Antibacterial wear-resistant tensile non-woven fabric as well as preparation method and application thereof
A non-woven fabric treated with Artemisia extracts and silver nanoparticles, and graphene oxide for antibacterial and wear-resistant properties addresses the limitations of polypropylene fabrics, providing sustained protection and mechanical strength.
Patent Information
- Application Number
- CN202411465671.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-21
- Publication Date
- 2024-12-06
AI Technical Summary
Existing non-woven fabrics, particularly polypropylene-based ones, face challenges with poor antibacterial efficacy, especially in terms of long-term stability, and lack wear-resistance and tensile strength, limiting their application in medical and sanitary products.
A non-woven fabric comprising polypropylene, an antibacterial sustained-release agent made from Artemisia extracts and silver nanoparticles, and a wear-resistant and tensile agent made from graphene oxide, magnesium nitrate, and pullulan, treated through ultrasonic cleaning, immersion, and electrostatic charging.
The fabric achieves sustained antibacterial efficacy, improved wear-resistance, and enhanced tensile strength, ensuring long-term protection and mechanical stability while maintaining breathability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nonwoven fabrics, and specifically relates to an antibacterial, wear-resistant and tensile-resistant nonwoven fabric and a preparation method and application thereof. Background Art
[0002] Non-woven fabrics are made of directional or random fibers. They are called cloth because they have the appearance and certain properties of cloth. Non-woven fabrics are breathable, soft, lightweight, non-toxic and non-irritating, colorful, and inexpensive. At present, non-woven fabrics are widely used in medical and sanitary products such as gauze and wound dressings, as well as sanitary cleaning materials such as cotton pads and facial masks. Both of these use scenarios are close to human skin or mucous membranes, and the skin and mucous membranes are the basic barriers of the human body. Therefore, they are required to have not only sufficient comfort, but also good antibacterial properties and mechanical properties.
[0003] Non-woven fabrics are widely used, including: surgical gowns, protective clothing, masks, disinfection wraps, diapers, civilian rags, wipes, wet face towels, magic towels, soft towel rolls, beauty products, sanitary napkins, sanitary pads, and disposable sanitary cloths. Polypropylene non-woven fabrics have the advantages of good air permeability, extremely low moisture regain, wear resistance, acid and alkali resistance, large output, low cost and high strength. However, polypropylene resin molecules have a non-polar crystalline linear structure, low surface activity and non-polarity. There are disadvantages such as poor surface printability, poor coating and bonding, difficulty in blending with polar polymers, and difficulty in compatibility with polar reinforcing fibers and fillers. Polypropylene molecules do not have any hydrophilic groups, so they have extremely strong inertness and hydrophobicity, which brings great difficulties to the functionalization of polypropylene non-woven fabric materials and limits the further development of polypropylene non-woven fabrics. Medical non-woven fabrics usually need to be sterile or antibacterial when used. Sterile non-woven fabrics need to undergo a sterilization process, but they will still be contaminated by bacteria during actual use. As for antibacterial non-woven fabrics, existing non-woven fabrics usually have poor antibacterial effects, or have certain antibacterial effects but the antibacterial effect is usually short-lived. During storage or use, the antibacterial effect gradually disappears and cannot meet the long-term antibacterial requirements. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an antibacterial, wear-resistant and tensile non-woven fabric. The process is environmentally friendly and the non-woven fabric has antibacterial, flexible and wear-resistant properties, thereby realizing the functionalization of the polypropylene non-woven fabric.
[0005] To achieve the above object, the technical solution adopted by the present invention is as follows: An antibacterial, wear-resistant and tensile nonwoven fabric comprises the following raw materials in parts by weight: 100 to 150 parts of polypropylene non-woven fabric, 150 to 250 parts of antibacterial sustained-release agent and 150 to 250 parts of wear-resistant and anti-tensile agent.
[0006] In a preferred example, the following raw materials are included in parts by weight: 125 parts of polypropylene non-woven fabric, 200 parts of antibacterial sustained-release agent and 200 parts of wear-resistant and anti-tensile agent.
[0007] Based on a general inventive concept, another object of the present invention is to provide a method for preparing the above-mentioned antibacterial and anti-wear non-woven fabric, comprising the following steps: (1) Ultrasonic cleaning of polypropylene nonwoven fabric with anhydrous ethanol and drying at room temperature; (2) immersing the cleaned polypropylene non-woven fabric in the antibacterial sustained-release agent for 4 to 6 times, each time for 20 minutes, taking it out, and drying it at 45°C to 49°C; (3) re-treating the polypropylene non-woven fabric dried in step (2) with a wear-resistant and tensile-resistant agent, and then heat-drying; (4) The polypropylene non-woven fabric after heat drying in step (3) is subjected to electrostatic charging to obtain an antibacterial and anti-wear non-woven fabric.
[0008] In a preferred example, in step (2), the bath ratio of the polypropylene nonwoven fabric and the antibacterial sustained-release agent is 1m 2 ∶400mL~800mL.
[0009] In a preferred example, in step (2), the preparation method of the antibacterial sustained-release agent is as follows: S1. Take Artemisia selengensis stems, add 5 to 6 times the weight of Artemisia selengensis stems, deionized water, 0.1% of the weight of Artemisia selengensis stems, stir and extract at 40°C to 60°C for 4h to 8h; wherein the plant hydrolase is food grade with an enzyme activity of 8000u / g; S2. extracting the Artemisia sphagnum stem extract after enzymatic hydrolysis by ethanol 5 to 6 times the weight of the Artemisia sphagnum stem for 8 to 16 hours to obtain an Artemisia sphagnum stem extract; S3. Mix the silver nanoparticles and the extract of Artemisia sphagnum stems, and perform ball milling to obtain an antibacterial sustained-release agent.
[0010] In a preferred example, the weight ratio of the silver nanoparticles to the Artemisia sphagnum stem extract is 1:4, and the rotation speed of the ball mill is 800 rpm to 1000 rpm.
[0011] In a preferred example, in step (3), the preparation method of the wear-resistant and anti-tensile agent is as follows: Graphene oxide, magnesium nitrate and triethanolamine are added to deionized water respectively, and ultrasonic dispersion is performed. Then, pullulan is added and magnetically stirred until it is completely dissolved to obtain a wear-resistant and anti-tensile agent. Wherein, the weight ratio of the graphene oxide, magnesium nitrate, triethanolamine, pullulan and deionized water is 1.5:1.5:1:0.5:6; In a preferred example, in step (3), the wear-resistant and anti-tensile agent is sprayed onto the surface of the polypropylene non-woven fabric dried in step (2), and the spraying amount is 1 to 10 g / m 2 .
[0012] Based on a general inventive concept, another object of the present invention is to protect the application of the above-mentioned antibacterial and anti-wear non-woven fabric in personal protection and air purification.
[0013] Compared with the prior art, the present invention achieves the effect of slow release of antibacterial effect through the treatment of antibacterial sustained-release agent, so that the polypropylene non-woven fabric has a sustained and stable antibacterial effect; through the treatment of wear-resistant and anti-tensile agent, the surface of the non-woven fabric is made denser, and the wear-resistant and anti-tensile properties of the non-woven fabric are improved; it prevents moisture from forming an isolation layer inside the non-woven fabric, improves the water absorption capacity and ensures sufficient air permeability; comprehensively improves and protects the antibacterial performance, load stability and release persistence of the antibacterial sustained-release agent, and the tensile and wear-resistant properties of the non-woven fabric, and can realize large-scale production. DETAILED DESCRIPTION
[0014] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in conjunction with specific embodiments, but the present invention is not limited to these embodiments. It should be noted that, under the premise of not conflicting, the embodiments described below or the technical features can be arbitrarily combined to form new embodiments. In the present invention, unless otherwise specified, all parts and percentages are mass units, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments, if not otherwise specified, are conventional methods in the art.
[0015] As used herein, the terms "comprises," "including," "contains," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0016] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range limited by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including a range of "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When a numerical range is described in this article, unless otherwise specified, the range is intended to include its end values and all integers and fractions within the range.
[0017] Example 1
[0018] An antibacterial, wear-resistant and tensile nonwoven fabric comprises the following raw materials in parts by weight: 125 parts of polypropylene non-woven fabric, 200 parts of antibacterial sustained-release agent and 200 parts of wear-resistant and anti-tensile agent; The method for preparing the above-mentioned antibacterial and anti-wear non-woven fabric comprises the following steps: (1) Ultrasonic cleaning of polypropylene nonwoven fabric with anhydrous ethanol and drying at room temperature; (2) immersing the cleaned polypropylene non-woven fabric in step (1) into the antibacterial sustained-release agent for 5 times, each time for 20 minutes, taking it out, and drying it at 47°C; The bath ratio of polypropylene nonwoven fabric and antibacterial sustained-release agent is 1m 2 ∶600mL; The preparation method of the antibacterial sustained-release agent is as follows: S1. Take Artemisia sphaerocephala stems, add 5 times the weight of Artemisia sphaerocephala stems deionized water, 0.1% of the weight of Artemisia sphaerocephala stems plant hydrolase, stir at 50 ° C for 6 hours; wherein the plant hydrolase is food grade, and the enzyme activity is 8000u / g; S2. The Artemisia sphagnum stem extract was extracted with ethanol 5 times the weight of the Artemisia sphagnum stem for 12 hours to obtain an Artemisia sphagnum stem extract; S3. The silver nanoparticles and the extract of Artemisia sphagnum stems were mixed and ball-milled to obtain an antibacterial slow-release agent; The weight ratio of the silver nanoparticles to the Artemisia sphagnum stem extract is 1:4, and the rotation speed of the ball mill is 900 rpm; (3) Spray the wear-resistant and anti-tensile agent onto the surface of the polypropylene non-woven fabric dried in step (2) at a spraying amount of 5 g / m 2 , then heat and bake; The preparation method of the wear-resistant and anti-tensile agent is as follows: Graphene oxide, magnesium nitrate and triethanolamine are added to deionized water respectively, and ultrasonic dispersion is performed. Then, pullulan is added and magnetically stirred until it is completely dissolved to obtain a wear-resistant and anti-tensile agent. Wherein, the weight ratio of the graphene oxide, magnesium nitrate, triethanolamine, pullulan and deionized water is 1.5:1.5:1:0.5:6; (4) The polypropylene non-woven fabric after heat drying in step (3) is subjected to electrostatic charging to obtain an antibacterial and anti-wear non-woven fabric.
[0019] Example 2
[0020] An antibacterial, wear-resistant and tensile nonwoven fabric comprises the following raw materials in parts by weight: 150 parts of polypropylene non-woven fabric, 150 parts of antibacterial sustained-release agent and 250 parts of wear-resistant and anti-tensile agent; The method for preparing the above-mentioned antibacterial and anti-wear non-woven fabric comprises the following steps: (1) Ultrasonic cleaning of polypropylene nonwoven fabric with anhydrous ethanol and drying at room temperature; (2) immersing the cleaned polypropylene non-woven fabric in step (1) into the antibacterial sustained-release agent for 6 times, each immersion for 20 minutes, taking it out, and drying it at 45°C; The bath ratio of polypropylene nonwoven fabric and antibacterial sustained-release agent is 1m 2 ∶800mL; The preparation method of the antibacterial sustained-release agent is as follows: S1. Take Artemisia selengensis stems, add 6 times the weight of Artemisia selengensis stems deionized water, 0.1% of the weight of Artemisia selengensis stems plant hydrolase, stir at 40 ° C for 8 hours; wherein the plant hydrolase is food grade, and the enzyme activity is 8000u / g; S2. The Artemisia sphagnum stem extract was extracted with ethanol 6 times the weight of the Artemisia sphagnum stem for 8 hours to obtain an Artemisia sphagnum stem extract; S3. The silver nanoparticles and the extract of Artemisia sphagnum stems were mixed and ball-milled to obtain an antibacterial slow-release agent; The weight ratio of the silver nanoparticles to the Artemisia sphagnum stem extract is 1:4, and the rotation speed of the ball mill is 1000 rpm; (3) Spray the wear-resistant and anti-tensile agent onto the surface of the polypropylene non-woven fabric dried in step (2) at a spraying amount of 5 g / m 2 , then heat and bake; The preparation method of the wear-resistant and anti-tensile agent is as follows: Graphene oxide, magnesium nitrate and triethanolamine are added to deionized water respectively, and ultrasonic dispersion is performed. Then, pullulan is added and magnetically stirred until it is completely dissolved to obtain a wear-resistant and anti-tensile agent. Wherein, the weight ratio of the graphene oxide, magnesium nitrate, triethanolamine, pullulan and deionized water is 1.5:1.5:1:0.5:6; (4) The polypropylene non-woven fabric after heat drying in step (3) is subjected to electrostatic charging to obtain an antibacterial and anti-wear non-woven fabric.
[0021] Example 3
[0022] An antibacterial, wear-resistant and tensile nonwoven fabric comprises the following raw materials in parts by weight: 100 parts of polypropylene non-woven fabric, 250 parts of antibacterial sustained-release agent and 150 parts of wear-resistant and anti-tensile agent; The method for preparing the above-mentioned antibacterial and anti-wear non-woven fabric comprises the following steps: (1) Ultrasonic cleaning of polypropylene nonwoven fabric with anhydrous ethanol and drying at room temperature; (2) immersing the cleaned polypropylene non-woven fabric in step (1) into the antibacterial sustained-release agent for 4 times, each time for 20 minutes, taking it out, and drying it at 49°C; The bath ratio of polypropylene nonwoven fabric and antibacterial sustained-release agent is 1m 2 ∶400mL; The preparation method of the antibacterial sustained-release agent is as follows: S1. Take Artemisia selengensis stems, add 6 times the weight of Artemisia selengensis stems deionized water, 0.1% of the weight of Artemisia selengensis stems plant hydrolase, 40 ℃ ~ 60 ℃ stirring extraction time for 4h ~ 8h; wherein the plant hydrolase is food grade, enzyme activity 8000u / g; S2. The Artemisia sphagnum stem extract was extracted with ethanol 5 times the weight of the Artemisia sphagnum stem for 16 hours to obtain an Artemisia sphagnum stem extract; S3. The silver nanoparticles and the extract of Artemisia sphagnum stems were mixed and ball-milled to obtain an antibacterial slow-release agent; The weight ratio of the silver nanoparticles to the Artemisia sphagnum stem extract is 1:4, and the rotation speed of the ball mill is 800 rpm; (3) Spray the wear-resistant and anti-tensile agent onto the surface of the polypropylene non-woven fabric dried in step (2) at a spraying amount of 5 g / m 2 , then heat and bake; The preparation method of the wear-resistant and anti-tensile agent is as follows: Graphene oxide, magnesium nitrate and triethanolamine are added to deionized water respectively, and ultrasonic dispersion is performed. Then, pullulan is added and magnetically stirred until it is completely dissolved to obtain a wear-resistant and anti-tensile agent. Wherein, the weight ratio of the graphene oxide, magnesium nitrate, triethanolamine, pullulan and deionized water is 1.5:1.5:1:0.5:6; (4) The polypropylene non-woven fabric after heat drying in step (3) is subjected to electrostatic charging to obtain an antibacterial and anti-wear non-woven fabric.
[0023] Comparative Example 1
[0024] The antibacterial sustained-release agent does not contain the Artemisia sphagnum stem extract, and the rest is the same as in Example 1.
[0025] Test Example 1
[0026] The antibacterial performance of the nonwoven fabrics prepared in Examples 1 to 3 and Comparative Example 1 was tested against Staphylococcus aureus and Escherichia coli according to the oscillation method of GB / T21510-2008, and the tensile strength and elongation at break of the nonwoven fabrics prepared in Examples 1 to 3 and Comparative Example 1 were tested according to the GB / T 24218.3-2010 standard. Referring to GB / T 21196.3-2007 "Determination of the abrasion resistance of textiles by the Martindale method - Part 3: Determination of mass loss", the nonwoven fabrics prepared in Examples 1 to 3 and Comparative Example 1 were cut into circular samples with a diameter of 50 mm, 5 in each group, weighed, and the average value was recorded as M0, and then rubbed 120 times under a pressure of 9 kPa, weighed again, and the average value was recorded as M1, and the average wear rate was calculated by M0 and M1; The results are shown in Table 1 below.
[0027] Table 1 Performance test results of nonwoven fabrics prepared in Examples 1 to 3 and Comparative Example 1
[0028] The above embodiments are merely preferred implementations of the present invention. Any simple modification, amendment and substitution of the above embodiments based on the technical essence of the present invention shall fall within the scope of the technical solution of the present invention.
Claims
1. An antibacterial, wear-resistant and tensile nonwoven fabric, characterized in that: The invention comprises the following raw materials in parts by weight: 100 to 150 parts of polypropylene non-woven fabric, 150 to 250 parts of antibacterial sustained-release agent and 150 to 250 parts of wear-resistant and anti-tensile agent.
2. The antibacterial, wear-resistant and tensile nonwoven fabric according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 125 parts of polypropylene non-woven fabric, 200 parts of antibacterial sustained-release agent and 200 parts of wear-resistant and anti-tensile agent.
3. The method for preparing an antibacterial, wear-resistant and tensile-resistant nonwoven fabric according to claim 1 or 2, characterized in that: The following steps are involved: (1) Ultrasonic cleaning of polypropylene nonwoven fabric with anhydrous ethanol and drying at room temperature; (2) immersing the cleaned polypropylene non-woven fabric in the antibacterial sustained-release agent for 4 to 6 times, each time for 20 minutes, taking it out, and drying it at 45°C to 49°C; (3) re-treating the polypropylene non-woven fabric dried in step (2) with a wear-resistant and tensile-resistant agent, and then heat-drying; (4) The polypropylene non-woven fabric after heat drying in step (3) is subjected to electrostatic charging to obtain an antibacterial and anti-wear non-woven fabric.
4. The method for preparing an antibacterial, wear-resistant and tensile-resistant nonwoven fabric according to claim 3, characterized in that: Step (2), the bath ratio of the polypropylene nonwoven fabric and the antibacterial sustained-release agent is 1m 2 ∶400mL~800mL.
5. The method for preparing an antibacterial, wear-resistant and tensile-resistant nonwoven fabric according to claim 3, characterized in that: Step (2), the preparation method of the antibacterial sustained-release agent is as follows: S1. Take Artemisia selengensis stems, add 5 to 6 times the weight of Artemisia selengensis stems, deionized water, 0.1% of the weight of Artemisia selengensis stems, stir and extract at 40°C to 60°C for 4h to 8h; wherein the plant hydrolase is food grade with an enzyme activity of 8000u / g; S2. extracting the Artemisia sphagnum stem extract after enzymatic hydrolysis by ethanol 5 to 6 times the weight of the Artemisia sphagnum stem for 8 to 16 hours to obtain an Artemisia sphagnum stem extract; S3. Mix the silver nanoparticles and the extract of Artemisia sphagnum stems, and perform ball milling to obtain an antibacterial sustained-release agent.
6. The method for preparing an antibacterial, wear-resistant and tensile-resistant nonwoven fabric according to claim 5, characterized in that: The weight ratio of the silver nanoparticles to the Artemisia sphagnum stem extract is 1:4, and the rotation speed of the ball mill is 800 rpm to 1000 rpm.
7. The method for preparing an antibacterial, wear-resistant and tensile-resistant nonwoven fabric according to claim 3, characterized in that: Step (3), the preparation method of the wear-resistant and anti-tensile agent is as follows: Graphene oxide, magnesium nitrate and triethanolamine are added to deionized water respectively, and ultrasonic dispersion is performed. Then, pullulan is added and magnetically stirred until it is completely dissolved to obtain a wear-resistant and anti-tensile agent. Wherein, the weight ratio of the graphene oxide, magnesium nitrate, triethanolamine, pullulan and deionized water is 2:2:1:1:
6.
8. The method for preparing an antibacterial, wear-resistant and tensile-resistant nonwoven fabric according to claim 3, characterized in that: Step (3), spraying the wear-resistant and anti-tensile agent onto the surface of the polypropylene non-woven fabric dried in step (2), with a spraying amount of 1 to 10 g / m 2 .
9. Use of the antibacterial, wear-resistant and tensile-resistant nonwoven fabric according to claim 1 or 2 in personal protection and air purification.