophobic nanoparticles in an alcohol solvent and adding a modifier, the final concentration of the modifier is 0.05 g / mL to 0.1 g / mL; (3) The temperature for carrying out the third reaction is 20°C to 60°C; (4) The third reaction is carried out for 5 to 15 hours; (5) The third reaction is carried out at a rotation speed of 300 rpm to 800 rpm.
7. The super hydrophobic coating according to any one of claims 1 to 6, wherein The method for preparing the polymer matrix containing Diels-Alder bonds comprises: performing a cycloaddition reaction using raw materials including a furan-terminated polymer prepolymer containing double bonds and maleimide.
8. A method for preparing a super hydrophobic coating, characterized in that, The raw materials including microcapsules, super-hydrophobic nanoparticles and a polymer matrix containing Diels-Alder bonds are mixed to prepare the super-hydrophobic coating according to any one of claims 1 to 7.
9. the application of the super-hydrophobic coating prepared by the super-hydrophobic coating described in any one of claims 1 to 7 or the preparation method described in claim 8 in preparing a super-hydrophobic coating with self-warning and self-repairing function.
10. A super hydrophobic coating with self-warning and self-repairing functions, characterized in that: The coating comprises the super hydrophobic coating according to any one of claims 1 to 7 or is obtained by curing the raw materials of the super hydrophobic coating prepared by the preparation method according to claim 8.
Citation Information
Patent Citations
Self-repairing water-based super-hydrophobic coating based on microcapsule type and preparing method thereof
CN105885679A
Microcapsule with damage hinting and repairing functions and application thereof in epoxy coating
CN106118367A
Wear-resisting super-hydrophobic coating composition as well as preparation method and application thereof
CN107987675A
Method for converting traditional paint into superhydrophobic paint
CN109777260A
Intelligent self-repairing easy-to-clean anti-fouling nano coating and preparation method thereof
CN112280458A
Cited By
BN-doped photo-thermal super-hydrophobic coating on surface of aluminum alloy and preparation method thereof
CN120230452A