Electrochromic film and preparation method and application thereof

The preparation of lithium-doped ζ-V2O5 films through electrochemical lithiation method solved the problem of small infrared modulation amplitude and poor reversibility of layered V2O5 crystal films, achieved efficient infrared band modulation, and broadened the application range of electrochromic materials .

CN119087720AActive Publication Date: 2024-12-06SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411232058.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The infrared modulation amplitude of the layered V2O5 crystal film is small and has poor reversibility, which limits its application in different application scenarios.

Method used

The V2O5 amorphous film is converted into a lithium-containing V2O5 amorphous film by electrochemical lithiation method, and annealing is performed to prepare lithium-doped ζ-V2O5 film. The lithium-doped ζ-V2O5 film is used to achieve infrared transmission under the action of an electric field The transmittance and reversibility of the infrared band are significantly improved.

Benefits of technology

The infrared modulation amplitude reaches 70%, and the modulation amplitude can still reach 63% after 50 cycles, effectively solving the problems of small infrared modulation amplitude and poor reversibility, and broadening the application of electrochromic materials in the fields of energy, construction, information and national defense. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087720A_ABST
    Figure CN119087720A_ABST
Patent Text Reader

Abstract

The invention discloses an electrochromic film and a preparation method and application thereof, and relates to the technical field of functional materials, the preparation method comprises the following steps: providing a V2O5 amorphous film; taking a lithium salt solution as a lithium source, and converting the V2O5 amorphous film into a lithium-containing V2O5 amorphous film through an electrochemical lithiation method; and after the lithium-containing V2O5 amorphous film is annealed, a lithium-doped zeta-V2O5 film is obtained, and the lithium-doped zeta-V2O5 film is the electrochromic film. The electrochromic film is prepared through a method of combining electrochemical lithiation with subsequent annealing, and when a voltage load is applied to the electrochromic film prepared through the electrochemical lithiation method, an infrared transmission or infrared blocking state exists, so that the electrochromic film has the infrared transmission or infrared blocking state; the transmittance of the infrared band of the electrochromic film is greatly changed while the electrochromic film reversibly changes, the infrared modulation amplitude reaches 70%, and the problem that the infrared modulation amplitude of a layered V2O5 crystal film is small is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional materials, and in particular to an electrochromic film and a preparation method and application thereof. Background Art

[0002] Electrochromic technology provides an effective way to control the optical properties of materials. Under the action of an electric field, the redox reaction inside the electrochromic material causes a reversible change in its valence, composition or phase structure, resulting in a stable and reversible change in the optical properties of the material (absorption, transmittance and reflectivity, etc.) in the visible, near-infrared and even microwave regions.

[0003] At present, organic electrochromic materials based on organic molecules, polymers and metal organic frameworks have fast response and rich colors. However, in practical applications, compared with inorganic electrochromic materials, organic electrochromic materials have poor thermal stability, light stability, chemical stability and radiation resistance. Therefore, the high stability and good durability of inorganic electrochromic materials make them show greater advantages than organic electrochromic materials in different application scenarios.

[0004] In inorganic electrochromic materials, layered V 2 O 5 The absorption edge of the visible light band of the crystal film can move reversibly. This movement of the optical absorption edge is due to the different band structures of different phases produced by the reversible phase transition. Through gradual ion intercalation, its phase transition can be controlled, thereby controlling its optical properties and achieving dynamic and selective regulation of the visible light and near-infrared spectra. Such optical properties are very suitable for the needs of multi-mode smart windows. However, layered V 2 O 5 The infrared modulation amplitude of crystal films is small, and achieving maximum infrared modulation will cause an irreversible phase change, which in turn leads to a significant attenuation of the reversibility and amplitude of the modulation, greatly limiting its application.

[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0006] Based on the above-mentioned deficiencies of the prior art, the object of the present invention is to provide an electrochromic film and a preparation method and application thereof, aiming to solve the problem of layered V 2 O 5 The problem of small infrared modulation amplitude of crystal thin film.

[0007] The technical solution of the present invention is as follows:

[0008] A first aspect of the present invention provides a method for preparing an electrochromic film, comprising the following steps:

[0009] Provide V 2 O5 amorphous film;

[0010] Using a lithium salt solution as a lithium source, the V 2 O 5 Amorphous films converted into lithium-containing V 2 O 5 amorphous film;

[0011] The lithium-containing V 2 O 5 After annealing of the amorphous film, lithium-doped ζ-V 2 O 5 The film is the electrochromic film.

[0012] Optionally, the electrochemical lithiation method is a constant current charging method.

[0013] Optionally, the process parameters adopted by the constant current charging method are as follows:

[0014] Current density is 10~30μA / cm 2 , time is 200~600s, and lithium salt concentration is 0.5~2mol / L.

[0015] Optionally, the lithium salt in the lithium salt solution includes at least one of lithium perchlorate, lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate and lithium tetrafluorooxalatophosphate.

[0016] Optionally, the solvent in the lithium salt solution includes at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl carbonate and diethyl carbonate.

[0017] Optionally, the annealing temperature is 250-450° C., and the annealing time is 1-5 hours.

[0018] Optionally, the V 2 O 5 The method for preparing an amorphous thin film comprises the steps of:

[0019] providing a substrate;

[0020] V is formed on the substrate by magnetron sputtering 2 O 5 Amorphous film.

[0021] A second aspect of the present invention provides an electrochromic film, wherein the electrochromic film is prepared by the preparation method as described above in the present invention.

[0022] The third aspect of the present invention provides an application of the electrochromic film as described above in the field of electrochromism.

[0023] Optionally, the electrochromic film is used as an electrochromic material to prepare an electrochromic device.

[0024] Beneficial effect: The present invention prepares an electrochromic film by combining electrochemical lithiation with subsequent annealing. When a voltage load is applied to the electrochromic film prepared by the electrochemical lithiation method, there is an infrared transmission or infrared blocking state. The electrochromic film undergoes a reversible change and greatly changes its infrared band transmittance. The infrared modulation amplitude reaches 70%, which effectively solves the problem of layered V 2 O 5 The infrared modulation amplitude of the crystal film is small (less than 60%). BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of the electrochromic film prepared in Example 1 of the present invention, with a magnification of 20k times.

[0026] Figure 2 This is a SEM image of the electrochromic film prepared in Example 2 of the present invention, with a magnification of 50k times.

[0027] Figure 3 1 is the XRD diagram of the electrochromic films prepared in Examples 1 to 3 of the present invention.

[0028] Figure 4 The figures are actual pictures of the electrochromic film prepared in Example 1 of the present invention at different voltages.

[0029] Figure 5 The XRD diagram of the electrochromic film prepared in Example 1 of the present invention when subjected to cyclic voltammetry at different voltage states.

[0030] Figure 6 The in-situ spectral transmittance variation curves of the electrochromic film prepared in Example 1 of the present invention in the colored state and the faded state.

[0031] Figure 7 The cyclic voltammetry curve of the electrochromic film prepared in Example 4 of the present invention.

[0032] Figure 8 This is a curve showing the change in spectral transmittance at 1100 nm of the electrochromic film prepared in Example 4 of the present invention during the electrochemical cycle. DETAILED DESCRIPTION

[0033] The present invention provides an electrochromic film and a preparation method and application thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0034] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0035] In layered crystals V 2 O 5 In the relationship between the phase change of the film and the change in transmittance, V 2 O 5 The phase transition process of the film is α, ε, δ, γ, ω and ω'. The phase transition in the range of α to γ ​​is reversible, but V 2 O 5 The infrared modulation of the thin film (320nm thick) cannot reach 60%. If the phase changes to ω', although 70% infrared modulation amplitude can be achieved, the reversibility is poor, and basically the second cycle has only 40% modulation amplitude. 2 O 5 The infrared modulation amplitude of the film is small, the reversibility of infrared modulation is poor, and the irreversible phase change will cause the modulation amplitude to decay significantly with the cycle, which greatly limits its application. 2 O 5 The modulation amplitude and reversibility of the infrared band of the film are of great significance to broadening the application of electrochromic materials in the fields of energy, construction, information and national defense. Based on this, an embodiment of the present invention provides a method for preparing an electrochromic film, which includes the following steps:

[0036] S1, provide V 2 O 5 amorphous film;

[0037] S2, using a lithium salt solution as a lithium source, and converting the V 2 O 5 Amorphous films converted into lithium-containing V 2 O 5 amorphous film;

[0038] S3, the lithium-containing V 2 O 5 After annealing of the amorphous film, lithium-doped ζ-V 2 O 5 The film is the electrochromic film.

[0039] The present invention uses a lithium salt solution as a lithium source, firstly obtains lithium-containing V by electrochemical lithiation method. 2 O 5 Amorphous film, followed by annealing, to prepare stable lithium-doped ζ-V 2 O 5 Specifically, the present invention uses an electrochemical lithiation method to make the Li in the lithium salt solution + Enter V 2 O 5 In the amorphous film, lithium-containing V 2 O 5 (It can also be expressed as Li x V 2 O 5 , x represents the number of Li atoms, for example, x:2 represents the ratio of the number of Li atoms to the molar ratio of V atoms) amorphous film, when further annealed, Li + On the one hand, it affects V 2 O 5 The crystallization behavior of 2 O 5 On the other hand, Li + Embedded in ζ-V 2 O 5 In the channel structure, the ζ-V with lithium embedded in the channel is obtained. 2 O 5 (It can also be expressed as ζ-Li x V 2 O 5 ) thin film, namely lithium-doped ζ-V 2 O 5 film.

[0040] When a voltage load is applied to the electrochromic film prepared by the electrochemical lithiation method of the present invention, there is an infrared transmission or infrared blocking state. The electrochromic film undergoes a reversible change and greatly changes its infrared band transmittance. The infrared modulation amplitude reaches 70% (thickness is 320nm), and after 50 cycles, the tempering amplitude can still reach 63%, which effectively solves the problem of layered V 2 O 5 The crystal film has the problems of small infrared modulation amplitude (when the thickness is 320nm, the first circle can not reach 60% at most) and poor phase change reversibility (when the thickness is 320nm, the second circle has only 40% modulation amplitude). The electrochromic film provided by the present invention has broad application prospects in the field of electrochromic.

[0041] The electrochromic film described in the embodiment of the present invention will cause phase change when ions (including but not limited to lithium ions) are injected or extracted, and different phases have different polaron transition modes, thereby producing different optical absorption, thereby achieving light transmission or blocking.

[0042] In step S1, in some embodiments, the V 2 O 5 The method for preparing an amorphous thin film comprises the steps of:

[0043] S11, providing a substrate;

[0044] S12, forming V on the substrate by magnetron sputtering 2 O 5 Amorphous film.

[0045] In step S1, the substrate is a conductive substrate, specifically, may be indium tin oxide conductive glass (ITO), fluorine-doped tin dioxide conductive glass (FTO), etc., but is not limited thereto.

[0046] In step S2, in one embodiment, a V 2 O 5 The amorphous film specifically includes the following steps:

[0047] Using vanadium as a target, magnetron sputtering is performed in an oxygen and argon environment to form V on the substrate. 2 O 5 Amorphous film.

[0048] Specifically, the sputtering power and sputtering gas pressure used in magnetron sputtering can be set according to actual needs.

[0049] The present invention combines the magnetron sputtering method in this embodiment with the above-mentioned electrochemical lithiation method to prepare a stable photochromic film.

[0050] In step S2, in some embodiments, the electrochemical lithiation method is a constant current charging method.

[0051] In some embodiments, the process parameters used in the constant current charging method are as follows:

[0052] Current density is 10~30μA / cm 2 , time is 200~600s, and lithium salt concentration is 0.5~2mol / L.

[0053] By controlling the current density, time and lithium salt concentration, V 2 O 5 Amorphous film conversion to ζ-V 2 O 5 , while controlling the embedded ζ-V 2 O 5 The amount of lithium in the channel eventually forms a lithium-doped ζ-V 2 O 5 film.

[0054] As an example, the current density may be 10 μA / cm 2 , 11μA / cm 2 , 12μA / cm 2 , 13μA / cm 2 , 14μA / cm 2 , 15μA / cm 2 , 16μA / cm 2 , 17μA / cm 2 , 18μA / cm 2 , 19μA / cm 2 , 20μA / cm 2 , 21μA / cm 2 , 22μA / cm 2 , 23μA / cm 2 , 24μA / cm 2 , 25μA / cm 2 , 26μA / cm 2 , 27μA / cm 2 , 28μA / cm 2 , 29μA / cm 2 or 30μA / cm 2 wait.

[0055] The time may be 200s, 210s, 220s, 230s, 240s, 250s, 260s, 270s, 280s, 290s, 300s, 310s, 320s, 330s, 340s, 350s, 360s, 370s, 380s, 390s, 400s, 410s, 420s, 430s, 440s, 450s, 460s, 470s, 480s, 490s, 500s, 510s, 520s, 530s, 540s, 550s, 560s, 570s, 580s, 590s or 600s, etc.

[0056] The lithium salt concentration may be 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2 mol / L, etc.

[0057] Specifically, a three-electrode system was used, with metallic lithium as the reference electrode and the counter electrode, and V 2 O 5The amorphous film was used as the working electrode, the lithium salt solution was used as the lithium source, and the constant current charging method was adopted, with a current of 10-30 μA / cm 2 The current density is 250 to 500 seconds, and the constant current charging is performed to prepare the Li x V 2 O 5 Amorphous film. By using this process parameter, better quality lithium-containing V 2 O 5 Amorphous film.

[0058] In some embodiments, the current density is 20 μA / cm 2 , the time is 400±30s (for example, 370s, 380s, 390s, 400s, 410s, 420s or 430s, etc.), to obtain lithium-containing V 2 O 5 Amorphous film. After a subsequent annealing step, lithium-doped ζ-V 2 O 5 The film, i.e. the electrochromic film, wherein the molar number of Li accounts for ζ-V 2 O 5 30% of the molar amount.

[0059] In some embodiments, the lithium salt in the lithium salt solution includes lithium perchlorate, lithium hexafluorophosphate (LiPF 6 ), lithium bis(oxalatoborate) (LiBOB), lithium tetrafluoroborate (LiBF 4 ), lithium difluorooxalatoborate (LiODFB), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium difluorophosphate (LiPO 2 F 2 ) and at least one of lithium tetrafluorooxalophosphate (LiFOP), but is not limited thereto.

[0060] In some embodiments, the solvent in the lithium salt solution includes at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl carbonate, and diethyl carbonate, but is not limited thereto.

[0061] In some embodiments, the annealing temperature is 250-450°C, and the annealing time is 1-5h. Specifically, the annealing temperature may be 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C or 450°C. The annealing time may be 1h, 2h, 3h, 4h or 5h. The annealing temperature of 250-450°C and the annealing time of 1-5h can ensure that the lithium-containing V 2 O 5 The amorphous film is fully crystallized, which is conducive to the realization of high-quality lithium-doped ζ-V 2 O 5 Preparation of thin films.

[0062] The present invention does not limit the thickness of the electrochromic film prepared by the above preparation method, which can be selected according to actual needs. For example, the thickness of the electrochromic film is 200-400nm, specifically, it can be 200nm, 250nm, 300nm, 350nm or 400nm.

[0063] Because the modulation of the transmittance of the film is positively correlated with the thickness, the thicker the film, the greater the modulation amplitude; at the same time, the greater the thickness, the lower the initial transmittance of the film (the more opaque), therefore, the embodiment of the present invention adopts the thickness as described above, that is, to ensure sufficient transmittance and a larger modulation amplitude. In addition, the stability of the process must also be considered. If the film thickness is less than 200nm, the uniformity of lithiation cannot be guaranteed, and the injection of lithium ions may be mainly distributed in the surface layer. The above process parameters currently used in the present invention are suitable for films of this thickness.

[0064] An embodiment of the present invention further provides an electrochromic film, which is prepared by the preparation method of the present invention as described above.

[0065] The electrochromic film provided in this embodiment can significantly adjust the transmittance of the film in the near-infrared band while adjusting the film to undergo reversible changes. Therefore, the application of the electrochromic film in the field of electrochromism solves the problem of layered crystal V 2 O 5The problem of poor reversibility of infrared modulation. In addition, the electrochromic film itself contains a certain amount of lithium, so that when it is used to make an electrochromic device, it can provide a certain amount of lithium to the electrode material, further broadening the application range of the electrochromic film. Specifically, when selecting the electrode material for the electrochromic material, not only the matching problem of the electrochemical window should be considered, but also the ion demand problem of the electrode material. If a large amount of ion injection is required to achieve color change of the material, and the electrolyte contained in the device is limited, its working performance will be affected. When ion injection is performed on the electrode material, the lithium ions contained in the electrochromic film itself provided by the present invention can enter the electrolyte, supplement the lithium therein, and make the device have better working performance.

[0066] The embodiment of the present invention further provides an application of the electrochromic film as described above in the electrochromic field.

[0067] In some embodiments, the electrochromic film is used as an electrochromic material to prepare an electrochromic device.

[0068] The present invention will be further described below by means of specific examples.

[0069] The present invention provides a method for preparing an electrochromic film, comprising the steps of:

[0070] (1) Providing commercial ITO, after cleaning, as a substrate;

[0071] (2) Using the magnetron sputtering method, pure metal vanadium (99.99%) target material was sputtered on the substrate for 120 minutes under the conditions of oxygen-argon volume ratio of 1:9, sputtering pressure of 1 Pa, and power of 150 W to obtain a 350 nm thick V 2 O 5 amorphous film;

[0072] (3) V obtained in step (2) 2 O 5 The amorphous film was placed in a glove box and electrochemically lithiated using a three-electrode system using an electrochemical workstation. 2 O 5 The amorphous film was used as the working electrode, the metal lithium sheet was used as the reference electrode and the counter electrode, and the 1 mol / L lithium perchlorate propylene carbonate solution was used as the lithium source. The constant current charging method was used for lithiation at a current density of 20 μA / cm 2 , the lithiation time is 400s, and lithium-containing V 2 O 5 The amorphous transparent film (attached to the ITO) was then rinsed with dimethyl carbonate and dried using a nitrogen gun.

[0073] (4) the lithium-containing V obtained in step (3) 2 O 5 The amorphous transparent film was annealed at 300 °C for 2 h to obtain lithium-doped ζ-V 2 O 5 The film, i.e. the electrochromic film, has a thickness of 320nm.

[0074] The surface morphology (i.e. SEM image) of the electrochromic film in Example 1 is as follows: Figure 1 shown.

[0075] Example 2

[0076] This embodiment provides a method for preparing an electrochromic film, comprising the following steps:

[0077] (1) Providing commercial ITO, after cleaning, as a substrate;

[0078] (2) Using the magnetron sputtering method, pure metal vanadium (99.99%) target material was sputtered on the substrate for 120 minutes under the conditions of oxygen-argon volume ratio of 1:9, sputtering pressure of 1 Pa, and power of 150 W to obtain a 350 nm thick V 2 O 5 amorphous film;

[0079] (3) V obtained in step (2) 2 O 5 The amorphous film was placed in a glove box and electrochemically lithiated using a three-electrode system using an electrochemical workstation. 2 O 5 The amorphous film was used as the working electrode, the metal lithium sheet was used as the reference electrode and the counter electrode, and the 1 mol / L lithium perchlorate propylene carbonate solution was used as the lithium source. The constant current charging method was used for lithiation at a current density of 20 μA / cm 2 , the lithiation time is 380s, and lithium-containing V 2 O 5 The amorphous transparent film (attached to the ITO) was then rinsed with dimethyl carbonate and dried using a nitrogen gun.

[0080] (4) the lithium-containing V obtained in step (3) 2 O 5 The amorphous transparent film was annealed at 300 °C for 2 h to obtain lithium-doped ζ-V 2 O 5 The film, i.e. the electrochromic film, has a thickness of 320nm.

[0081] The surface morphology (i.e. SEM image) of the electrochromic film in Example 2 is as follows: Figure 2 shown.

[0082] Example 3

[0083] This embodiment provides a method for preparing an electrochromic film, comprising the following steps:

[0084] (1) Providing commercial ITO, after cleaning, as a substrate;

[0085] (2) Using the magnetron sputtering method, pure metal vanadium (99.99%) target material was sputtered on the substrate for 120 minutes under the conditions of oxygen-argon volume ratio of 1:9, sputtering pressure of 1 Pa, and power of 150 W to obtain a 350 nm thick V 2 O 5 amorphous film;

[0086] (3) V obtained in step (2) 2 O 5 The amorphous film was placed in a glove box and electrochemically lithiated using a three-electrode system using an electrochemical workstation. 2 O 5 The amorphous film was used as the working electrode, the metal lithium sheet was used as the reference electrode and the counter electrode, and the 1 mol / L lithium perchlorate propylene carbonate solution was used as the lithium source. The constant current charging method was used for lithiation at a current density of 20 μA / cm 2 The lithiation time is 420s, and lithium-containing V 2 O 5 The amorphous transparent film (attached to the ITO) was then rinsed with dimethyl carbonate and dried using a nitrogen gun.

[0087] (4) the lithium-containing V obtained in step (3) 2 O 5 The amorphous transparent film was annealed at 300 °C for 2 h to obtain lithium-doped ζ-V 2 O 5 The film, i.e. the electrochromic film, has a thickness of 320nm.

[0088] test:

[0089] The XRD results of the electrochromic films in Examples 1-3 are as follows: Figure 3 As shown, Figure 3 The two diffraction peaks at 9.2° and 12.4° correspond to Li 0.3 V 2 O 5 The (001) and (200) planes (Li 0.3 V 2 O 5 The standard PDF card number is 04-006-0889).

[0090] The electrochromic performance test of the electrochromic film prepared in Example 1 was carried out:

[0091] 1) Using cyclic voltammetry, the electrochromic film was scanned with a voltage range of 2.25-4.00 V and a scanning speed of 1 mV / s. During the scanning process, the color change of the film immersed in the solution at different voltages was as follows: Figure 4 As shown, it can be seen that the color of the film is different under different voltages.

[0092] 2) Cyclic voltammetry was used to capture the in-situ spectral transmittance change curves in the colored and faded states. The XRD patterns at different voltages during the cyclic voltammetry test were as follows: Figure 5 As shown, it can be seen that during the ion injection and extraction process of the electrochromic film, when the voltage is greater than 2.6eV, only ion intercalation (no phase change) occurs, while when the voltage is between 2.3 and 2.6eV, a phase change process occurs.

[0093] 3) The in-situ spectral transmittance change curves of the colored and faded states are as follows: Figure 6 As shown, it can be seen that when a voltage load is applied to the electrochromic film, there is an infrared transmission or infrared blocking state.

[0094] 4) Cyclic voltammetry was used with a cycle interval of 2.2 to 3.2 V and a scan rate of 1 mV / s for 50 cycles. The changes in the electrochemical cyclic voltammetry curve were recorded. The results are as follows: Figure 7 As shown, the variation of the spectral transmittance at 1100nm during the electrochemical cycle was recorded in situ. The results are shown in Figure 8 As shown, it can be seen that the electrochromic film switches between different infrared transmittances and has good stability. After one cycle, the infrared modulation amplitude is 70%, and after 50 cycles, the modulation amplitude is 63%.

[0095] Comparative Example 1

[0096] This comparative example provides a method for preparing a thin film, which differs from Example 1 only in that the current density is 35 μA / cm 2 , the lithiation time is 650s.

[0097] The film prepared in this comparative example does not have the infrared modulation amplitude of the film described in Example 1.

[0098] Comparative Example 2

[0099] This comparative example provides a method for preparing a thin film, which differs from Example 1 only in that the current density is 8 μA / cm 2 , the lithiation time is 150s.

[0100] The film prepared in this comparative example does not have the infrared modulation amplitude of the film described in Example 1.

[0101] In summary, the present invention provides an electrochromic film and a preparation method and application thereof. The present invention prepares an electrochromic film by combining electrochemical lithiation with subsequent annealing. When a voltage load is applied to the electrochromic film prepared by the electrochemical lithiation method of the present invention, there is an infrared transmission or infrared blocking state. The electrochromic film undergoes a reversible change while greatly changing its infrared band transmittance. The infrared modulation amplitude reaches 70%, which effectively solves the problem of layered V 2 O 5 The infrared modulation amplitude of the crystal film is small (less than 60%). In addition, the electrochromic film itself contains a certain amount of lithium, so that when it is used to make an electrochromic device, it can provide a certain amount of lithium for the electrode material, further broadening the application range of the electrochromic film. The electrochromic film provided by the present invention has broad application prospects.

[0102] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing an electrochromic film, It is characterized in that The steps include: Provide V 2 O 5 amorphous film; Using a lithium salt solution as a lithium source, the V 2 O 5 Amorphous films converted to lithium-containing V 2 O 5 amorphous film; The lithium-containing V 2 O 5 After annealing of the amorphous film, lithium-doped ζ-V 2 O 5 The film is the electrochromic film.

2. The preparation method according to claim 1, It is characterized in that The electrochemical lithiation method is a constant current charging method.

3. The preparation method according to claim 2, It is characterized in that The process parameters used in the constant current charging method are as follows: Current density is 10~30μA / cm 2 , time is 200~600s, and lithium salt concentration is 0.5~2mol / L.

4. The preparation method according to claim 1, It is characterized in that The lithium salt in the lithium salt solution includes at least one of lithium perchlorate, lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate and lithium tetrafluorooxalatophosphate.

5. The preparation method according to claim 1, It is characterized in that The solvent in the lithium salt solution includes at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl carbonate and diethyl carbonate.

6. The preparation method according to claim 1, It is characterized in that The annealing temperature is 250-450° C., and the annealing time is 1-5 hours.

7. The preparation method according to claim 1, It is characterized in that The V 2 O 5 The method for preparing an amorphous thin film comprises the steps of: providing a substrate; V is formed on the substrate by magnetron sputtering 2 O 5 Amorphous film.

8. An electrochromic film, It is characterized in that The preparation is obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the electrochromic film according to claim 8 in the field of electrochromism.

10. The use according to claim 9, It is characterized in that The electrochromic film is used as an electrochromic material for preparing an electrochromic device.

Citation Information

Patent Citations

  • Chromogenically tunable photonic crystals

    CA2597095A1

  • Electrochemical doping method for electrochromic thin film

    CN107142508A

  • Multi-color electrochromic film, device and preparation method of multi-color electrochromic film

    CN114859611A

  • Preparation method of electrochromic material and electrochromic device

    CN117777992A

  • Electrode for electrochromic device having excellent water resistant property, and method for preparing the same

    KR1020080086655A