Flame-retardant antibacterial low-melting cotton fiber and preparation method thereof
By adding long-chain alkyl naphthol derivative quaternary ammonium salt in the copolymerization stage of polyester fibers, the copolymerized flame retardant polyester is solved, and the problem that flame retardant only exists on the fiber surface in the prior art is realized. The improvement of internal flame retardant effect and the enhancement of antibacterial properties extend the flame retardant time and impart the soft and fluffy properties of the fiber.
Patent Information
- Application Number
- CN202411313988.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-06
AI Technical Summary
The flame retardant of existing polyester fibers can only exist as finishing agents on the fiber surface, resulting in a short flame retardant effect and decompose at high temperatures, making it impossible to effectively introduce the flame retardant into the fiber, resulting in flammability of polyester fibers.
Flame-retardant and antibacterial low-melting cotton fibers with a leather core structure are formed by adding long-chain alkyl naphthol derivative quaternary ammonium salt as flame retardant and low-melting point polyester in the polyester copolymerization stage. and copolymerized flame retardant semi-optical polyester ensure that flame retardant is introduced into the fiber and that subsequent blending or finishing agents are avoided by copolymerized polyester.
The effective introduction of internal flame retardants of fibers is achieved, the flame retardant performance and antibacterial properties are improved, the flame retardant effect is extended, the fiber is avoided rapidly burning at high temperatures, and the fiber is given a soft and fluffy feel and excellent physical and chemical properties.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester fibers, in particular to a flame-retardant, antibacterial, low-melting cotton fiber and a preparation method thereof. Background Art
[0002] Low-melting-point polyester is a type of polyester material that has developed rapidly in recent years. It is made by introducing flexible chain segments into ordinary polyester. It has a similar chemical structure to ordinary polyester. Therefore, low-melting-point polyester has excellent compatibility with ordinary polyester materials. In addition, low-melting-point polyester also has the characteristics of softness, fluffyness, and high peel strength. Therefore, low-melting-point polyester fibers and ordinary polyester often appear in the form of a sheath-core structure composite polyester fiber with a low-melting-point polyester sheath layer and a common polyester core layer. For example, the flame-retardant low-melting-point polyester fiber and its preparation method disclosed in Publication No. CN106811830B, the method for producing low-melting-point regenerated polyester for sheath-core type polyester by hydrolysis and degradation disclosed in Publication No. CN103145959B, the low-melting-point polyester sheath-core composite colored fiber and its production method disclosed in Publication No. CN102953148A, and other prior arts all adopt a sheath-core composite structure.
[0003] Polyester materials are flammable. Therefore, in order to improve the flame retardant properties of polyester fibers, flame retardants are added to polyester fibers in the prior art to improve the flame retardant properties of polyester fibers. Currently disclosed polyester fiber flame retardants include halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants and inorganic flame retardants, among which nitrogen flame retardants are mainly quaternary ammonium salt flame retardants. Currently commonly used quaternary ammonium salt flame retardants will decompose into ammonia and nitric acid at 110°C, so they are often used as finishing agents on the surface of fibers. However, the finishing agents are only attached to the surface of the fibers and will be separated from the fiber surface during long-term use, resulting in a decrease in the flame retardant effect. In addition, quaternary ammonium salt flame retardants achieve flame retardant effects through rapid endothermic reactions. Therefore, when used as finishing agents, they can only exert flame retardant effects on polyester fibers for a short time. When the finishing agent on the surface of the polyester fiber is completely ineffective, the polyester inside the polyester fiber will still burn rapidly. Therefore, it is of great significance to provide a quaternary ammonium salt flame retardant that can be introduced into the polyester fiber. Summary of the invention
[0004] In order to overcome the problem that the conventional quaternary ammonium salt flame retardant in the prior art can only be used as a finishing agent on the surface of polyester fiber and has a short flame retardant effect, the present invention provides a flame retardant, antibacterial and low-melting cotton fiber and a preparation method thereof. The fiber material is a sheath-core structure, the sheath is a copolymerized high-gloss flame retardant, antibacterial and low-melting polyester, and the core is a copolymerized flame retardant semi-gloss polyester. The polyester raw materials of the sheath and core layers of the fiber are both polyester materials prepared by adding a flame retardant to a copolymerization reaction during the polyester copolymerization synthesis stage. The use of the copolymerized polyester can avoid the problem of subsequent blending or finishing agents changing the performance of the polyester fiber. In addition, the long-chain alkyl naphthol derivative quaternary ammonium salt in the sheath of the present invention can not be decomposed in the PET polymerization reaction, and the long-chain alkyl structure contained in it can also reduce the melting point of the PET polyester. The long-chain alkyl naphthol derivative quaternary ammonium salt also has excellent antibacterial properties, so that the copolymerized high-gloss flame retardant, antibacterial and low-melting polyester has the advantages of flame retardancy, antibacterial, softness and fluffiness.
[0005] The specific technical scheme of the present invention is: A flame retardant, antibacterial, low-melting cotton fiber comprises a cortex and a core layer. The raw material of the core layer is a copolymerized flame retardant semi-glossy polyester. The raw material of the cortex layer is a copolymerized bright flame retardant, antibacterial, low-melting polyester. The copolymerized bright flame retardant, antibacterial, low-melting polyester is copolymerized with a long-chain alkyl naphthol derivative quaternary ammonium salt, terephthalic acid, and ethylene glycol as raw materials. The long-chain alkyl naphthol derivative quaternary ammonium salt is prepared by reacting a long-chain alkyl naphthol derivative and a quaternary ammonium salt as raw materials.
[0006] The invention provides a flame-retardant and antibacterial low-melting cotton fiber. The cotton fiber adopts a skin-core composite structure. The skin layer is a copolymerized high-gloss flame-retardant and antibacterial low-melting polyester, and the core layer is a copolymerized flame-retardant semi-gloss polyester. The polyester raw materials of the skin layer and the core layer of the cotton fiber of the invention both adopt copolymerized flame-retardant polyester. The copolymerized flame-retardant polyester is prepared by adding a flame retardant in the polyester copolymerization synthesis stage. The advantage of using the copolymerized flame-retardant polyester is that the problem of changing the performance of the polyester fiber by blending the flame retardant with the polyester and treating the polyester surface with a flame retardant finishing agent can be avoided. In addition, adding the flame retardant in the copolymerization stage of the polyester fiber can introduce the flame retardant between the polyester molecules, and the flame retardant effect is better than blending and surface treatment.
[0007] The cortex of the invention is a copolymerized light-resistant flame-retardant antibacterial low-melting-point polyester. The copolymerized light-resistant flame-retardant antibacterial low-melting-point polyester is prepared by adding a long-chain alkyl naphthol derivative quaternary ammonium salt in the copolymerization synthesis stage of PET polyester raw materials. The long-chain alkyl naphthol derivative quaternary ammonium salt is a high-temperature resistant quaternary ammonium salt prepared by reacting a long-chain alkyl naphthol derivative with a quaternary ammonium salt. The quaternary ammonium salt will not decompose in the entire reaction system of PET polyester synthesis, and the quaternary ammonium salt can be introduced into PET polyester molecules. The long-chain alkyl naphthol quaternary ammonium salt contains a long-chain alkyl branched chain, and after being added to PET polyester, the melting point of PET polyester can be reduced, so that the cortex structure has a soft and fluffy hand feel. The low-melting-point PET polyester cortex has good compatibility with the core layer PET polyester and has high peeling strength. In addition, the long-chain alkyl naphthol quaternary ammonium salt has excellent antibacterial function and can give the cortex excellent antibacterial performance.
[0008] Preferably, the copolymerized flame-retardant semi-gloss polyester is made from 1,2-dicarboxyethyldiphenylphosphine oxide, terephthalic acid, ethylene glycol and titanium dioxide as raw materials.
[0009] Preferably, the quaternary ammonium salt is one of chloroacetyldecylamine, chloroacetyldodecylamine and chloroacetyltetradecylamine.
[0010] Preferably, the long-chain alkylnaphthalene is prepared by alkylation reaction of N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine and C12 olefin in the presence of a catalyst.
[0011] Preferably, the catalyst is one of HY molecular sieve and Hβ molecular sieve.
[0012] A method for preparing the flame-retardant, antibacterial, low-melting cotton fiber is characterized by comprising the following steps: Step 1: subjecting N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and a catalyst to an alkylation reaction, filtering, distilling and recrystallizing to obtain a long-chain alkylnaphthol derivative, and adding the long-chain alkylnaphthol derivative and a quaternary ammonium salt to a solvent for reaction to obtain a long-chain alkylnaphthol derivative quaternary ammonium salt; Step 2: Evenly mix terephthalic acid, ethylene glycol and a long-chain alkylnaphthol derivative quaternary ammonium salt, and then perform esterification reaction and polycondensation reaction to prepare a copolymerized light-emitting flame-retardant antibacterial low-melting-point polyester; Step 3: adding 1,2-dicarboxyethyldiphenylphosphine oxide, terephthalic acid, ethylene glycol, a catalyst and a stabilizer into a container to respectively carry out esterification reaction and polycondensation reaction to prepare a copolymer flame-retardant polyester, and then blending the copolymer flame-retardant polyester with titanium dioxide to prepare a copolymer flame-retardant semi-gloss polyester; Step 4: After drying, the copolymerized bright flame-retardant antibacterial low-melting-point polyester and the copolymerized flame-retardant semi-bright polyester are injected into a melt spinning device for sheath-core composite spinning to produce flame-retardant antibacterial low-melting cotton fibers.
[0013] Preferably, the conditions of the alkylation reaction in step 1 include: reaction temperature of 130-160° C., reaction pressure of 0.5-2 MPa.
[0014] Preferably, in step 1, the molar ratio of N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine to C12 olefin is 3 to 6:1.
[0015] Preferably, in step three, the catalyst is butyl phthalate, the stabilizer is one of triphenyl phosphite and trimethyl phosphate, the amount of 1,2-dicarboxyethyldiphenylphosphine oxide is 9-20%, the amount of the catalyst is 0-0.05%, and the amount of the stabilizer is 0-0.05%.
[0016] Preferably, the conditions for the sheath-core composite spinning in step 4 include: a spinning temperature of 200-280° C., a ring blowing temperature of 10-30° C., a cold stretching ratio of the pre-spun raw yarn of 100-400%, and a total stretching ratio of 100-400%.
[0017] Compared with the prior art, this application has the following technical effects: (1) The present invention provides a flame retardant, antibacterial, low-melting cotton fiber and a preparation method thereof. The fiber material is a sheath-core structure, the sheath is a copolymerized bright flame retardant, antibacterial, low-melting polyester, and the core is a copolymerized flame retardant semi-bright polyester. The polyester raw materials of the sheath and core layers of the fiber are both polyester materials prepared by adding a flame retardant to a copolymerization reaction during the polyester copolymerization synthesis stage. The use of copolymerized polyester can avoid the problem of subsequent blending or finishing agents changing the properties of polyester fibers. (2) The long-chain alkyl naphthol derivative quaternary ammonium salt in the cortical fiber of the present invention can not only not decompose in the PET polymerization reaction, but also the long-chain alkyl structure contained in it can reduce the melting point of PET polyester, so that the cortical layer has a soft and fluffy feel. The long-chain alkyl naphthol derivative quaternary ammonium salt also has excellent antibacterial properties, which can make the cortical layer have multiple effects such as flame retardancy, antibacterial, softness and fluffyness. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the embodiments.
[0019] Embodiment 1: The invention discloses a flame retardant, antibacterial and low-melting cotton fiber, comprising a skin layer and a core layer. The raw material of the core layer is a copolymerized flame retardant semi-bright polyester, and the raw material of the skin layer is a copolymerized bright flame retardant, antibacterial and low-melting polyester.
[0020] A method for preparing the flame-retardant, antibacterial, low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 6:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 160°C, reaction pressure 1MPa, reaction time 6h, HY molecular sieve (particle size 20-40 mesh) is provided in the reaction vessel, and the crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio 1:3 ) mixed solvent for crystallization separation to obtain long-chain alkyl naphthol derivatives; adding the long-chain alkyl naphthol derivatives and chloroacetyldecylamine to a methanol / ethanol mixture with a volume ratio of 1:1, stirring at a temperature of 120°C for 32 hours to obtain a crude product, the crude product is rotary evaporated in a 60°C water bath at a speed of 110r / min to obtain a purified product, and then the purified product is added to an ethanol / petroleum ether mixture (volume ratio of 1:4) solvent for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0021] Step 2: Evenly mix terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivatives in a molar ratio of 1:1.8:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, and after the esterification reaction, add a catalyst (0.02% butyl phthalate) and a stabilizer (0.03% trimethyl phosphate) and heat to 260-280°C to maintain the reaction for 2 hours for polycondensation reaction to prepare a copolymerized light-resistant flame-retardant, antibacterial and low-melting-point polyester.
[0022] Step 3: Mix terephthalic acid, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, and after the esterification reaction, add a catalyst (butyl phthalate with an addition amount of 0.02%) and a stabilizer (trimethyl phosphate with an addition amount of 0.03%), first react for 30 minutes at a pressure of 500Pa and a temperature of 260°C, and then react for 50 minutes at a pressure of 100Pa and a temperature of 25°C to prepare a copolymer flame-retardant polyester, and then blend the copolymer flame-retardant polyester with titanium dioxide (added in an amount of 0.3%) to prepare a copolymer flame-retardant semi-bright polyester.
[0023] Step 4: Place the copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices in an 80°C oven and dry them for 24 hours, then inject the dried copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices into the spinning device respectively, and the cortical screw temperature sections are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C, zone 1 Zone 0 is 200-260°C; the temperature section of the core layer screw is: zone 1 is 250-280°C, zone 2 is 250-280°C, zone 3 is 250-280°C, zone 4 is 250-280°C, and zone 5 is 250-280°C. After extrusion, the screw enters the spinning box and is extruded through the spinning assembly and is ring-blown (ring-blowing temperature is 20°C, ring-blowing speed is 5m / s) to form a core-sheath composite fiber filament. The core-sheath composite fiber filament is cold-drawn into a front-spinning fiber with a front-spinning stretching ratio of 100-400%. The front-spinning fiber is then placed in a post-spinning device for stretching to form a flame-retardant, antibacterial, low-melting cotton fiber with a total stretching ratio of 200%.
[0024] Embodiment 2: The invention discloses a flame retardant, antibacterial and low-melting cotton fiber, comprising a skin layer and a core layer. The raw material of the core layer is a copolymerized flame retardant semi-bright polyester, and the raw material of the skin layer is a copolymerized bright flame retardant, antibacterial and low-melting polyester.
[0025] A method for preparing the flame-retardant, antibacterial, low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 4:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 150°C, reaction pressure 2MPa, reaction time 12h, HY molecular sieve (particle size 20-40 mesh) is provided in the reaction vessel, and the crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio 1: 4) using a mixed solvent for crystallization separation to obtain a long-chain alkyl naphthol derivative; adding the long-chain alkyl naphthol derivative and chloroacetyldecylamine to a methanol / ethanol mixture in a volume ratio of 1:1, stirring at 120°C for 32 hours to obtain a crude product, and rotary evaporating the crude product in a 60°C water bath at a speed of 110 r / min to obtain a purified product, and then adding the purified product to an ethanol / petroleum ether mixture (volume ratio of 1:4) for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0026] Step 2: Evenly mix terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivatives in a molar ratio of 1:1.8:0.05 and inject them into the reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintaining the esterification rate above 96%. After the esterification reaction is completed, add a catalyst (0.02% butyl phthalate) and a stabilizer (0.03% trimethyl phosphate) and heat to 270°C to maintain the reaction for 2 hours for polycondensation reaction to prepare a copolymerized light-resistant flame-retardant, antibacterial and low-melting-point polyester.
[0027] Step 3: Mix terephthalic acid, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, and after the esterification reaction, add a catalyst (butyl phthalate with an addition amount of 0.02%) and a stabilizer (trimethyl phosphate with an addition amount of 0.03%), first react at a pressure of 500Pa and a temperature of 260°C for 30min, and then react at a pressure of 100Pa and a temperature of 25°C for 50min to prepare a copolymer flame-retardant polyester, and then blend the copolymer flame-retardant polyester with titanium dioxide (added in an amount of 0.3%) to prepare a copolymer flame-retardant semi-bright polyester.
[0028] Step 4: Place the copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices in an 80°C oven and dry for 24 hours, then inject the dried copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices into the spinning device respectively, and the cortical screw temperature sections are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C, Zone 10: 200-260°C; the temperature section of the core layer screw is: zone 1: 250-280°C, zone 2: 250-280°C, zone 3: 250-280°C, zone 4: 250-280°C, zone 5: 250-280°C. After extrusion, the screw enters the spinning box and is extruded through the spinning assembly and is ring-blown (ring-blowing temperature: 10°C, ring-blowing speed: 0.5m / s) to form a core-sheath composite fiber filament. The core-sheath composite fiber filament is cold-drawn into a front-spinning fiber with a front-spinning stretching ratio of 100%. The front-spinning fiber is then placed in a post-spinning device for stretching to form a flame-retardant, antibacterial, low-melting cotton fiber with a total stretching ratio of 400%.
[0029] Embodiment 3: The invention discloses a flame retardant, antibacterial and low-melting cotton fiber, comprising a skin layer and a core layer. The raw material of the core layer is a copolymerized flame retardant semi-bright polyester, and the raw material of the skin layer is a copolymerized bright flame retardant, antibacterial and low-melting polyester.
[0030] A method for preparing the flame-retardant, antibacterial, low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 3:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 160°C, reaction pressure 0.5MPa, reaction time 24h, and Hβ molecular sieve (particle size 40-80 mesh) is provided in the reaction vessel. The crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio 1 :3) using a mixed solvent for crystallization separation to obtain a long-chain alkyl naphthol derivative; adding the long-chain alkyl naphthol derivative and chloroacetyldecylamine to a methanol / ethanol mixture in a volume ratio of 1:1, stirring at 120°C for 32 hours to prepare a crude product, and rotary evaporating the crude product in a 60°C water bath at a speed of 110 r / min to obtain a purified product, and then adding the purified product to an ethanol / petroleum ether mixture (volume ratio of 1:4) solvent for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0031] Step 2: Evenly mix terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivatives in a molar ratio of 1:1.8:0.05 and inject them into the reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintaining the esterification rate above 96%. After the esterification reaction is completed, add a catalyst (0.02% butyl phthalate) and a stabilizer (0.03% trimethyl phosphate) and heat to 270°C to maintain the reaction for 2 hours for polycondensation reaction to prepare a copolymerized light-resistant flame-retardant, antibacterial and low-melting-point polyester.
[0032] Step 3: Mix terephthalic acid, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, and after the esterification reaction, add a catalyst (butyl phthalate with an addition amount of 0.02%) and a stabilizer (trimethyl phosphate with an addition amount of 0.03%), first react at a pressure of 500Pa and a temperature of 260°C for 30min, and then react at a pressure of 100Pa and a temperature of 25°C for 50min to prepare a copolymer flame-retardant polyester, and then blend the copolymer flame-retardant polyester with titanium dioxide (added in an amount of 0.3%) to prepare a copolymer flame-retardant semi-bright polyester.
[0033] Step 4: Place the copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices in an 80°C oven and dry for 24 hours, then inject the dried copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices into the spinning device respectively, and the cortical screw temperature sections are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C , zone 10 200~260℃; core layer screw temperature section is: zone 1 250~280℃, zone 2 250~280℃, zone 3 250~280℃, zone 4 250~280℃, zone 5 250~280℃. After extrusion, the screw enters the spinning box and then passes through the spinning assembly for extrusion and ring blowing (ring blowing temperature 30℃, ring blowing speed 10m / s) to form skin-core composite fiber filaments. The skin-core composite fiber filaments are cold-drawn into front spinning with a front spinning stretching ratio of 200%. The front spinning is then placed in a post-spinning device for stretching to form a flame-retardant, antibacterial, low-melting cotton fiber with a total stretching ratio of 200%.
[0034] Embodiment 4: The invention discloses a flame retardant, antibacterial and low-melting cotton fiber, comprising a skin layer and a core layer. The raw material of the core layer is a copolymerized flame retardant semi-bright polyester, and the raw material of the skin layer is a copolymerized bright flame retardant, antibacterial and low-melting polyester.
[0035] A method for preparing the flame-retardant, antibacterial, low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 6:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 130-160°C, reaction pressure 0.5-2MPa, reaction time 12h, HY molecular sieve (particle size 20-40 mesh) is provided in the reaction vessel, and the crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio The long-chain alkyl naphthol derivatives were separated by crystallization in a mixed solvent of ethanol / trichloromethane (volume ratio 1:3); the long-chain alkyl naphthol derivatives and chloroacetyltetradecylamine were added to a mixed solution of acetonitrile / n-pentane (volume ratio 1:2), stirred at 100°C for 40 hours to prepare a crude product, the crude product was rotary evaporated in a water bath at 80°C and a speed of 120 r / min to obtain a purified product, and the purified product was added to an ethanol / trichloromethane mixed solution (volume ratio 1:3) solvent for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0036] Step 2: Evenly mix terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivatives in a molar ratio of 1:1.8:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, after the esterification reaction, add a catalyst (butyl phthalate with an addition amount of 0.02%) and a stabilizer (trimethyl phosphate with an addition amount of 0.03%), and heat to 270°C and keep the reaction for 2 hours to carry out a condensation reaction to prepare a copolymerized light-emitting low-melting polyester, and then blend the copolymerized light-emitting low-melting polyester with a silver ion antibacterial agent (solid content of 0.75%) to prepare a copolymerized light-emitting flame-retardant antibacterial low-melting polyester.
[0037] Step 3: Mix terephthalic acid, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, and after the esterification reaction, add a catalyst (butyl phthalate with an addition amount of 0.02%) and a stabilizer (trimethyl phosphate with an addition amount of 0.03%), first react at a pressure of 500Pa and a temperature of 260°C for 30min, and then react at a pressure of 100Pa and a temperature of 25°C for 50min to prepare a copolymer flame-retardant polyester, and then blend the copolymer flame-retardant polyester with titanium dioxide (added in an amount of 0.3%) to prepare a copolymer flame-retardant semi-bright polyester.
[0038] Step 4: Place the copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices in an 80°C oven and dry for 24 hours, then inject the dried copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices into the spinning device respectively, and the cortical screw temperature sections are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C , zone 10 200~260℃; core layer screw temperature section is: zone 1 250~280℃, zone 2 250~280℃, zone 3 250~280℃, zone 4 250~280℃, zone 5 250~280℃. After extrusion, the screw enters the spinning box and then passes through the spinning assembly for extrusion and ring blowing (ring blowing temperature 20℃, ring blowing speed 5m / s) to form sheath-core composite fiber filaments. The sheath-core composite fiber filaments are cold-drawn into front spinning with a front spinning stretching ratio of 200%. The front spinning is then placed in a post-spinning device for stretching to form a flame-retardant, antibacterial, low-melting cotton fiber with a total stretching ratio of 200%.
[0039] Embodiment 5: The invention discloses a flame retardant, antibacterial and low-melting cotton fiber, comprising a skin layer and a core layer. The raw material of the core layer is a copolymerized flame retardant semi-bright polyester, and the raw material of the skin layer is a copolymerized bright flame retardant, antibacterial and low-melting polyester.
[0040] A method for preparing the flame-retardant, antibacterial, low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 6:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 160°C, reaction pressure 1MPa, reaction time 12h, HY molecular sieve (particle size 20-40 mesh) is provided in the reaction vessel, and the crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio 1:3 ) mixed solvent for crystallization separation to obtain long-chain alkyl naphthol derivatives; adding the long-chain alkyl naphthol derivatives and chloroacetyl octadecylamine into a benzene / trichloromethane mixture with a volume ratio of 1:2, stirring at a temperature of 100°C for 40 hours to obtain a crude product, the crude product is rotary evaporated in a water bath at 80°C and a speed of 120r / min to obtain a purified product, and then the purified product is added into an ethanol / petroleum ether mixture (volume ratio of 1:3) solvent for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0041] Step 2: Evenly mix terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivatives in a molar ratio of 1:1.8:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, after the esterification reaction, add a catalyst (butyl phthalate with an addition amount of 0.02%) and a stabilizer (trimethyl phosphate with an addition amount of 0.03%), and heat to 270°C and keep the reaction for 2 hours to carry out a condensation reaction to prepare a copolymerized light-emitting low-melting polyester, and then blend the copolymerized light-emitting low-melting polyester with a silver ion antibacterial agent (solid content of 0.75%) to prepare a copolymerized light-emitting flame-retardant antibacterial low-melting polyester.
[0042] Step 3: Mix terephthalic acid, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 and inject them into a reactor, introduce nitrogen and heat to 230°C for esterification reaction, maintain the esterification rate above 96%, and after the esterification reaction, add a catalyst (butyl phthalate with an addition amount of 0.02%) and a stabilizer (trimethyl phosphate with an addition amount of 0.03%), first react at a pressure of 500Pa and a temperature of 260°C for 30min, and then react at a pressure of 100Pa and a temperature of 25°C for 50min to prepare a copolymer flame-retardant polyester, and then blend the copolymer flame-retardant polyester with titanium dioxide (added in an amount of 0.3%) to prepare a copolymer flame-retardant semi-bright polyester.
[0043] Step 4: Place the copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices in an 80°C oven and dry for 24 hours, then inject the dried copolymerized bright flame retardant antibacterial low melting point polyester slices and the copolymerized flame retardant semi-bright polyester slices into the spinning device respectively, and the cortical screw temperature sections are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C, Zone 10: 200-260°C; the temperature section of the core layer screw is: zone 1: 250-280°C, zone 2: 250-280°C, zone 3: 250-280°C, zone 4: 250-280°C, zone 5: 250-280°C. After extrusion, the screw enters the spinning box and is extruded through the spinning assembly and is ring-blown (ring-blowing temperature: 10°C, ring-blowing speed: 0.5m / s) to form a core-sheath composite fiber filament. The core-sheath composite fiber filament is cold-drawn into a front-spinning fiber with a front-spinning stretching ratio of 100%. The front-spinning fiber is then placed in a post-spinning device for stretching to form a flame-retardant, antibacterial, low-melting cotton fiber with a total stretching ratio of 400%.
[0044] Comparative Example 1: Compared with Examples 1 to 3, in Comparative Example 1, ordinary low-melting point PET polyester is used as the skin layer polyester material and copolymerized flame-retardant semi-gloss polyester is used to make flame-retardant low-melting point cotton fiber with a skin-core structure, and then the PET low-melting point skin layer polyester is surface treated with a quaternary ammonium salt flame retardant finishing agent.
[0045] Comparative Example 2: Compared with Examples 1 to 3, in Comparative Example 2, the copolymerized high-gloss flame-retardant, antibacterial and low-melting-point polyester made of quaternary ammonium salts of long-chain alkyl naphthol derivatives in Examples 1 to 3 is blended with ordinary low-melting-point PET polyester to obtain a blended flame-retardant, antibacterial and low-melting-point polyester, and then the blended flame-retardant, antibacterial and low-melting-point polyester is used as the sheath polyester to prepare a flame-retardant low-melting-point cotton fiber with a sheath-core structure together with the copolymerized flame-retardant semi-gloss polyester.
[0046] Comparative Example 3: Compared with Example 4, in Comparative Example 3, ordinary low-melting point PET polyester is used as the skin layer polyester material and copolymerized flame-retardant semi-gloss polyester is used to make flame-retardant low-melting point cotton fiber with a skin-core structure, and then a quaternary ammonium salt flame retardant finishing agent is used to surface treat the PET low-melting point skin layer polyester.
[0047] Comparative Example 4: Compared with Example 4, in Comparative Example 4, the copolymerized high-gloss flame-retardant, antibacterial and low-melting-point polyester made of quaternary ammonium salt of long-chain alkyl naphthol derivatives in Example 4 is blended with ordinary low-melting-point PET polyester to obtain a blended flame-retardant, antibacterial and low-melting-point polyester, and then the blended flame-retardant, antibacterial and low-melting-point polyester is used as the sheath polyester to prepare a flame-retardant low-melting-point cotton fiber with a sheath-core structure together with the copolymerized flame-retardant semi-gloss polyester.
[0048] Comparative Example 5: Compared with Example 5, in Comparative Example 5, ordinary low-melting point PET polyester is used as the skin layer polyester material and copolymerized flame-retardant semi-gloss polyester is used to make flame-retardant low-melting point cotton fiber with a skin-core structure, and then the PET low-melting point skin layer polyester is surface treated with a quaternary ammonium salt flame retardant finishing agent.
[0049] Comparative Example 6: Compared with Example 5, in Comparative Example 6, the copolymerized high-gloss flame-retardant, antibacterial and low-melting-point polyester made of quaternary ammonium salt of long-chain alkyl naphthol derivatives in Example 1 is blended with ordinary low-melting-point PET polyester to obtain a blended flame-retardant, antibacterial and low-melting-point polyester, and then the blended flame-retardant, antibacterial and low-melting-point polyester is used as the sheath polyester to prepare a flame-retardant low-melting-point cotton fiber with a sheath-core structure together with the copolymerized flame-retardant semi-gloss polyester.
[0050] Test example: The antibacterial properties, flame retardant properties and physical and chemical properties of the flame retardant and antibacterial low-melting cotton fibers prepared in the above Examples 1 to 5 and Comparative Examples 1 to 6 were tested; The physical and chemical properties test methods refer to GB / T 14344-2022 Test method for tensile properties of chemical fiber filaments and FZ / T50004-2011 Test method for dry heat shrinkage of polyester staple fibers; The antibacterial performance test method refers to "GB / T 20944-2007 Evaluation of Antibacterial Performance of Textiles"; The flame retardant performance test method refers to GB / T 5454: Determination of the burning performance of textiles by oxygen index method; The physical and chemical properties test performance is shown in Table 1; The flame retardant and antibacterial properties test results are shown in Table 2; Table 1 Physical and chemical properties test results Breaking strength (cN / dtex) Elongation at break (%) 125℃ dry heat shrinkage (%) Example 1 1.50 180 14 Example 2 1.65 165 12 Example 3 1.82 178 13 Example 4 2.36 150 11 Example 5 4.00 45 8 Table 2 Flame retardant and antibacterial properties test results Candida albicans (%) Escherichia coli (%) Staphylococcus aureus (%) Limiting oxygen index (%) Example 1 >99 >99 >99 31 Example 2 >99 >99 >99 32 Example 3 >99 >99 >99 31 Example 4 >99 >99 >99 33 Example 5 >99 >99 >99 33 Comparative Example 1 >99 >99 >99 20 Comparative Example 2 >90 >90 >90 27 Comparative Example 3 >99 >99 >99 21 Comparative Example 4 >90 >90 >90 28 Comparative Example 5 >99 >99 >99 20 Comparative Example 6 >90 >90 >90 27 As shown in Table 1, the physical and chemical properties of the flame retardant, antibacterial and low-melting cotton fibers prepared in Examples 1 to 5 show that the flame retardant, antibacterial and low-melting cotton fibers prepared in the present invention have a breaking strength between 1.5 and 4.0 cN / dtex, an elongation at break between 40 and 180%, and a dry heat shrinkage at 125°C of less than 15%, and have excellent fiber strength and elastic properties.
[0051] As shown in Table 2, the flame retardant and antibacterial low-melting cotton fibers prepared in Examples 1 to 5 have an antibacterial property of more than 99% against Candida albicans, Escherichia coli and Staphylococcus aureus, and a limiting oxygen index greater than 30%, which is a flame retardant material with excellent flame retardant effect.
[0052] In Comparative Examples 1 to 6, the flame retardant finishing agent and the flame retardant blending were tested respectively. After analyzing the test results, it was found that the antibacterial properties of the fiber after using the flame retardant finishing agent against Candida albicans, Escherichia coli and Staphylococcus aureus all reached more than 99%, but the antibacterial effect of the blended cotton fiber on Candida albicans, Escherichia coli and Staphylococcus aureus was only more than 90%. The above results show that the long-chain alkyl naphthol derivative quaternary ammonium salt prepared in the present application has excellent antibacterial properties, and the finishing agent and copolymerization synthesis can make the antibacterial effect of the long-chain alkyl naphthol derivative quaternary ammonium salt more significant. In order to ensure the mechanical properties of the blended fiber, the blending ratio needs to be controlled, resulting in the antibacterial effect of the long-chain alkyl naphthol derivative quaternary ammonium salt being limited and unable to fully exert its antibacterial properties.
[0053] Through the flame retardant performance structure analysis of Examples 1 to 6 and Examples 1 to 5, it was found that although the oxygen limit index of the flame retardant fibers obtained in Examples 2, 4, 6 and Examples 1 to 5 was above 27%, they were all flame retardant materials, but the oxygen limit index of Examples 2, 4, 6 was less than that of Examples 1 to 5. The above results show that the flame retardant performance of the copolymerized flame retardant antibacterial cotton fiber provided by the present application is more significant. In addition, it was found in the experiment that since the cortex of the present application adopts low melting point polyester, the flame burning will easily melt and drip the cortex polyester. Since the polyester cotton fiber using the flame retardant finishing agent in Examples 1, 3, and 5 is only The polyester surface can be flame-retarded. After dripping, the low-melting-point polyester in the cortical polyester that has not been treated with the finishing agent will burn quickly, and the combustion performance is poor. In addition, although the blended quaternary ammonium salt flame retardant can form a foam covering layer, since the ratio of the flame-retardant polyester to the ordinary polyester needs to be strictly controlled during the blending process, the problem of incomplete coverage of the flame-retardant foam covering layer will occur. When it continues to contact the fire source, the uncovered part will still burn. The copolymerized polyester fiber provided in the present application will form a uniform foam covering layer on the cortex after contacting the fire source, thereby protecting the low-melting-point polyester from dripping and avoiding fiber combustion.
[0054] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A flame retardant and antibacterial low-melting cotton fiber, characterized in that: The invention comprises a skin layer and a core layer, wherein the raw material of the core layer is a copolymerized flame-retardant semi-glossy polyester, and the raw material of the skin layer is a copolymerized bright flame-retardant antibacterial low-melting-point polyester. The copolymerized bright flame-retardant antibacterial low-melting-point polyester is copolymerized with a long-chain alkyl naphthol derivative quaternary ammonium salt, terephthalic acid and ethylene glycol as raw materials, and the long-chain alkyl naphthol derivative quaternary ammonium salt is prepared by reacting a long-chain alkyl naphthol derivative and a quaternary ammonium salt as raw materials.
2. The flame retardant and antibacterial low-melting cotton fiber according to claim 1 is characterized in that: The copolymerized flame-retardant semi-bright polyester is prepared from 1,2-dicarboxyethyldiphenylphosphine oxide, terephthalic acid, ethylene glycol and titanium dioxide as raw materials.
3. The flame retardant and antibacterial low-melting cotton fiber according to claim 1 is characterized in that: The quaternary ammonium salt is one of chloroacetyl decylamine, chloroacetyl dodecylamine and chloroacetyl tetradecylamine.
4. The flame retardant and antibacterial low-melting cotton fiber according to claim 1 is characterized in that: The long-chain alkyl naphthalene is prepared by an alkylation reaction between N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine and C12 olefin in the presence of a catalyst.
5. The flame retardant and antibacterial low-melting cotton fiber according to claim 4 is characterized in that: The catalyst is one of HY molecular sieve and Hβ molecular sieve.
6. A method for preparing the flame-retardant, antibacterial, low-melting cotton fiber according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: subjecting N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and a catalyst to an alkylation reaction, filtering, distilling and recrystallizing after the reaction to obtain a long-chain alkylnaphthol derivative, and adding the long-chain alkylnaphthol derivative and a quaternary ammonium salt to a solvent for reaction to obtain a long-chain alkylnaphthol derivative quaternary ammonium salt; Step 2: Evenly mix terephthalic acid, ethylene glycol and a long-chain alkylnaphthol derivative quaternary ammonium salt, and then perform esterification reaction and polycondensation reaction to prepare a copolymerized light-emitting flame-retardant antibacterial low-melting-point polyester; Step 3: adding 1,2-dicarboxyethyldiphenylphosphine oxide, terephthalic acid, ethylene glycol, a catalyst and a stabilizer into a container to respectively carry out esterification reaction and polycondensation reaction to prepare a copolymer flame-retardant polyester, and then blending the copolymer flame-retardant polyester with titanium dioxide to prepare a copolymer flame-retardant semi-gloss polyester; Step 4: After drying, the copolymerized bright flame-retardant antibacterial low-melting-point polyester and the copolymerized flame-retardant semi-bright polyester are injected into a melt spinning device for sheath-core composite spinning to produce flame-retardant antibacterial low-melting cotton fibers.
7. The preparation method according to claim 6, characterized in that: The conditions of the alkylation reaction in step 1 include: reaction temperature 130-160° C., reaction pressure 0.5-2 MPa.
8. The preparation method according to claim 6 or 7, characterized in that: In step 1, the molar ratio of N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine to C12 olefin is 3-6:
1.
9. The preparation method according to claim 6, characterized in that: In step 3, the catalyst is butyl phthalate, the stabilizer is one of triphenyl phosphite and trimethyl phosphate, the amount of 1,2-dicarboxyethyl diphenyl phosphine oxide is 9-20%, the amount of the catalyst is 0-0.05%, and the amount of the stabilizer is 0-0.05%.
10. The preparation method according to claim 6, characterized in that: The conditions for the core-skin composite spinning in step 4 include: a spinning temperature of 200-280°C, a ring blowing temperature of 10-30°C, a cold stretching ratio of the pre-spun raw yarn of 100-400%, and a total stretching ratio of 100-400%.