Adhesive film with LDS (Laser Direct Structuring) function and preparation method thereof
By uniformly mixing LDS additives in the adhesive film and activating them during laser engraving, the problems of poor dispersion of additives and reduced mechanical properties in traditional LDS processes are solved, and the preparation of high-precision metal lines on the surface of composite materials and the preparation of high-performance materials are realized. application.
Patent Information
- Application Number
- CN202411234590.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
In the traditional LDS process, metal salt additives are difficult to disperse uniformly in composite materials, resulting in reduced mechanical properties and difficult to meet the performance requirements of large parts.
Adopt a film with LDS function, including resin matrix, additives and diluents. After uniform mixing and grinding, LDS additives are added to form a film, and selective electroless plating is achieved during laser engraving to avoid adding additives to the matrix. In the material.
The preparation of high-precision metal lines on the surface of composite materials has been realized, the application range of LDS processes has been expanded, the mechanical properties of the matrix materials have been maintained, and the needs of high-performance materials have been met.
Smart Images

Figure CN119081558A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adhesive films, and in particular to an adhesive film with LDS function and a preparation method thereof. Background Art
[0002] LDS (Laser Direct Structuring) technology, also known as molded interconnect device (MID), is a process that directly transfers to the target part surface through laser processing, uses the three-dimensional surface of the three-dimensional part to form circuit interconnections, or realizes metallized vias through laser drilling. This traditional process evenly adds LDS activator to the part material, uses laser processing to scan the target pattern, laser activates and shallowly etches the part surface, and uses chemical plating to selectively deposit copper on the patterned part processed by laser to achieve the effect of patterned circuit preparation. In order to achieve the three-proof effect or to be suitable for special processes, other metal materials such as nickel, silver, and gold can also be deposited on the copper layer. The LDS process realizes the rapid manufacturing of three-dimensional circuits quickly, integratedly, and at low cost through simple laser scanning, and is widely used in communications, medical, automotive and other industries. At present, the traditional LDS material is to melt and evenly mix the LDS additive with the thermoplastic plastic to achieve the purpose of laser activation processing. LDS additives are mostly metal salts, which are added to the material body, greatly reducing the mechanical properties of the material. Due to the manufacturing process of thermosetting resins, LDS additives are difficult to mix and add. In addition, the LDS process is currently mainly used for small-sized parts with low requirements for mechanical properties of parts, such as mobile phones, smart watches, headphones, car speaker circuit boards, hearing aids and other consumer electronics parts. For large parts, adding LDS additives is expensive and the process is complicated.
[0003] Adhesive film is a commonly used bonding material in composite materials. It is also used as a surface film to improve the surface quality of composite materials or to obtain surface functionalization through functions. Surface films are often used with the same polymer as the composite prepreg resin and composite materials. They can be used for bonding, surface quality improvement and functionalization of flat and curved parts through paving. Common functional surface films in the aerospace field mainly include conductive adhesive films to achieve lightning protection and electromagnetic shielding.
[0004] For composite materials, due to the continuous fibers contained in them and their unique manufacturing process, LDS additives are difficult to evenly disperse into the material body. At the same time, adding LDS additives, which are generally metal salts, to the non-metallic material body will greatly reduce its mechanical properties and fail to meet the performance requirements of the target parts.
[0005] Therefore, the inventors provide an adhesive film with LDS function and a preparation method thereof. Summary of the invention
[0006] (1) Technical issues to be solved
[0007] The embodiment of the present invention provides an adhesive film with LDS function and a preparation method thereof. The use of this type of new adhesive film can realize the preparation of high-precision metal circuits on the surface of composite materials, and at the same time solves the technical problem that the LDS additive of metal salts is added to the non-metallic material body to reduce its mechanical properties.
[0008] (2) Technical solution
[0009] A first aspect of the present invention provides an adhesive film with LDS function, comprising a release layer, an adhesive layer and a protective layer laminated in sequence, wherein the adhesive layer comprises a resin matrix, an auxiliary agent, a diluent and an LDS additive.
[0010] Furthermore, the resin matrix is any one of a polymer, a monomer capable of generating a polymer, an oligomer and a prepolymer.
[0011] Furthermore, the resin matrix includes at least one of epoxy resin, bismaleimide resin, cyanate resin, polyimide resin, polyurethane, hydroxy polyether, urea-formaldehyde resin, polysiloxane, polysilazane, polysilane, polysilocarbonane, modified epoxy resin, phenolic resin, benzoxazine resin and melamine formaldehyde resin.
[0012] Furthermore, the resin matrix also includes at least one of polyethersulfoneketone, polyetheretherketone, polyaryletherketone, polyethersulfone, polysulfone, polyimide ether, polycarbonate, polyphenylene ether and liquid crystal polymer.
[0013] Furthermore, the weight of the resin matrix is 100 parts, the weight of the auxiliary agent is 0 to 100 parts, the weight of the diluent is 0 to 10 parts, and the weight of the LDS additive is 1 to 30 parts.
[0014] Furthermore, the weight portion of the LDS additive is 3 to 10 parts.
[0015] Furthermore, the LDS additive is a metal salt of copper, arsenic or tin.
[0016] Furthermore, the LDS additive includes at least one of copper chromite, copper hydroxyphosphate, arsenic trioxide and tin dioxide.
[0017] The second aspect of the present invention provides a method for preparing the above-mentioned adhesive film having LDS function, comprising the following steps:
[0018] One or more resin matrices are mixed uniformly using a homogenizer according to a first preset ratio, different types and proportions of additives are added in sequence and stirred uniformly at a predetermined modification temperature, and a diluent is added and mixed according to a second preset ratio to obtain a resin body;
[0019] Adding LDS additive to the resin body according to a third preset ratio, mixing and grinding the mixture thoroughly, and vacuuming and degassing the mixture to obtain a rubber material;
[0020] The adhesive material is made into an adhesive film, the adhesive film is made on a release layer, and covered with a protective layer to obtain an adhesive film with LDS function.
[0021] Furthermore, after obtaining the adhesive film with LDS function, the method further includes: placing the adhesive film with LDS function in an oven for surface drying and pre-curing.
[0022] (3) Beneficial effects
[0023] In summary, the present invention expands the application scope and application scenarios of LDS process (laser engraving-chemical plating) for preparing patterned conductive circuits by adding LDS additives to the film to realize the function of surface LDS activation. Since LDS additives are not added to the matrix material, the matrix properties will not be lost, especially mechanical properties, dielectric properties, etc., which can meet the application of composite materials in the field of high-performance materials. The use of the film can realize the preparation of high-precision metal circuits on the surface of composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments of the present invention are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0025] Figure 1 is a schematic structural diagram of an adhesive film with LDS function provided by an embodiment of the present invention;
[0026] Figure 2 It is a schematic flow chart of a method for preparing a film with LDS function provided in an embodiment of the present invention.
[0027] In the figure:
[0028] 1- Release layer; 2- Adhesive layer; 3- Protective layer. DETAILED DESCRIPTION
[0029] The following detailed description of the embodiments of the present invention is provided in conjunction with the accompanying drawings and examples. The following detailed description of the embodiments and the accompanying drawings are used to illustrate the principles of the present invention, but cannot be used to limit the scope of the present invention, that is, the present invention is not limited to the described embodiments.
[0030] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0031] Figure 1 is a schematic diagram of the structure of a film with LDS function provided by an embodiment of the present invention, such as Figure 1 As shown, the adhesive film may include a release layer 1, an adhesive layer 2 and a protective layer 3 which are laminated in sequence, and the components of the adhesive layer 2 include a resin matrix, an auxiliary agent, a diluent and an LDS additive.
[0032] In the above embodiment, the release layer 1 refers to a thin film layer that can be separated from the adhesive layer 2. The release layer 1 has no stickiness or slight stickiness after contacting with a specific material under limited conditions. It is separated after the film is bonded and does not contact the workpiece or remain on the workpiece, and only supports the adhesive layer 2. The adhesive layer 2 is the core structure of the film and plays a bonding role. The protective layer 3 is used to protect the surface of the adhesive layer 2 during transportation and storage, and is removed before use. The LDS additive is an additive used to activate the reaction during the laser engraving process, thereby realizing selective chemical plating (chemical deposition).
[0033] As an optional embodiment, the resin matrix is any one of a polymer, a monomer, an oligomer and a prepolymer that can generate a polymer. The resin matrix includes at least one of epoxy resin, bismaleimide resin, cyanate resin, polyimide resin, polyurethane, hydroxy polyether, urea-formaldehyde resin, polysiloxane, polysilazane, polysilane, polysilocarbonane, modified epoxy resin, phenolic resin, benzoxazine resin and melamine formaldehyde resin. For bismaleimide resin, cyanate resin, polyimide resin, etc., often by compounding epoxy resin to reduce curing temperature, improve curing efficiency, improve heat resistance. In addition, thermoplastic resins are often added to the resin matrix to improve material toughness, such as polyether sulfone ketone, polyether ether ketone, polyarylether ketone, polyether sulfone, polysulfone, polyimide ether, polycarbonate, polyphenylene oxide, liquid crystal polymer, etc.
[0034] The additives can be curing agents, accelerators, coupling agents, chain extenders, leveling agents, defoamers, drying agents, anti-skinning agents, anti-settling agents, antioxidants, mildew inhibitors, plasticizers, slow-release agents, rust removers, foaming agents, photosensitizers, tackifiers, etc. The additives here can also be powders, particles, microbeads, and fibers added to improve the performance of the film, such as polymer powders, polytetrafluoroethylene powders, liquid crystal polymer powders, glass microbeads, ceramic microbeads, carbon nanotubes, graphene, aluminum oxide (corundum), zinc oxide, titanium dioxide, mullite, calcium carbonate, magnesium carbonate, calcium silicate, aluminum silicate, magnesium silicate, potassium aluminum silicate, barium sulfate, silicon carbide, silicon nitride, boron nitride, silicon dioxide, whiskers, zirconium dioxide, yttrium dioxide, tungsten sulfide, adamantane, montmorillonite, nano silver, cage Type polyhedral oligomeric silsesquioxane (POSS), MXene, ferrite, color powder, etc., such as continuous or chopped fibers, organic fibers, inorganic fibers or metal wires, including carbon fiber, glass fiber, quartz fiber, mullite fiber, basalt fiber, lignin fiber, natural fiber, carbon nanotube fiber, ceramic fiber, boron fiber, aramid fiber, Kevlar fiber, ultra-high molecular weight polyethylene fiber, liquid crystal polymer (LCP), optical fiber, polyaryletherketone fiber, nylon fiber, polyimide fiber, etc.
[0035] Diluent is a solvent used to adjust the viscosity of the film. It is sometimes added in small amounts during the mixing process to promote the dissolution of the resin. The diluent is mainly selected according to the type of resin and can be water, butanone, acetone, cyclohexanone, methanol, ethanol, isopropanol, etc.
[0036] As an optional embodiment, the weight of the resin matrix is 100 parts, the weight of the auxiliary agent is 0-100 parts, the weight of the diluent is 0-10 parts, and the weight of the LDS additive is 1-30 parts. Furthermore, the weight of the LDS additive is 3-10 parts.
[0037] As an optional embodiment, the LDS additive is a metal salt of copper, arsenic or tin. Specifically, the LDS additive may include at least one of copper chromite, copper hydroxyphosphate, arsenic trioxide and tin dioxide. Here, it should be noted that the selection of the ingredients of the LDS additive is a key factor affecting the quality of the film. Adding too much additive will affect the mechanical properties of the film, the adhesion to the substrate, and the additive is difficult to disperse evenly in the film, thereby affecting the quality of the metal circuit on the surface after the film is finally cured. Adding too little additive will cause the material to have poor laser activation performance, which is mainly manifested in the inability to prepare metal circuits due to the lack of plating after laser processing, or the need for many laser processing times, which affects the production schedule, or the power required during the laser processing is high, which affects the accuracy of the metal circuit.
[0038] Figure 2is a schematic diagram of a process for preparing a film having LDS function provided by an embodiment of the present invention, such as Figure 2 As shown, the method may include the following steps:
[0039] S100, one or more resin matrices are mixed uniformly using a homogenizer according to a first preset ratio, additives of different types and ratios are added in sequence and stirred uniformly at a predetermined modification temperature, and a diluent is added and mixed according to a second preset ratio to obtain a resin body.
[0040] Specifically, according to different formulas of the resin matrix, different types and proportions of additives are added in sequence and stirred evenly at a speed of 300 to 2000 r / min at a predetermined modification temperature.
[0041] S200, adding LDS additive to the resin body according to a third preset ratio, fully mixing and grinding, and vacuuming and degassing to obtain a rubber material.
[0042] Specifically, due to the high viscosity of the rubber, the LDS additive is a powder material with a small particle size, light density and strong viscosity-increasing effect, which makes it difficult to disperse evenly in the rubber. Therefore, it is necessary to regulate the viscosity of the rubber, add various additives to adjust, and select a suitable modification temperature based on the characteristics of the resin, combined with the curing curve and the temperature-viscosity curve. For rubber with high viscosity, the viscosity is reduced by mixing with a diluent to facilitate the addition of the LDS additive. And according to the different resin formula components and viscosity, a suitable additive dispersion method can be selected, mainly including one or more of mechanical stirring, ball mill, open mill, and three-roll grinder.
[0043] S300, making the adhesive material into an adhesive film, making the adhesive film on the release layer, and covering it with a protective layer to obtain an adhesive film with LDS function.
[0044] Specifically, the manufacturing method can adopt a laminating machine to press into a film, or adopt a casting machine to cast into a film, or coat the rubber material on a base film.
[0045] As an optional implementation, after obtaining the adhesive film with LDS function in step S300, the method further includes: placing the adhesive film with LDS function in an oven for surface drying and pre-curing. According to different resin systems, some adhesive films need to be further heated in an oven for surface drying and step pre-curing.
[0046] Example 1
[0047] The method for preparing a film having LDS function comprises the following steps:
[0048] (1) Add 100 parts of bisphenol A epoxy resin and 40 parts of elastomer toughening agent in a container, stir at 80°C for 0.5h, and cool to room temperature; disperse 30 parts of dicyandiamide curing agent, 10 parts of polyester chain extender, 1 part of accelerator, 1 part of defoamer, and 5 parts of LDS additive in a homogenizer at a speed of 800r / min for 5min, then increase the temperature to 120°C and stir for modification for 2h; use vacuum degassing in a vacuum homogenizer for 10min to remove internal tiny bubbles;
[0049] (2) Preheat the bottom plate of the film forming machine to 70°C, and use the film forming machine to hot-press and calender the film to control the film thickness to 200 μm.
[0050] Example 2
[0051] The method for preparing a film having LDS function comprises the following steps:
[0052] (1) Weigh 100 parts of bismaleimide resin, 50 parts of allyl bisphenol A or bisphenol A bisallyl ether, 1 part of stabilizer, and 3 parts of antioxidant in a kneader, and knead at 130° C. for 30 minutes;
[0053] (2) adding 10 parts of thermoplastic toughening agent and 3 parts of LDS additive into a kneader at 100° C., kneading for 10 to 30 minutes, and then vacuum kneading for 30 minutes;
[0054] (3) The rubber compound is formed into a film on a hot melt laminating machine at 80°C, and the film thickness is controlled to be 100 μm.
[0055] Example 3
[0056] The method for preparing a film having LDS function comprises the following steps:
[0057] (1) 100 parts by mass of bisphenol A cyanate resin, 50 parts by mass of phenolic cyanate resin, and 50 parts by mass of bismaleimide modified cyanate resin were added into an internal mixer and kneaded at 130° C. for 30 min;
[0058] (2) Add 20 parts by weight of acrylic elastomer toughening agent, 2 parts by weight of accelerator, 1 part by weight of coupling agent, and 1 part by weight of antioxidant into an internal mixer, and continue mixing at 90° C. for 20 minutes;
[0059] (3) Take out the rubber material, put it into a vacuum drying oven, and vacuum dry it at 60°C for 20 min;
[0060] (4) The above-mentioned rubber compound was formed into a film on a three-roller film-coating machine at 80°C, and the film thickness was controlled to be 120 μm.
[0061] It should be clear that the various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The present invention is not limited to the specific steps and structures described above and shown in the figures. In addition, for the sake of brevity, a detailed description of known methods and technologies is omitted here.
[0062] The above are only embodiments of the present application and are not limited to the present application. For those skilled in the art, the present application may have various changes and variations without departing from the scope of the present invention. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A film having LDS function, characterized in that: It comprises a release layer (1), an adhesive layer (2) and a protective layer (3) which are laminated in sequence, wherein the adhesive layer (2) comprises components of a resin matrix, an auxiliary agent, a diluent and an LDS additive.
2. The adhesive film with LDS function according to claim 1, characterized in that: The resin matrix is any one of a polymer, a monomer capable of generating a polymer, an oligomer and a prepolymer.
3. The adhesive film with LDS function according to claim 1 or 2, characterized in that: The resin matrix includes at least one of epoxy resin, bismaleimide resin, cyanate resin, polyimide resin, polyurethane, hydroxy polyether, urea-formaldehyde resin, polysiloxane, polysilazane, polysilane, polysilocarbonane, modified epoxy resin, phenolic resin, benzoxazine resin and melamine formaldehyde resin.
4. The adhesive film with LDS function according to claim 3, characterized in that: The resin matrix also includes at least one of polyethersulfoneketone, polyetheretherketone, polyaryletherketone, polyethersulfone, polysulfone, polyimide ether, polycarbonate, polyphenylene ether and liquid crystal polymer.
5. The adhesive film with LDS function according to claim 1, characterized in that: The weight of the resin matrix is 100 parts, the weight of the auxiliary agent is 0 to 100 parts, the weight of the diluent is 0 to 10 parts, and the weight of the LDS additive is 1 to 30 parts.
6. The adhesive film with LDS function according to claim 5, characterized in that: The weight portion of the LDS additive is 3 to 10 parts.
7. The adhesive film with LDS function according to claim 1, characterized in that: The LDS additive is a metal salt of copper, arsenic or tin.
8. The adhesive film with LDS function according to claim 7, characterized in that: The LDS additive includes at least one of copper chromite, copper hydroxyphosphate, arsenic trioxide and tin dioxide.
9. A method for preparing an adhesive film having LDS function as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: One or more resin matrices are mixed uniformly using a homogenizer according to a first preset ratio, different types and proportions of additives are added in sequence and stirred uniformly at a predetermined modification temperature, and a diluent is added and mixed according to a second preset ratio to obtain a resin body; Adding LDS additive to the resin body according to a third preset ratio, mixing and grinding the mixture thoroughly, and vacuuming and degassing the mixture to obtain a rubber material; The adhesive material is made into an adhesive film, the adhesive film is made on a release layer, and covered with a protective layer to obtain an adhesive film with LDS function.