Heterogeneous composite substrate and preparation method and application thereof

By performing oxygen ion implantation and annealing repair treatment on the cracked surface of the heterogeneous composite substrate precursor, the resistance problem of silicon-based semiconductor materials under high temperature and high pressure is solved, and the quality factor and substrate performance of the device are significantly improved.

CN119092397APending Publication Date: 2024-12-06TJ INNOVATIVE SEMICON SUBSTRATE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197758.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing silicon-based semiconductor materials have poor resistance at high temperatures and high pressures, which affects the quality factors of the device, especially the bonding interface strength between silicon carbide and silicon oxide, and the resistance of the amorphous silicon layer is not as good as that of the silicon carbide layer.

Method used

The oxygen ion implantation is carried out on the cracking surface of the precursor of the heterogeneous composite substrate, accurately control the oxygen ion concentration distribution, improve the rate of conversion of the amorphous silicon layer into the SiO2 layer, deposit the amorphous silicon layer by sputtering method and perform annealing repair treatment , improve the substrate's high temperature and high pressure resistance.

Benefits of technology

It significantly improves the high temperature and high pressure resistance of heterogeneous composite substrates, improves the quality factor of the device, and ensures uniform conversion of the amorphous silicon layer and overall performance of the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092397A_ABST
    Figure CN119092397A_ABST
Patent Text Reader

Abstract

The invention provides a heterogeneous composite substrate and a preparation method and application thereof. The preparation method comprises the following steps: preparing a silicon substrate and a silicon carbide substrate, performing oxidation on the surface of one side of the silicon substrate to form a SiO2 layer, and performing ion implantation on the surface of one side of the silicon carbide substrate to form a weakening layer; depositing an amorphous silicon layer, and then bonding the ion implantation surface of the silicon carbide substrate and the SiO2 surface of the silicon substrate to obtain a bonded body; carrying out splitting treatment on the bonding body to obtain a residual material layer and a heterogeneous composite substrate precursor; oxygen ion implantation is carried out from the cracking surface of the heterogeneous composite substrate precursor, so that oxygen ions are implanted into the amorphous silicon layer, then annealing repair treatment is carried out, so that at least part of the amorphous silicon layer is converted into the SiO2 layer, and the heterogeneous composite substrate is obtained. According to the preparation method, the high-temperature and high-pressure resistance of the heterogeneous composite substrate can be improved, and the quality factor of a device prepared based on the method is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor devices, and in particular relates to a heterogeneous composite substrate and a preparation method and application thereof. Background Art

[0002] Nowadays, silicon-based semiconductor materials composed of insulating substrates and silicon carbide combine the advantages of silicon on insulators and silicon carbide, and are suitable for the preparation of high-temperature and high-power devices. The preparation scheme is to transfer the silicon carbide film to the silicon oxide substrate in a bonding manner by ion implantation combined with stripping technology in the silicon carbide substrate.

[0003] The commonly used bonding method is room temperature bonding technology. The composite substrate prepared by this method can solve the warping problem caused by the difference in thermal expansion coefficients of heterogeneous materials during bonding because the bonding process does not require high temperature. However, when silicon carbide is directly bonded to silicon oxide using room temperature bonding technology, the bonding interface bonding strength is poor.

[0004] The existing technology can improve the bonding strength by introducing amorphous silicon between silicon oxide and silicon carbide, and bonding through amorphous silicon as an intermediate layer. The prepared composite substrate includes silicon oxide layer-amorphous silicon layer-silicon carbide layer in sequence. However, as a semiconductor layer, the amorphous silicon layer has poorer high temperature and high voltage resistance than the silicon carbide layer, and its presence directly affects the high temperature and high voltage resistance of the composite substrate.

[0005] Therefore, how to further improve the high temperature and high pressure resistance of the composite substrate and enhance the quality factor of the device is a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a heterogeneous composite substrate and a preparation method and application thereof. The present invention implants oxygen ions into the amorphous silicon layer by implanting oxygen ions on the cracked surface of the heterogeneous composite substrate precursor. This strategy can accurately control the uniformity of the concentration distribution of the oxygen ion implantation and improve the conversion of the amorphous silicon layer into SiO 2 The heterogeneous composite substrate prepared by this preparation method has excellent high temperature and high pressure resistance, and the quality factor of the device prepared based on this is also further improved.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a heterogeneous composite substrate, the method comprising the following steps:

[0009] (1) A silicon substrate and a silicon carbide substrate are prepared, and one surface of the silicon substrate is oxidized to form SiO 2 layer, performing ion implantation on a surface of one side of the silicon carbide substrate to form a weakened layer;

[0010] (2) In the SiO 2 A first amorphous silicon sub-layer is deposited on the surface of the SiO layer, and a second amorphous silicon sub-layer is deposited on the ion implantation surface of the silicon carbide substrate; or 2 Depositing an amorphous silicon layer on the surface of the layer; or depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate;

[0011] The ion implantation surface of the silicon carbide substrate and the SiO 2 Surface bonding, the structure obtained is silicon layer / SiO 2 A bonding body of a silicon layer / amorphous silicon layer / silicon carbide substrate;

[0012] (3) performing a splitting process on the bonded body, so that the silicon carbide substrate in the bonded body is split along the weakening to obtain a residual layer and a heterogeneous composite substrate precursor;

[0013] (4) performing oxygen ion implantation from the cracked surface of the heterogeneous composite substrate precursor so that the oxygen ions are implanted into the amorphous silicon layer, and then performing annealing repair treatment so that the amorphous silicon layer is at least partially converted into SiO 2 layer to obtain the heterogeneous composite substrate.

[0014] The present invention implants oxygen ions into the amorphous silicon layer by implanting oxygen ions on the cracked surface of the heterogeneous composite substrate precursor. This strategy can accurately control the concentration distribution uniformity and depth distribution of the oxygen ion implantation, thereby improving the conversion of the amorphous silicon layer into SiO 2 The heterogeneous composite substrate prepared by this preparation method has excellent high temperature and high pressure resistance, and the quality factor of the device prepared based on this is also further improved.

[0015] It should be noted that the residual layer can be recycled and reused as a silicon carbide substrate.

[0016] Preferably, the SiO 2 The thickness of the layer is 100-500 nm, for example, it can be 100 nm, 200 nm, 300 nm, 400 nm or 500 nm.

[0017] Preferably, the types of ions implanted in step (a) include hydrogen ions and / or helium ions.

[0018] Preferably, the depth of the ion implantation in step (a) is ≤1 μm, for example, it may be 1 μm, 0.8 μm, 0.6 μm, 0.4 μm or 0.2 μm, etc., preferably 0.3-0.8 μm.

[0019] Preferably, in step (2), the first sub-amorphous silicon layer, the second sub-amorphous silicon layer and the amorphous silicon layer are deposited by sputtering.

[0020] In the present invention, the sputtering method refers to using Ar atoms to bombard a silicon target material and depositing the silicon target material onto the surface to be deposited by sputtering. The bonding body obtained by this method has a stronger bonding force.

[0021] Preferably, in the bonding body, the thickness of the amorphous silicon layer is 5-20 nm, for example, 5 nm, 10 nm, 15 nm or 20 nm.

[0022] In the present invention, the thickness of the deposited amorphous silicon layer is 5-20 nm, which can ensure the bonding strength during bonding and the subsequent bonding to SiO 2 The efficiency of conversion.

[0023] Preferably, the bonding parameters in step (2) include:

[0024] The bonding pressure is 10-100 kN, for example, 10 kN, 30 kN, 50 kN, 70 kN or 90 kN, and the vacuum degree is less than 1×10 -6 Pa, for example, can be 8×10 -7 Pa, 5×10 -7 Pa, 3×10 -7 Pa or 1×10 -7 Pa, etc., the bonding temperature is 20-30°C, for example, it can be 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, etc.

[0025] Preferably, the temperature of the splitting treatment in step (3) is 800-1200°C, for example, it can be 800°C, 900°C, 1000°C, 1100°C or 1200°C.

[0026] Preferably, the time for the splitting treatment in step (3) is 1-60 min, for example, it can be 1 min, 5 min, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0027] Preferably, in the heterogeneous composite substrate precursor in step (3), the thickness of the silicon carbide layer is 0.3-1.2 μm, for example, it can be 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm or 1.2 μm, etc.

[0028] Preferably, the range projection of the oxygen ion implantation in step (4) is distributed in the amorphous silicon layer.

[0029] It should be noted that ion implantation is a process in which compound molecules containing impurities are ionized into impurity ions, which are then gathered into beams and accelerated with a strong electric field to become high-energy ion beams. After being screened by a magnetic field, the beams directly bombard semiconductor materials. The advantage of ion implantation is that the implantation concentration and depth can be precisely controlled. Therefore, when O is implanted using the ion implantation method, almost the same O concentration distribution can be obtained at the same implantation depth.

[0030] In the present invention, the range projection of oxygen ion implantation is ensured to be distributed in the amorphous silicon layer, which can effectively improve the conversion of the amorphous silicon layer into SiO 2 At the same time, the projection range deviation is also included in the thickness range of the amorphous silicon layer, which can further improve the conversion efficiency.

[0031] Preferably, the peak value of the implantation concentration distribution of the oxygen ion implantation in step (4) is distributed in the amorphous silicon layer, and preferably the optimal implantation concentration distribution peak value is located in the middle of the amorphous silicon layer.

[0032] Preferably, the oxygen ion implantation method in step (4) includes a channel implantation method.

[0033] Preferably, the parameters of the channel implantation method include:

[0034] The oxygen ion implantation energy is 1-1000kev, for example, 1kev, 10kev, 100kev, 500kev or 1000kev, and the oxygen ion implantation dose is 1×10 16 -1×10 18 Ions / cm 2 , for example, it can be 1×10 16 Ions / cm 2 , 5×10 16 Ions / cm 2 , 1×10 17 Ions / cm 2 , 5×101 7 Ions / cm 2 or 1×10 18 Ions / cm 2 etc. The Tilt angle is 0 to 60°, for example, 1×10 16 Ions / cm 2 , 5×10 16 Ions / cm 2 , 1×10 17 Ions / cm 2 , 5×101 7 Ions / cm 2 or 1×10 18 Ions / cm 2The twist angle is 0 to 90°, for example, it can be 0, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80° or 90°.

[0035] Preferably, the temperature of the oxygen ion implantation in step (4) is 20-800°C, for example, 20°C, 50°C, 100°C, 200°C, 400°C, 600°C or 800°C, etc., preferably 500-650°C.

[0036] In the present invention, the injection temperature during oxygen ion injection is controlled to be 20-800°C, which can reduce damage to the silicon carbide substrate, and preferably 500-650°C. This is because the diffusion coefficient of the element is small due to the characteristics of silicon carbide itself. As the temperature increases, the injected ions are more likely to reach the target depth, that is, the O concentration can be relatively increased, and it is more convenient to combine with amorphous silicon. If the injection temperature is too low, it may cause increased damage to silicon carbide, which is not conducive to subsequent repair and affects device performance, and has a negative impact on the conversion of the amorphous silicon layer into SiO 2 If the injection temperature is high, the injection depth may become deeper, that is, the peak oxygen ion concentration is no longer in the amorphous silicon layer, which will cause a certain impact on the conversion of the amorphous silicon layer into SiO 2 Cause a certain impact.

[0037] Preferably, in the amorphous silicon layer in step (4), the uniformity of oxygen ion implantation is ≤0.5%, for example, it may be 0.5%, 0.4%, 0.3%, 0.2% or 0.1%.

[0038] In the present invention, since the uniformity of ion implantation is controlled within 0.5%, the corresponding O concentration distribution in the amorphous silicon layer is very uniform, and the conversion efficiency is relatively consistent.

[0039] Preferably, the temperature of the annealing repair treatment in step (4) is 800-1300°C, for example, it can be 800°C, 900°C, 1000°C, 1100°C, 1200°C or 1300°C.

[0040] In the present invention, if the temperature of the annealing repair treatment is too low, the amorphous silicon layer cannot be effectively converted into SiO 2 If the annealing temperature is too high, it may cause certain thermal stress, deformation, and the conversion of the amorphous silicon layer into SiO 2 Cause a certain impact.

[0041] Preferably, the annealing repair treatment time in step (4) is 30-600 min, for example, it can be 30 min, 50 min, 100 min, 200 min, 300 min, 400 min, 500 min or 600 min.

[0042] Preferably, the annealing repair process in step (4) is carried out in an oxygen-containing atmosphere, preferably an oxygen atmosphere.

[0043] Preferably, the gas in the oxygen-containing atmosphere includes oxygen and an inert gas.

[0044] It should be noted that the inert gas is not limited, and can be argon or nitrogen, for example.

[0045] Preferably, the preparation method comprises the following steps:

[0046] (1) A silicon substrate and a silicon carbide substrate are prepared, and a SiO2 layer with a thickness of 100-500 nm is formed on one surface of the silicon substrate by oxidation. 2 layer, implanting hydrogen ions and / or helium ions on one side surface of the silicon carbide substrate to form a weakened layer, wherein the depth of the hydrogen ions and / or helium ions implanted is ≤1 μm;

[0047] (2) Using a sputtering method, on the SiO 2 A first amorphous silicon sub-layer is deposited on the surface of the SiO layer, and a second amorphous silicon sub-layer is deposited on the ion implantation surface of the silicon carbide substrate; or 2 Depositing an amorphous silicon layer on the surface of the layer; or depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate;

[0048] The ion implantation surface of the silicon carbide substrate and the SiO 2 Surface bonding, the structure obtained is silicon layer / SiO 2 A bonded body of a silicon layer / amorphous silicon layer / silicon carbide substrate, wherein the thickness of the amorphous silicon layer is 5-20 nm;

[0049] The bonding parameters include: bonding pressure of 10-100 kN, vacuum degree of <1×10 -6 Pa, bonding temperature is 20-30°C;

[0050] (3) performing a splitting treatment on the bonded body at a temperature of 800-1200° C. for 1-60 min, so that the silicon carbide substrate in the bonded body is split along the weakened part to obtain a residual layer and a silicon layer / SiO 2 A heterogeneous composite substrate precursor of a layer / amorphous silicon layer / silicon carbide layer, wherein the thickness of the silicon carbide layer is 0.8-1.2 μm;

[0051] (4) using a channel implantation method, at a temperature of 500-650° C., implanting oxygen ions from the silicon carbide layer side of the heterogeneous composite substrate precursor, so that the oxygen ions are implanted into the amorphous silicon layer, and then performing an annealing repair treatment in an oxygen atmosphere, wherein the annealing repair treatment temperature is 800-1300° C., and the time is 30-600 min, so that at least 50% of the amorphous silicon layer is converted into SiO 2 layer to obtain the heterogeneous composite substrate;

[0052] The parameters of the channel implantation method include: oxygen ion implantation energy of 1-1000kev, oxygen ion implantation dose of 1×10 16 -1×10 18 Ions / cm 2 , the Tilt angle is 0~60°, and the Twist angle is 0~90°.

[0053] In a second aspect, the present invention provides a heterogeneous composite substrate, which is prepared by the preparation method described in the first aspect.

[0054] In a third aspect, the present invention provides an application of the heterogeneous composite substrate as described in the second aspect, wherein the heterogeneous composite substrate is used for preparing a semiconductor device.

[0055] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] The present invention implants oxygen ions into the amorphous silicon layer by implanting oxygen ions on the cracked surface of the heterogeneous composite substrate precursor. This strategy can accurately control the concentration distribution uniformity of the oxygen ion implantation and improve the conversion of the amorphous silicon layer into SiO 2 The heterogeneous composite substrate prepared by this preparation method has excellent high temperature and high pressure resistance, and the quality factor of the device prepared based on this is also further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 This is a process flow chart provided for Example 1 of the present invention. DETAILED DESCRIPTION

[0059] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0060] Example 1

[0061] This embodiment provides a method for preparing a heterogeneous composite substrate, and its process flow chart is as follows: Figure 1 As shown, the preparation method comprises the following steps:

[0062] (1) A silicon substrate and a silicon carbide substrate were prepared. A SiO layer with a thickness of 200 nm was formed on one surface of the silicon substrate by thermal oxidation. 2 The oxidation temperature is 1000°C for 90 minutes, and hydrogen ions are implanted on one side of the silicon carbide substrate to form a weakened layer, wherein the depth of the hydrogen ion implantation is 0.5 μm;

[0063] (2) Using a sputtering method, on the SiO 2 A first amorphous silicon layer is deposited on the surface of the layer, and a second amorphous silicon layer is deposited on the ion implantation surface of the silicon carbide substrate, wherein the total thickness of the first amorphous silicon layer and the second amorphous silicon layer is 10 nm;

[0064] The ion implantation surface of the silicon carbide substrate and the SiO 2 Surface bonding, the structure obtained is silicon layer / SiO 2 A bonding body of a silicon layer / amorphous silicon layer / silicon carbide substrate;

[0065] The bonding parameters include: bonding pressure of 50 kN, vacuum degree of 1×10 -7 Pa, the bonding temperature is 25°C;

[0066] (3) The bonded body is subjected to a splitting treatment at a temperature of 1000° C. for 30 minutes, so that the silicon carbide substrate in the bonded body is split along the weakened part to obtain a residual layer and a silicon layer / SiO 2 A heterogeneous composite substrate precursor of a silicon layer / amorphous silicon layer / silicon carbide layer, wherein the thickness of the silicon carbide layer is 0.5 μm;

[0067] (4) using a channel implantation method, at a temperature of 600° C., oxygen ion implantation is performed from the silicon carbide layer side of the heterogeneous composite substrate precursor, so that the range projection of the oxygen ions is distributed in the amorphous silicon layer, the projection range deviation is contained within the thickness range of the amorphous silicon layer, the implantation concentration of the oxygen ions is also distributed in the amorphous silicon layer, and the oxygen ion implantation uniformity in the amorphous silicon layer is 0.35%;

[0068] Then, an annealing treatment is performed in an oxygen atmosphere at a temperature of 1000°C for 120 minutes to convert 75% of the amorphous silicon layer into SiO 2 layer to obtain the heterogeneous composite substrate;

[0069] The parameters of the channel implantation method include: oxygen ion implantation energy of 225kev, oxygen ion implantation dose of 2.5×10 17 Ions / cm 2 , the Tilt angle is 17°, and the Twist angle is 0°.

[0070] Example 2

[0071] This embodiment provides a method for preparing a heterogeneous composite substrate, the method comprising the following steps:

[0072] (1) A silicon substrate and a silicon carbide substrate were prepared. A SiO layer with a thickness of 200 nm was formed on one surface of the silicon substrate by thermal oxidation. 2 The oxidation temperature is 1000° C., the time is 90 min, helium ions are implanted on one side surface of the silicon carbide substrate to form a weakened layer, and the depth of the helium ion implantation is 0.4 μm;

[0073] (2) Using a sputtering method, on the SiO 2 A first amorphous silicon layer is deposited on the surface of the layer, and a second amorphous silicon layer is deposited on the ion implantation surface of the silicon carbide substrate, wherein the total thickness of the first amorphous silicon layer and the second amorphous silicon layer is 10 nm;

[0074] The ion implantation surface of the silicon carbide substrate and the SiO 2 Surface bonding, the structure obtained is silicon layer / SiO 2 A bonding body of a silicon layer / amorphous silicon layer / silicon carbide substrate;

[0075] The bonding parameters include: bonding pressure of 50 kN, vacuum degree of 1×10 -7 Pa, the bonding temperature is 25°C;

[0076] (3) The bonded body is subjected to a splitting treatment at a temperature of 850° C. for 50 min, so that the silicon carbide substrate in the bonded body is split along the weakened portion to obtain a residual layer and a silicon layer / SiO 2 A heterogeneous composite substrate precursor of a silicon layer / amorphous silicon layer / silicon carbide layer, wherein the thickness of the silicon carbide layer is 0.4 μm;

[0077] (4) using a channel implantation method, at a temperature of 500° C., oxygen ion implantation is performed from the silicon carbide layer side of the heterogeneous composite substrate precursor, so that the range projection of the oxygen ions is distributed in the amorphous silicon layer, the projection range deviation is contained within the thickness range of the amorphous silicon layer, the implantation concentration of the oxygen ions is also distributed in the amorphous silicon layer, and the oxygen ion implantation uniformity in the amorphous silicon layer is 0.38%;

[0078] Then, an annealing repair process is performed in an oxygen atmosphere at a temperature of 900° C. for 180 min, so that 68% of the amorphous silicon layer is converted into SiO 2 layer to obtain the heterogeneous composite substrate;

[0079] The parameters of the channel implantation method include: oxygen ion implantation energy of 180kev, oxygen ion implantation dose of 2×10 17 Ions / cm 2 , the Tilt angle is 17°, and the Twist angle is 0°.

[0080] Example 3

[0081] This embodiment provides a method for preparing a heterogeneous composite substrate, the method comprising the following steps:

[0082] (1) A silicon substrate and a silicon carbide substrate were prepared. A SiO layer with a thickness of 200 nm was formed on one surface of the silicon substrate by thermal oxidation. 2 The oxidation temperature is 1000°C for 90 minutes, and hydrogen ions are implanted on one side of the silicon carbide substrate to form a weakened layer, wherein the depth of the hydrogen ion implantation is 0.6 μm;

[0083] (2) Using a sputtering method, on the SiO 2 A first amorphous silicon layer is deposited on the surface of the layer, and a second amorphous silicon layer is deposited on the ion implantation surface of the silicon carbide substrate, wherein the total thickness of the first amorphous silicon layer and the second amorphous silicon layer is 10 nm;

[0084] The ion implantation surface of the silicon carbide substrate and the SiO 2 Surface bonding, the structure obtained is silicon layer / SiO 2 A bonding body of a silicon layer / amorphous silicon layer / silicon carbide substrate;

[0085] The bonding parameters include: bonding pressure of 50 kN, vacuum degree of 1×10 -7 Pa, the bonding temperature is 25°C;

[0086] (3) The bonded body is subjected to a splitting treatment at a temperature of 1100° C. for 20 minutes, so that the silicon carbide substrate in the bonded body is split along the weakened part to obtain a residual layer and a silicon layer / SiO 2 A heterogeneous composite substrate precursor of a silicon layer / amorphous silicon layer / silicon carbide layer, wherein the thickness of the silicon carbide layer is 0.6 μm;

[0087] (4) using a channel implantation method, at a temperature of 650° C., oxygen ion implantation is performed from the silicon carbide layer side of the heterogeneous composite substrate precursor, so that the range projection of the oxygen ions is distributed in the amorphous silicon layer, the projection range deviation is contained within the thickness range of the amorphous silicon layer, the implantation concentration of the oxygen ions is also distributed in the amorphous silicon layer, and the oxygen ion implantation uniformity in the amorphous silicon layer is 0.37%;

[0088] Then, an annealing treatment is performed in an oxygen atmosphere at a temperature of 1100° C. for 60 min, so that 67% of the amorphous silicon layer is converted into SiO 2 layer to obtain the heterogeneous composite substrate;

[0089] The parameters of the channel implantation method include: oxygen ion implantation energy of 300kev, oxygen ion implantation dose of 3×10 17 Ions / cm 2 , the Tilt angle is 17°, and the Twist angle is 0°.

[0090] Example 4

[0091] The difference between this embodiment and embodiment 1 is that the oxygen atmosphere in step (4) is replaced by a nitrogen atmosphere.

[0092] The rest of the preparation methods and parameters were the same as those in Example 1.

[0093] Example 5

[0094] The difference between this embodiment and embodiment 1 is that the temperature of oxygen ion implantation in step (4) is 20°C.

[0095] The rest of the preparation methods and parameters were the same as those in Example 1.

[0096] Example 6

[0097] The difference between this embodiment and embodiment 1 is that the temperature of oxygen ion implantation in step (4) is 800°C.

[0098] The rest of the preparation methods and parameters were the same as those in Example 1.

[0099] Example 7

[0100] The difference between this embodiment and embodiment 1 is that the temperature of the annealing repair treatment in step (4) is 500°C.

[0101] The rest of the preparation methods and parameters were the same as those in Example 1.

[0102] Example 8

[0103] The difference between this embodiment and embodiment 1 is that the temperature of the annealing repair treatment in step (4) is 1500°C.

[0104] The rest of the preparation methods and parameters were the same as those in Example 1.

[0105] Example 9

[0106] The difference between this embodiment and embodiment 1 is that the uniformity of oxygen ion implantation in the amorphous silicon layer in step (4) is 5%.

[0107] The rest of the preparation methods and parameters were the same as those in Example 1.

[0108] Comparative Example 1

[0109] The difference between this comparative example and Example 1 is that no amorphous silicon layer is deposited in step (2).

[0110] The rest of the preparation methods and parameters were the same as those in Example 1.

[0111] Comparative Example 2

[0112] The difference between this comparative example and Example 1 is that step (4) is not performed.

[0113] The rest of the preparation methods and parameters were the same as those in Example 1.

[0114] Comparative Example 3

[0115] The difference between this comparative example and Example 1 is that the oxygen ion implantation process in step (4) is performed before the bond body is cleaved.

[0116] The rest of the preparation methods and parameters were the same as those in Example 1.

[0117] Performance Testing

[0118] The bonding strength, interface thermal resistance and thermal conductivity of the heterogeneous composite substrates prepared in the above embodiments and comparative examples were tested. The specific test conditions included: the conversion rate was evaluated by XRD; the bonding strength was tested by opening crack; and the interface thermal resistance was tested by Time-domain thermoreflectance (TDTR).

[0119] The above heterogeneous composite substrate is made into a microring resonant device, and the quality factor Q is calculated using the following formula: Q = 1 / (R × √(L / C)), where R is the resistance value in the parallel resonant circuit, L is the inductance value, and C is the capacitance value. At this time, the capacitor C and the inductor L are connected in parallel.

[0120] The results are shown in Table 1.

[0121] Table 1

[0122]

[0123]

[0124] analyze:

[0125] As can be seen from the above table, the present invention implants oxygen ions into the amorphous silicon layer by implanting oxygen ions on the cracked surface of the heterogeneous composite substrate precursor. This strategy can accurately control the concentration distribution uniformity of the oxygen ion implantation and improve the conversion of the amorphous silicon layer into SiO 2 The heterogeneous composite substrate prepared by this preparation method has excellent high temperature and high pressure resistance, and the quality factor of the device prepared based on this is also further improved.

[0126] By comparing Example 1 with Example 4, it can be seen that if the annealing repair process is performed in a nitrogen atmosphere, the amorphous silicon layer is converted into SiO 2 The conversion rate is greatly reduced.

[0127] It can be seen from the comparison between Example 1 and Examples 5-6 that if the temperature of oxygen ion implantation is low, it may cause increased damage to silicon carbide, which is not conducive to subsequent repair and affects device performance, and has a negative impact on the conversion of the amorphous silicon layer into SiO 2 If the temperature of oxygen ion implantation is high, high-temperature diffusion may occur, that is, the implantation depth becomes deeper, which is not conducive to the subsequent diffusion of O and the conversion of amorphous silicon layer into SiO 2 Cause a certain impact.

[0128] It can be seen from the comparison between Example 1 and Examples 7-8 that if the temperature of the annealing repair treatment is too low, it is not conducive to the lattice repair and the subsequent conversion of the amorphous silicon layer into SiO 2 If the annealing temperature is too high, it may cause certain thermal stress, deformation, and the conversion of the amorphous silicon layer into SiO 2 Cause a certain impact.

[0129] From the comparison between Example 1 and Example 9, it can be seen that if the oxygen ion implantation uniformity in the amorphous silicon layer is poor, each region of the amorphous silicon layer is converted into SiO 2 The conversion rate is inconsistent, some areas are high and some areas are low. Devices with high conversion rates have good performance, while devices with low conversion rates have poor performance.

[0130] By comparing Example 1 with Comparative Example 1, it can be seen that if the amorphous silicon layer is not provided, the bonding strength is poor, and there is a risk that the top SiC layer will fall off in the subsequent process, making the composite substrate meaningless, and the falling film layer will bring certain risks to the subsequent processes and equipment.

[0131] By comparing Example 1 with Comparative Example 2, it can be seen that if the conversion process of the amorphous silicon layer is not performed, the thermal resistance of the bonding interface is large, indicating that the composite substrate has poor performance and large damage compared to the single crystal substrate, and the quality factor of the subsequent device is poor, which is not conducive to production and affects the device performance.

[0132] By comparing Example 1 with Comparative Example 3, it can be seen that if the oxygen ion implantation process is performed before the bond body is cracked, it is difficult to distribute the oxygen ions in the amorphous silicon layer area. The required implantation energy and dosage are very large, which cannot be achieved by the mainstream equipment currently on the market. In addition, the implantation is very time-consuming and will cause very serious deformation after the implantation, and the subsequent process cannot continue.

[0133] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a heterogeneous composite substrate, characterized in that: The preparation method comprises the following steps: (1) preparing a silicon substrate and a silicon carbide substrate, performing oxidation on one surface of the silicon substrate to form a SiO2 layer, and performing ion implantation on one surface of the silicon carbide substrate to form a weakened layer; (2) depositing a first amorphous silicon layer on the surface of the SiO2 layer, and depositing a second amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; or, depositing an amorphous silicon layer on the surface of the SiO2 layer; or, depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; Bonding the ion implanted surface of the silicon carbide substrate and the SiO2 surface of the silicon substrate to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate; (3) performing a splitting process on the bonded body, so that the silicon carbide substrate in the bonded body is split along the weakening to obtain a residual layer and a heterogeneous composite substrate precursor; (4) performing oxygen ion implantation from the cracked surface of the heterogeneous composite substrate precursor so that the oxygen ions are implanted into the amorphous silicon layer, and then performing annealing repair treatment so that the amorphous silicon layer is at least partially converted into a SiO2 layer to obtain the heterogeneous composite substrate.

2. The preparation method according to claim 1, characterized in that: The thickness of the SiO2 layer in step (1) is 100-500nm; Preferably, the types of ions implanted in step (a) include hydrogen ions and / or helium ions; Preferably, the depth of the ion implantation in step (a) is ≤1 μm, preferably 0.3-0.8 μm.

3. The preparation method according to claim 1 or 2, characterized in that: Step (2) The first sub-amorphous silicon layer, the second sub-amorphous silicon layer and the amorphous silicon layer are deposited by sputtering; Preferably, in the bonding body, the thickness of the amorphous silicon layer is 5-20 nm.

4. The preparation method according to any one of claims 1 to 3, characterized in that The bonding parameters of step (2) include: The bonding pressure is 10-100kN, and the vacuum degree is less than 1×10 -6 Pa, the bonding temperature is 20-30℃.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The temperature of the splitting treatment in step (3) is 800-1200° C. Preferably, the time for the splitting treatment in step (3) is 1-60 min; Preferably, in the heterogeneous composite substrate precursor in step (3), the thickness of the silicon carbide layer is 0.3-1.2 μm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The range projection of the oxygen ion implantation in step (4) is distributed in the amorphous silicon layer; Preferably, the oxygen ion implantation method in step (4) includes a channel implantation method; Preferably, the parameters of the channel implantation method include: The oxygen ion implantation energy is 1-1000kev, and the oxygen ion implantation dose is 1×10 16 -1×10 18 Ions / cm 2 , Tilt angle is 0~60°, Twist angle is 0~90°; Preferably, the temperature of the oxygen ion implantation in step (4) is 20-800° C., preferably 500-650° C.; Preferably, in the amorphous silicon layer in step (4), the uniformity of oxygen ion implantation is ≤0.5%.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The temperature of the annealing repair treatment in step (4) is 800-1300° C. Preferably, the annealing repair treatment time in step (4) is 30-600 min.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) preparing a silicon substrate and a silicon carbide substrate, performing oxidation on one surface of the silicon substrate to form a SiO2 layer with a thickness of 100-500 nm, and performing hydrogen ion and / or helium ion implantation on one surface of the silicon carbide substrate to form a weakened layer, wherein the depth of the hydrogen ion and / or helium ion implantation is ≤1 μm; (2) depositing a first amorphous silicon layer on the surface of the SiO2 layer and a second amorphous silicon layer on the ion implantation surface of the silicon carbide substrate by sputtering; or, depositing an amorphous silicon layer on the surface of the SiO2 layer; or, depositing an amorphous silicon layer on the ion implantation surface of the silicon carbide substrate; Bonding the ion implantation surface of the silicon carbide substrate and the SiO2 surface of the silicon substrate to obtain a bonded body having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide substrate, wherein the thickness of the amorphous silicon layer is 5-20 nm; The bonding parameters include: bonding pressure of 10-100 kN, vacuum degree of <1×10 -6 Pa, bonding temperature is 20-30°C; (3) performing a splitting treatment on the bonded body at a temperature of 800-1200° C. for 1-60 min, so that the silicon carbide substrate in the bonded body is split along the weakening, to obtain a residual layer and a heterogeneous composite substrate precursor having a structure of silicon layer / SiO2 layer / amorphous silicon layer / silicon carbide layer, wherein the thickness of the silicon carbide layer is 0.3-1.2 μm; (4) using a channel implantation method, at a temperature of 500-650° C., oxygen ions are implanted from the silicon carbide layer side of the heterogeneous composite substrate precursor so that the oxygen ions are implanted into the amorphous silicon layer, and then annealing and repairing treatment is performed in an oxygen atmosphere at a temperature of 800-1300° C. for 30-600 min, so that at least 50% of the amorphous silicon layer is converted into a SiO2 layer, thereby obtaining the heterogeneous composite substrate; The parameters of the channel implantation method include: oxygen ion implantation energy of 1-1000kev, oxygen ion implantation dose of 1×10 16 -1×10 18 Ions / cm 2 , the Tilt angle is 0~60°, and the Twist angle is 0~90°.

9. A heterogeneous composite substrate, characterized in that: The heterogeneous composite substrate is prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the heterogeneous composite substrate as claimed in claim 9, characterized in that: The heterogeneous composite substrate is used for preparing semiconductor devices.